Coated article

The antimicrobial coating of low-priced copper oxide coating with multi-layer structure solves the problems of high cost and poor wear resistance in the existing technology, realizes wide application in medical care facilities, and provides economical and efficient antimicrobial coating. Effect.

CN118773545APending Publication Date: 2024-10-15VAPOR TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410414968.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2024-04-08
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing antimicrobial coating materials suffer from high cost, poor abrasion resistance and unsuitable appearance, making them difficult to implement widely, especially in healthcare facilities.

Method used

A low-cost copper oxide coating with a multi-layer structure, at least five times thicker than a single layer, is used as an antimicrobial coating, combined with the substrate and adhesion layer, and is manufactured by chemical vapor deposition or physical vapor deposition technology.

Benefits of technology

Provides an economical, highly effective antimicrobial coating with improved wear resistance and applicability for use on a variety of surfaces, including medical devices and decorative surfaces, to effectively inhibit microbial growth and spread.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004780512350000061
    Figure BDA0004780512350000061
  • Figure BDA0004780512350000071
    Figure BDA0004780512350000071
  • Figure BDA0004780512350000101
    Figure BDA0004780512350000101
Patent Text Reader

Abstract

A coated article having an antimicrobial coating is provided. The coated article includes a substrate and at least one adhesion layer disposed on the substrate. The at least one adhesion layer includes a component selected from the group consisting of copper oxides, zirconium oxides, and combinations thereof. Advantageously, an antimicrobial low valent copper oxide layer is disposed on the at least one adhesion layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Application Serial No. 63 / 457,602, filed on April 6, 2023, the disclosure of which is hereby incorporated by reference into this application in its entirety. Technical Field

[0003] In at least one aspect, the present invention relates to antimicrobial coatings and articles coated with such coatings, and more particularly to an antimicrobial coating containing cuprous oxide. Background Art

[0004] Coatings with bioactive properties can be used for various purposes. Bioactivity refers to materials that have biological or physiological effects on organisms. For example, bioactive materials include materials that cause changes in the normal biological functions or physiological mechanisms of organisms. As used herein, bioactivity includes beneficial and harmful effects on microorganisms or changes in the normal functions of microorganisms. A common bioactive material is an antimicrobial substance. Antimicrobial coatings have many uses. Typically, antimicrobial coatings inhibit the growth of microorganisms (like viruses, bacteria or fungal organisms) or kill them. A particularly relevant example includes preventing the spread of communicable diseases by using antimicrobial materials. Antimicrobial materials can also be used for sanitary purposes. The desire to prevent the spread of disease and enhance hygiene has led to significant efforts in the development of antimicrobial materials. The use of antimicrobial materials in healthcare facilities and health treatments can provide significant benefits. Healthcare facilities (such as hospitals) present a unique environment that combines high concentrations of germs and individuals with fragile immunity. Therefore, facilities (such as hospitals) benefit from antimicrobial surfaces. Antimicrobial materials used in medical equipment can reduce the burden of disinfection and prevent the spread of disease. In addition, affordable antimicrobial surfaces can present benefits on any surface that comes into contact with organisms. For example, surfaces involved in cooking or commonly touched surfaces like door handles can benefit from antimicrobial properties. Even surfaces that are primarily decorative, if affordable, can benefit from antimicrobial properties and help inhibit the spread and growth of harmful or undesirable antimicrobial organisms.

[0005] Antimicrobial materials can be difficult and expensive to produce. In addition, antimicrobial properties can have other undesirable properties. For example, some antimicrobial materials can be too soft. Other antimicrobial materials can have poor wear resistance. Antimicrobial additives are sold, like silver phosphate glass that can be mixed into paint. In some applications, the appearance of the paint may be undesirable. Some antimicrobial coatings can use nanoparticle vapor deposition to deposit nanoparticles with antimicrobial properties on the surface of the coating. For example, Protec Antimicrobial coatings are those that use nanoparticles. However, using nanoparticles can be complex and expensive. In addition, such coatings can have a brittle surface or poor wear resistance. Another example of an antimicrobial material includes various metals. For example, silver is known to have antimicrobial properties. However, silver can be expensive and its properties may not be suitable for many applications. For example, the appearance or wear resistance of silver may not be suitable for certain applications.

