Optical coating process for large-angle antireflection film with wave band of 1510-1575 nm

Through the combination of magnetron sputtering equipment and Nb2O5/SiO2/Si film system, the problem of preparing large-angle anti-reflection coatings in the 1510nm-1575nm band has been solved, efficient optical coatings have been achieved, and the anti-reflection performance of optical devices and coating layers have been improved. quality.

CN118773546APending Publication Date: 2024-10-15江苏先导微电子科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410771119.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve optical coating of large-angle (AOI=40-66°) anti-reflective films in the 1510nm-1575nm band, and the traditional process has deficiencies in anti-reflective performance.

Method used

Magnetron sputtering equipment is used, combined with medium frequency Nb2O5 and Si targets, and the coating is prepared through an RF ion source. The single crystal silicon transmission characteristics and high refractive index of the Nb2O5/SiO2/Si film system are used to achieve high precision and high controllability. The coating layer is deposited to ensure the stability and reliability of the process.

Benefits of technology

The optical coating of large angle (AOI=40-66°) anti-reflection film in the 1510nm-1575nm band is realized, which improves the anti-reflection performance of optical devices, reduces material absorption, and improves the stacking density and compactness of the coating layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773546A_ABST
    Figure CN118773546A_ABST
Patent Text Reader

Abstract

The invention discloses an optical coating process of a large-angle antireflection film with a wave band of 1510-1575 nm. The optical coating process comprises the following steps: S1, cleaning the surface of a substrate; s2, selecting a pair of intermediate-frequency Nb2O5 targets, a pair of intermediate-frequency Si targets and an RF ion source for a process cavity of magnetron sputtering equipment; s3, the base is fixed to the lower surface of the rotating table, and the process cavity is vacuumized; s4, cleaning the substrate by adopting an RF ion source; s5, the Nb2O5 / SiO2 / Si film system data are grabbed by the magnetron sputtering equipment; s6, the rotating table drives the substrate to rotate, and rotation of targets, corresponding to the plated film layer, in the pair of intermediate-frequency Nb2O5 targets and the pair of intermediate-frequency Si targets is started based on Nb2O5 / SiO2 / Si film system data; simultaneously starting medium-frequency power supplies and RF ion sources corresponding to the pair of medium-frequency Nb2O5 targets and the pair of medium-frequency Si targets, correspondingly controlling the introduction or non-introduction of Ar gas and the introduction or non-introduction of oxygen, and maintaining the exhaust of the process cavity so as to maintain the flow type pressure of the process chamber; and S7, plating the whole film system according to the film system data.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of optical coating technology, and more specifically to an optical coating technology for a large-angle anti-reflection film in the 1510nm-1575nm band. Background Art

[0002] With the continuous development of optical technology, the performance requirements for optical devices are also increasing. Especially in specific bands, such as the 1510nm-1575nm band, the anti-reflection performance requirements for optical devices are extremely high. Therefore, it is of great significance to develop an optical coating process that can achieve a large-angle (AOI = 40-66°) anti-reflection film (Rs, Rp < 1.0%) in the 1510nm-1575nm band. Summary of the invention

[0003] In view of the problems existing in the background technology, an object of the present invention is to provide an optical coating process for a large-angle anti-reflection film in the 1510nm-1575nm band, which can realize the optical coating of a large-angle (AOI=40-66°) anti-reflection film (Rs, Rp<1.0%) in the 1510nm-1575nm band.

[0004] Thus, an optical coating process for a large-angle anti-reflection film in the 1510nm-1575nm band includes the following steps: S1, cleaning the surface of a substrate; S2, selecting a pair of medium-frequency Nb2O5 targets, a pair of medium-frequency Si targets, and an RF ion source for a process chamber of a magnetron sputtering device, wherein the pair of medium-frequency Nb2O5 targets, the pair of medium-frequency Si targets, and the RF ion source are all below a rotating table at the top of the process chamber; S3, fixing the base on the lower surface of the rotating table, and evacuating the process chamber to a vacuum of less than 9.0×10 -5Pa; S4, using RF ion source to clean the surface of the substrate; S5, magnetron sputtering equipment captures Nb2O5 / SiO2 / Si film system data, when a pair of medium-frequency Nb2O5 targets are used to deposit Nb2O5 film layers, Ar gas is introduced at the position of a pair of medium-frequency Nb2O5 targets, and oxygen is introduced at the RF ion source and the process chamber is kept exhausted; when a pair of medium-frequency Si targets are used to deposit SiO2 film layers, Ar gas is introduced at the position of a pair of medium-frequency Si targets, and oxygen is introduced at the RF ion source and the process chamber is kept exhausted; when a pair of medium-frequency Si targets are used to deposit Si film layers, Ar gas is introduced at the position of a pair of medium-frequency Si targets, and oxygen is not introduced at the RF ion source but Ar gas is introduced. And maintain the exhaust of the process chamber; S6, the turntable drives the substrate to rotate, and based on the Nb2O5 / SiO2 / Si film system data, start the rotation of the targets corresponding to the coated film layer in a pair of medium frequency Nb2O5 targets and a pair of medium frequency Si targets, and at the same time, start the medium frequency power supply and RF ion source corresponding to the pair of medium frequency Nb2O5 targets and a pair of medium frequency Si targets, and correspondingly control the introduction or non-introduction of Ar gas and the introduction or non-introduction of oxygen, and maintain the exhaust of the process chamber to maintain the flow pressure of the process chamber; S7, after the entire film system is plated according to the film system data, turn off the medium frequency power supply and RF ion source, stop the introduction of Ar gas and oxygen, stop exhausting the process chamber, and stop the rotation of the turntable.

[0005] The beneficial effects of the present disclosure are as follows.

[0006] In the optical coating process of the large-angle anti-reflection film in the 1510nm-1575nm band according to the present disclosure, the optical coating of the large-angle (AOI=40-66°) anti-reflection film (Rs, Rp<1.0%) in the 1510nm-1575nm band can be achieved, thereby effectively improving the anti-reflection performance of optical devices.

[0007] In the optical coating process of the large-angle anti-reflection film in the 1510nm-1575nm band according to the present disclosure, three types of Nb2O5 / SiO2 / Si thin films are obtained by using two target materials, Nb2O5 target and Si target. This film system structure utilizes the transmission characteristics of single crystal silicon in the infrared band and the