[0006] Therefore, there is a need for an antimicrobial coating that addresses one or more of these problems or provides an alternative to existing antimicrobial materials. Summary of the invention

[0007] In at least one aspect, a coated article having an antimicrobial coating is provided. The coated article comprises a substrate and at least one adhesion layer disposed on the substrate. The at least one adhesion layer comprises a component selected from the group consisting of copper oxide, zirconium oxide, and a combination thereof. Advantageously, the antimicrobial subvalent copper oxide layer is disposed on the at least one adhesion layer. Characteristically, even if the antimicrobial subvalent copper oxide layer is a multilayer structure, the antimicrobial subvalent copper oxide layer is at least 5 times thicker than the at least one adhesion layer.

[0008] In another aspect, a coated article having an antimicrobial coating is provided. The coated article comprises a substrate and a subvalent copper oxide adhesion layer disposed on the substrate. The antimicrobial subvalent copper oxide layer is disposed on the at least one adhesion layer. Characteristically, even if the antimicrobial subvalent copper oxide layer is a multilayer structure, the antimicrobial subvalent copper oxide layer is at least 5 times thicker than the at least one adhesion layer.

[0009] In another aspect, a coated article having an antimicrobial coating is provided. The coated article comprises a substrate and a copper oxide adhesion layer disposed on the substrate. A subvalent copper oxide layer is disposed on and optionally contacts the copper oxide adhesion layer. Advantageously, the coating on the coated article does not contain metals other than copper.

[0010] The foregoing summary is illustrative only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments, and features described above, further aspects, embodiments, and features will become apparent by reference to the drawings and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] For a further understanding of the nature, objects and advantages of the present disclosure, reference should be made to the following detailed description, read in conjunction with the following drawings, in which like reference numerals represent like elements and in which:

[0012] Figure 1A is a cross section of a coated article having an antimicrobial layer.

[0013] Figure 1B is a cross section of a coated article having an antimicrobial layer with a transparent oxide outer coating.

[0014] Figure 2 is an EDS scan of a substrate coated with an adhesion layer and a subvalent copper oxide layer.

[0015] Figure 3A and Figure 3B is a SEM micrograph of a low-valent copper oxide layer.

[0016] Figure 4 It is related to copper and copper oxide (Cu 2 O) X-ray diffraction pattern of the peak-aligned subvalent copper oxide layer. DETAILED DESCRIPTION

[0017] Reference will now be made in detail to the currently preferred compositions, embodiments and methods of the present invention, which constitute the best modes of practicing the present invention currently known to the inventors. The accompanying drawings are not necessarily drawn to scale. However, it should be understood that the disclosed embodiments are merely examples of the present invention, which can be implemented in different and alternative forms. Therefore, the specific details disclosed herein should not be interpreted as limiting, but only as representative benchmarks for any aspect of the present invention and / or as representative benchmarks for teaching those skilled in the art to use the present invention in a variety of ways.

[0018] Except in the examples or otherwise explicitly stated, all numerical quantities in this specification indicating the amount of material or reaction and / or use conditions should be understood as being modified by the word "about" when describing the broadest scope of the invention. Practice within the stated numerical limits is generally preferred. And, unless expressly stated to the contrary: percentages, "parts of..." and ratios are by weight; unless otherwise stated, the molecular weight provided for any polymer refers to the weight average molecular weight; the description of a group or class of materials suitable or preferred for a given object in conjunction with the present invention means that any mixture of two or more of the members of the group or class is equally suitable or preferred; the description of ingredients in chemical terms refers to the ingredients when added to any combination specified in this specification, and does not necessarily exclude chemical interactions that occur among the ingredients of the mixture once mixed; the first definition of an acronym or other abbreviation applies to all subsequent uses of the same abbreviation in this article, and applies to normal expression variants of the initially defined abbreviation with necessary modifications; and, unless expressly stated to the contrary, the measurement of the same property is determined by the same technique for reference to the property before and after.

[0019] It should also be understood that the present invention is not limited to the specific embodiments and methods described below, as specific components and / or conditions may of course vary. In addition, the terminology used herein is only for the purpose of describing specific embodiments of the present invention, and is not intended to be limiting in any way.

[0020] It must also be noted that, as used in this specification and the appended claims, the singular forms "a", "an", and "the" include plural referents unless the context clearly dictates otherwise. For example, a component mentioned in the singular is intended to include plural components.

[0021] The term "comprising" is synonymous with "including," "having," "containing," or "characterized by." These terms are inclusive and open-ended, and do not exclude additional, unrecited elements or method steps.

[0022] The phrase "consisting of" excludes any element, step, or ingredient not specified in the claim. When the phrase appears in a clause of the body of a claim, rather than immediately following the preamble, it is limited only to the elements set forth in that clause; other elements are not excluded from the claim as a whole.

[0023] The phrase "consisting essentially of limits the scope of a claim to the specified materials or steps, plus those that do not materially affect the basic and novel characteristic(s) of the claimed subject matter.

[0024] With respect to the terms "comprising," "consisting of," and "consisting essentially of," when one of these three terms is used herein, the presently disclosed and claimed subject matter may include the use of either of the other two terms.

[0025] It should also be understood that the integer range clearly includes all intermediate integers. For example, the integer range 1-10 clearly includes 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. Similarly, the range 1 to 100 includes 1, 2, 3, 4 ... 97, 98, 99, 100. Similarly, when any range is needed, the difference between the upper limit and the lower limit can be divided by the intermediate digit of the increment of 10 as an alternative upper limit or lower limit. For example, if the scope is 1.1 to 2.1, the following numbers 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 and 2.0 can be selected as the lower limit or upper limit. In the specific examples set forth herein, concentration, temperature and reaction conditions (for example, pressure, pH, etc.) can be implemented by being expressed as a value rounded to three significant figures plus or minus 50%. In a refinement, the concentration, temperature, and reaction conditions (e.g., pressure, pH, etc.) may be implemented with values ​​expressed as rounding the values ​​provided in the examples to three significant figures plus or minus 30%. In another refinement, the concentration, temperature, and reaction conditions (e.g., pH, etc.) may be implemented with values ​​expressed as rounding the values ​​provided in the examples to three significant figures plus or minus 10%.

[0026] The term "low-valent copper oxide" means a copper oxide having a higher copper to oxygen atomic ratio than the copper to oxygen ratio in copper oxide (CuO). Thus, the copper to oxygen ratio is greater than 1:1. For example, cuprous oxide (Cu 2 O) is considered a low-valent copper oxide. For example, a low-valent copper oxide is a copper oxide having the formula Cu z O, wherein z is 3 to 1.1. In a refinement, z is at least 1.1, 1.3, 1.5, 1.6, 1.7 or 1.8 and at most 3, 2.7, 2.5, 2.4, 2.3, 2.2 or 2.1.

[0027] The term "copper oxide" means a compound having the formula Cu x O, wherein x is 2.2 to 0.6. In a refinement, x is at least 0.6, 0.7, 0.9 or 0.95 and at most 2.2, 2.0, 1.8, 1.6, 1.4 or 1.2.

[0028] The term "zirconium oxide" means a compound having the formula Zr y O 2 The compound wherein y is 3 to 0.6.

[0029] abbreviation:

[0030] "EDS" means energy dispersive X-ray spectroscopy.

[0031] "SEM" means scanning electron microscope.

[0032] refer to Figure 1Aand Figure 1B , a schematic diagram of a coated article with an antimicrobial coating is provided. The coated article 10 includes a substrate 12 and at least one adhesion layer 14 disposed on the substrate. The at least one adhesion layer 14 comprises a component selected from the group consisting of copper oxide, zirconium oxide and a combination thereof. An antimicrobial low-valent copper oxide layer 18 is disposed on the at least one adhesion layer 14. Characterized in that the antimicrobial low-valent copper oxide layer 18 is at least 5 times thicker than the at least one adhesion layer 14. In an improved solution, the antimicrobial low-valent copper oxide layer 18 has a thickness greater than 0.5 microns. In a further improved solution, the low-valent copper oxide layer 18 has a thickness of about 0.5 microns to about 10 microns. Advantageously, the at least one adhesion layer 14 and the low-valent copper oxide layer 18 can be manufactured by chemical vapor deposition or by physical vapor deposition. Suitable physical vapor deposition techniques include arc deposition and reactive sputtering. Typically, the at least one adhesion layer 14 has a thickness of about 20nm to 200nm. Figure 1B A variant is provided in which the copper suboxide layer 18 is coated with a top layer 20 .

[0033] In another aspect, the top layer 20 is a transparent metal oxide layer 20, such as a layer comprising zirconium oxide.

[0034] In another aspect, the top layer 20 is a silane-containing antimicrobial layer, as disclosed in U.S. Patent Publication No. 2022 / 0235232; the entire disclosure of which is hereby incorporated by reference. In this regard, the silane-containing antimicrobial layer may include a microbial inhibition material having a first silane compound and a metal ion, wherein the first silane compound includes a functional group that binds to the metal ion. For example, the silane-containing antimicrobial layer may include an antimicrobial material. Specifically, the silane-containing antimicrobial layer includes a first silane compound and a metal ion. Characterized in that the silane compound includes a functional group that binds to the metal ion. In a further improvement, the silane-containing antimicrobial layer further includes a fingerprint inhibition material, which includes a silane compound (e.g., a second silane compound) that may be preferably hydrophobic.

[0035] In another aspect, the first silane compound is described by formula (I):

[0036]

[0037] in:

[0038] R 1 Selected from the group consisting of: -C 1 -C x+1 Alkyl-S(R 3 ) y (M), -C 2 -C x+2Alkenyl-S(R 3 ) y (M), -C 3 -C x+3 Alkynyl-S(R 3 ) y (M), -C 1 -C x Alkyl-N(R 3 ) y (M), -C 2 -C x Alkenyl-N(R 3 ) y (M), -C 3 -C x Alkynyl-N(R 3 ) y (M), -C 1 -C x+1 Alkyl-P(R 3 ) y (M), -C 2 -C x+2 Alkenyl-P(R 3 ) y (M) and -C 3 -C x+3 Alkynyl-P(R 3 ) y (M); each R 2 are the same or different and are a bond to another Si atom of the repeating structure, or are selected from the group consisting of: hydrogen, -C 1 -C 10 Alkyl, -C 2 -C 10 Alkenyl, -C 3 -C 10 Alkynyl;

[0039] n is a positive integer (e.g., 1 to 500 or more);

[0040] x is a positive integer (e.g., 1 to 20 or more);

[0041] y is a positive integer (e.g., 1 to 4 or greater); and

[0042] M is a metal ion or a metal.

[0043] In another aspect, n is a positive integer greater than or equal to 1, 2, 10, 20, 50, 100, 200, 300, 400, or 450. In a refinement, n is a positive integer less than or equal to 500, 450, 400, 300, 200, 100, 50, 20, 10, 5, or 2. Combinations of the above-referenced ranges are also contemplated.

[0044] In another aspect, x is a positive integer greater than or equal to 1, 2, 4, 6, 8, 10, 12, 14, 16, or 18. In a refinement, x is a positive integer less than or equal to 20, 18, 16, 14, 12, less than or equal to 10, 8, 6, 4, or 2. Combinations of the above-referenced ranges are also contemplated.

[0045] In another aspect, y is a positive integer greater than or equal to 1, 2, or 3. In a refinement, y is less than or equal to 4, 3, or 2. Combinations of the above-referenced ranges are also contemplated.

[0046] In a refinement, M is a metal ion selected from the group consisting of: copper ions (e.g., Cu + , Cu 2+ ), titanium ions (e.g., Ti 3+ 、Ti 4+ ), vanadium ions (e.g., V 2+ 、V 3+ ), chromium ions (e.g., Cr 2+ Cr 3+ ), manganese ions (e.g., Mn 2+ , Mn 4+ ), iron ions (e.g., Fe 2+ , Fe 3+ ), cobalt ions (e.g., Co 2+ 、Co 3+ ), nickel ions (e.g., Ni 2+ ), zinc ions (e.g., Zn 2+ ), zirconium ions (e.g., Zr 2+ ), palladium ions (e.g., Pd 2+ ), cadmium ions (e.g., Cd 2+ ), platinum ions (e.g., Pt 2+ , Pt 4+ ), gold ions (e.g., Au + 、Au 3+ ), mercury ions (e.g., Hg 2+ ), terbium ions (e.g., Tb 3+ ), tungsten ions (e.g., W 4+ ), aluminum ions (e.g., Al 3+ ), gallium ions (e.g., Ga 3+ ), germanium ions (e.g., Ge 2+ ), arsenic ions (e.g., As 3+ ), selenium ions (e.g., Se 2+ ), tin ions (e.g., Sn 2+ ), antimony ions (e.g., Sb 3+ ), tellurium ions (e.g., Te 2+ ), lead ions (e.g., Pb 4+), bismuth ions (e.g., Bi 3+ ), and / or combinations thereof. In another refinement, M is a metal selected from the group consisting of Ag, Cu, Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Zr, Pd, Cd, Pt, Au, Hg, W, Al, Ga, Ge, Tb, As, Se, Sn, Sb, Te, Pb, and Bi.

[0047] In some refinements, each R 2 are the same or different and are a bond to another Si atom of the repeating structure, or are selected from the group consisting of: hydrogen, -C 1 -C 10 Alkyl, -C 2 -C 10 Alkenyl, -C 3 -C 10 Alkynyl.

[0048] In the improved scheme, R 1 and R 2 Each carbon atom and / or hydrogen atom in is independently optionally substituted by deuterium, halogen, -OH, -CN, -OR 3 , -CO 2 H、-C(O)OR 3 、-C(O)NH 2 、C(O)NH(C 1 -C 10 alkyl), -C(O)N(C 1 -C 10 alkyl) 2 , SC 1 -C 10 Alkyl, -S(O)C 1 -C 10 Alkyl, -S(O) 2 C 1 -C 10 Alkyl, -S(O)NH(C 1 -C 10 Alkyl), S(O) 2 NH(C 1 -C 10 alkyl), -S(O)N(C 1 -C 10 alkyl) 2 、-S(O) 2 N(C 1 -C 10 alkyl) 2 、-NR 3 、-NH 2 , -C 2 H 8 N2 NH(C 1 -C 10 Alkyl), -P(C 1 -C 10 alkyl) 2 、-P(O)(C 1 -C 10 alkyl) 2 ,-PO 3 H 2 or -Si(-OC 1 -C 10 alkyl) 3 .

[0049] In the improved scheme, each R 3 Selected from the group consisting of: bond, hydrogen, deuterium, -C 1 -C 10 Alkyl, -C 2 -C 10 Alkenyl, -C 2 -C 10 Alkynyl, -C 3 -C 10 Cycloalkyl and -C 1 -C 10 Alkyl-OC 1 -C 10 Alkyl, optionally substituted and n is a positive integer.

[0050] In some variations, the first silane compound is fixed to the substrate. The first silane compound can be chemically bonded to the substrate via covalent bonds and / or non-covalent bonds.

[0051] The silane-containing antimicrobial layer is not limited by the amount of microbial inhibitory material. For example, the microbial inhibitory material may be present in an amount of about 0.1 wt. % (ie, 0.1% by weight) to about 100 wt. %.

[0052] In a variation, the silane-containing antimicrobial layer further comprises a fingerprint suppressing material. The fingerprint suppressing material comprises a second silane compound. The second silane compound can provide hydrophobic properties. In an improved solution, the fingerprint suppressing material comprises a hydrophobic and oleophilic invisible fingerprint material and / or a hydrophobic and oleophobic anti-fingerprint material. In a variation, the second silane compound is described by structure (II):

[0053]

[0054] in:

[0055] R 1 'Selected from the group consisting of: -C 1 -C 20 Alkyl, -C2 -C 20 Alkenyl and -C 3 -C 20 alkynyl groups, any of which may optionally be at least partially halogenated (e.g., fluorinated); and

[0056] R 2 ' are the same or different and are the connecting bonds to the substrate, or are selected from the group consisting of: hydrogen, -C 1 -C 10 Alkyl, -C 2 -C 10 Alkenyl and -C 3 -C 10 In the improved scheme, R 1 ' and R 2 ' can be used as above for R 1 and R 2 Same as stated.

[0057] The silane-containing antimicrobial layer is not limited by the amount of fingerprint inhibitory material. For example, the fingerprint inhibitory material may be present in an amount of about 0.1 wt.% to about 100 wt.%.

[0058] In the variant, R 1 ' and R 2 Each carbon atom and / or hydrogen atom in ' is independently optionally substituted by deuterium, halogen, -OH, -CN, -OR 3 , -CO 2 H、-C(O)OR 3 、-C(O)NH 2 、C(O)NH(C 1 -C 10 alkyl), -C(O)N(C 1 -C 10 alkyl) 2 , SC 1 -C 10 Alkyl, -S(O)C 1 -C 10 Alkyl, -S(O) 2 C 1 -C 10 Alkyl, -S(O)NH(C 1 -C 10 Alkyl), -S(O) 2 NH(C 1 -C 10 alkyl), -S(O)N(C 1 -C 10 alkyl) 2 、-S(O) 2 N(C 1-C 10 alkyl) 2 、-NR 3 、-NH 2 , -C 2 H 8 N 2 、-NH(C 1 -C 10 Alkyl), -P(C 1 -C 10 alkyl) 2 、-P(O)(C 1 -C 10 alkyl) 2 ,-PO 3 H 2 or -Si(-OC 1 -C 10 alkyl) 3 ; and each R 3 Selected from the group consisting of: hydrogen, deuterium, -C 1 -C 10 Alkyl, -C 2 -C 10 Alkenyl, -C 2 -C 10 Alkynyl, -C 3 -C 10 Cycloalkyl and -C 1 -C 10 Alkyl-OC 1 -C 10 Alkyl, optionally substituted.

[0059] In one variation, the at least one adhesion layer comprises a copper oxide layer composed of a copper oxide different from the antimicrobial subvalent copper oxide layer. The copper oxide can be represented by the formula Cu x O is described, wherein x is 2.2 to 0.6. In a refinement, x is at least 0.6, 0.7, 0.8, 0.9 or 0.95 and at most 2.2, 2.0, 1.8, 1.6, 1.4 or 1.2. In a refinement, the at least one adhesion layer is a copper oxide (i.e., Cu(II)O) layer. In a refinement, the copper oxide layer has a thickness of about 10 to 200 nm. In a further refinement, the copper oxide layer has a thickness of at least 5 nm, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm and at most 300 nm, 250 nm, 200 nm, 180 nm, 150 nm, 120 nm or 100 nm.

[0060] In another variant, the at least one adhesion layer comprises a zirconium oxide layer composed of zirconium oxide. Zirconium oxide can be represented by the formula Zr y O 2In another embodiment, y is about 1 and the at least one adhesion layer comprises a zirconium oxide layer (ZrO 2 ). In a refinement, the zirconium oxide layer has a thickness of about 10 to 300 nm. In a further refinement, the zirconium oxide layer has a thickness of at least 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, or 80 nm and at most 400 nm, 300 nm, 250 nm, 200 nm, 180 nm, 150 nm, 120 nm, or 100 nm.

[0061] In another variation, the at least one adhesion layer is a bilayer comprising a zirconium oxide layer and a copper oxide layer. Figure 1A and Figure 1B , the at least one adhesion layer 14 includes a zirconium oxide layer 22 disposed on and optionally in contact with the substrate 12, and a copper oxide layer 24 disposed on and optionally in contact with the zirconium oxide layer 22. As described above, the zirconium oxide can be represented by the formula Zr y O 2 In another embodiment, y is about 1 and the at least one adhesion layer comprises a zirconium oxide layer (ZrO 2 In an improved solution, the copper oxide layer 24 is made of Cu 2 O, CuO, Cu 4 O 3 or a combination thereof. In an improved embodiment, the copper oxide layer 24 is composed of a Cu x O described copper oxide, wherein x is 2.2 to 0.6. In an improved solution, x is at least 0.6, 0.7, 0.9, 0.9 or 0.95 and at most 2.2, 2.0, 1.8, 1.6, 1.4 or 1.2. In an improved solution, the at least one adhesion layer is a copper oxide (i.e., Cu(II)O) layer. In an improved solution, the zirconium oxide layer and the copper oxide layer each independently have a thickness of about 10 to 300 nm. In a further improved solution, the zirconium oxide layer and the copper oxide layer each independently have a thickness of at least 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm or 80 nm and at most 400 nm, 300 nm, 250 nm, 200 nm, 180 nm, 150 nm, 120 nm or 100 nm.

[0062] In an improved embodiment, the low-valent copper oxide layer 18 is composed of a copper oxide having the formula Cu z O, wherein z is 3 to 1.1. In a further embodiment, z is at least 1.1, 1.3, 1.5, 1.6, 1.7 or 1.8 and at most 3, 2.7, 2.5, 2.4, 2.3, 2.2 or 2.1. In a further embodiment, the subvalent copper oxide layer comprises cuprous oxide (Cu 2 O).

[0063] In a variation, the subvalent copper oxide layer 18 has a uniform stoichiometry within 20 mol% throughout the thickness of the subvalent copper oxide layer. In a refinement, the subvalent copper oxide layer has a uniform stoichiometry within 10 mol% throughout the thickness of the subvalent copper oxide layer. In another variation, the copper atomic percentage in the subvalent copper oxide layer decreases with increasing distance from the substrate. In other words, the ratio of copper to oxygen decreases with increasing distance from the substrate. Figure 2 An EDS scan is provided which provides an elemental analysis of the stainless steel substrate. The analysis shows that in the copper suboxide layer, the ratio of copper to oxygen decreases with increasing distance from the substrate.

[0064] In a variant, the subvalent copper oxide layer 18 has a dark gray non-iridescent color. When acquiring color, the subvalent copper oxide layer 18 can be characterized by Lab color space coordinates L*, a*, and b* relative to CIE standard illuminants (such as F2, L2, D65, and D50). In a modified embodiment, the subvalent copper oxide layer 18 has color space coordinates of CIE standard illuminant D65: L* of 35 to 55, a* of -5 to 5, and b* of -10 to -4.

[0065] In a variant, the copper suboxide layer comprises a plurality of crystalline pillars extending from the substrate. In a refinement, the pillars expand in a direction perpendicular to the substrate (ie, the cross-section of the pillars increases). Figure 3A and Figure 3B A SEM micrograph of the copper suboxide layer 18 is provided, showing columnar growth. Figure 4 An X-ray diffraction pattern of the subvalent copper oxide layer is provided, which reveals that the crystals are unoriented.

[0066] In a variant, the adhesive layer comprises copper oxide, wherein the antimicrobial copper suboxide layer is disposed on the adhesive layer. As set forth above, the antimicrobial copper suboxide layer is at least 5 times thicker than the adhesive layer. Advantageously, the combination of the adhesive layer and the antimicrobial copper suboxide layer does not contain other metals other than copper. In this context, free means that both the adhesive layer and the antimicrobial copper suboxide layer independently contain less than 1 mol % of other metals.

[0067] Table 1 provides the properties of an antimicrobial low-valent copper oxide layer (e.g., cuprous oxide). Table 2 provides the properties of an adhesion layer comprising a copper oxide (e.g., a cupric oxide layer). Table 3 provides the properties of an adhesion layer comprising a zirconium oxide (e.g., a zirconium oxide layer).

[0068] Table 1. Antimicrobial low-valent copper oxide layer properties

[0069]

[0070] Table 2. Copper oxide layer characteristics

[0071] Adhesion (copper oxide) layer maximum Minimum Nominal Thickness(μm) 0.5 0.01 0.05 Composition (%Cu) 67 40 50 Composition (%O) 60 33 50

[0072] Table 3. Characteristics of zirconium-containing layers

[0073]

[0074]

[0075] Table 4 provides the color characteristics of the coated stainless steel substrates.

[0076] Table 4. Color characteristics of coated products

[0077]

[0078] Table 5 provides examples of multi-layer coatings on stainless steel substrates.

[0079] Table 5. Examples of multi-layer coatings

[0080]

[0081] Although exemplary embodiments have been described above, this does not mean that these embodiments describe all possible forms of the present invention. On the contrary, the words used in this specification are descriptive, rather than restrictive, and it should be understood that various changes can be made without departing from the spirit and scope of the present invention. In addition, the features of the embodiments of different implementations can be combined to form further embodiments of the present invention.

Claims

1. A coated product comprising: Base material; at least one adhesion layer disposed on the substrate, the at least one adhesion layer comprising a component selected from the group consisting of copper oxide, zirconium oxide, and combinations thereof; as well as An antimicrobial subvalent copper oxide layer disposed on the at least one adhesive layer, wherein the antimicrobial subvalent copper oxide layer is at least 5 times thicker than the at least one adhesive layer.

2. The coated product according to claim 1, wherein The antimicrobial subvalent copper oxide layer comprises a z O, wherein z is 3 to 1.

1.

3. The coated product according to claim 1, wherein The antimicrobial subvalent copper oxide layer comprises cuprous oxide.

4. The coated product according to claim 1, wherein The at least one adhesion layer comprises a Cu x O, wherein x is from 2.2 to 0.

6.

5. The coated product according to claim 1, wherein The at least one adhesion layer comprises a Zr y O2 compound, wherein y is 3 to 0.

6.

6. The coated article according to claim 1, wherein The antimicrobial subvalent copper oxide layer has a uniform stoichiometry within 20 mol % throughout the antimicrobial subvalent copper oxide layer.

7. The coated article according to claim 1, wherein The atomic percentage of copper in the antimicrobial subvalent copper oxide layer decreases with increasing distance from the substrate.

8. The coated article of claim 1, wherein: The antimicrobial subvalent copper oxide layer has a thickness greater than 0.5 microns.

9. The coated article of claim 1, wherein: The antimicrobial subvalent copper oxide layer has a thickness of about 0.5 microns to about 10 microns.

10. The coated article of claim 1, wherein: The antimicrobial subvalent copper oxide layer has a grey non-iridescent color.

11. The coated article of claim 1, wherein: The at least one adhesion layer has a thickness of less than about 250 nm.

12. The coated article of claim 1, wherein: The at least one adhesion layer has a thickness of about 10 nm to about 200 nm.

13. The coated article of claim 1, wherein: The antimicrobial subvalent copper oxide layer includes a plurality of crystalline pillars extending from the substrate.

14. The coated article of claim 1, wherein: The antimicrobial subvalent copper oxide layer has color space coordinates for illuminant D65: L* of 35 to 55, a* of -5 to 5, and b* of -10 to -4.

15. The coated article of claim 1, further comprising a transparent metal oxide layer disposed on the antimicrobial subvalent copper oxide layer.

16. The coated article of claim 1 further comprising a silane-containing antimicrobial layer disposed on the antimicrobial subvalent copper oxide layer.

17. The coated article of claim 16, wherein: The silane-containing antimicrobial layer comprises: A microbial inhibitory material comprising: a first silane compound; and Metal ions; The first silane compound comprises a functional group that binds to the metal ion.

18. The coated article of claim 17, wherein the first silane compound is described by formula (I): in: R1 is selected from the group consisting of: -C1-C x+1 Alkyl-S(R3) y (M), -C2-C x+2 Alkenyl-S(R3) y (M), -C3-C x+3 Alkynyl-S(R3) y (M), -C1-C x Alkyl-N(R3) y (M), -C2-C x Alkenyl-N(R 3 ) y (M), -C3-C x Alkynyl-N(R3) y (M), -C1-C x+1 Alkyl-P(R3) y (M), -C2-C x+2 Alkenyl-P(R3) y (M), -C3-C x+3 Alkynyl-P(R3) y (M); Each R2 is the same or different and is a bond to another Si atom of the repeating structure, or is selected from the group consisting of hydrogen, -C1-C 10 Alkyl, -C2-C 10 Alkenyl, -C3-C 10 Alkynyl; n is a positive integer; x is a positive integer; y is a positive integer; and M is a metal ion or a metal.

19. The coated article of claim 17, wherein: The silane-containing antimicrobial layer further comprises a fingerprint inhibiting material.

20. A coated article comprising: Base material; an adhesion layer disposed on the substrate, the adhesion layer comprising copper oxide; as well as an antimicrobial subvalent copper oxide layer disposed on the adhesive layer, wherein the antimicrobial subvalent copper oxide layer is at least 5 times thicker than the adhesive layer and wherein the combination of the adhesive layer and the antimicrobial subvalent copper oxide layer is substantially free of metals other than copper.

21. The coated article of claim 20, wherein: The antimicrobial subvalent copper oxide layer comprises a z O, wherein z is 3 to 1.

1.

22. The coated article of claim 20, wherein: The antimicrobial subvalent copper oxide layer comprises cuprous oxide.

23. The coated article of claim 20, wherein: The adhesion layer comprises a Cu x O, wherein x is from 2.2 to 0.

6.

24. The coated article of claim 20, wherein: The atomic percentage of copper in the antimicrobial subvalent copper oxide layer decreases with increasing distance from the substrate.

25. The coated article of claim 20, wherein: The antimicrobial subvalent copper oxide layer has a thickness greater than 0.5 microns.

26. The coated article of claim 20, wherein: The antimicrobial subvalent copper oxide layer has a thickness of about 0.5 microns to about 10 microns.

27. The coated article of claim 20, wherein: The antimicrobial subvalent copper oxide layer has a grey non-iridescent color.

28. The coated article of claim 20, wherein: The adhesion layer has a thickness of less than about 250 nm.

29. The coated article of claim 20, wherein: The adhesion layer has a thickness of about 10 nm to about 200 nm.

30. The coated article of claim 20, wherein: The antimicrobial subvalent copper oxide layer includes a plurality of crystalline pillars extending from the substrate.

31. The coated article of claim 20, wherein: The antimicrobial subvalent copper oxide layer has color space coordinates for illuminant D65: L* of 35 to 55, a* of -5 to 5, and b* of -10 to -4.

32. The coated article of claim 20, further comprising a silane-containing antimicrobial layer disposed on the antimicrobial subvalent copper oxide layer.

33. The coated article of claim 32, wherein: The silane-containing antimicrobial layer comprises: A microbial inhibitory material comprising: a first silane compound; and Metal ions; The first silane compound comprises a functional group that binds to the metal ion.

34. The coated article of claim 33, wherein the first silane compound is described by formula (I): in: R1 is selected from the group consisting of: -C1-C x+1 Alkyl-S(R3) y (M), -C2-C x+2 Alkenyl-S(R3) y (M), -C3-C x+3 Alkynyl-S(R3) y (M), -C1-C x Alkyl-N(R3) y (M), -C2-C x Alkenyl-N(R3) y (M), -C3-C x Alkynyl-N(R3) y (M), -C1-C x+1 Alkyl-P(R3) y (M), -C2-C x+2 Alkenyl-P(R3) y (M), -C3-C x+3 Alkynyl-P(R3) y (M); Each R2 is the same or different and is a bond to another Si atom of the repeating structure, or is selected from the group consisting of hydrogen, -C1-C 10 Alkyl, -C2-C 10 Alkenyl, -C3-C 10 Alkynyl; n is a positive integer; x is a positive integer; y is a positive integer; and M is a metal ion or a metal.

35. The coated article of claim 33, wherein: The silane-containing antimicrobial layer further comprises a fingerprint inhibiting material.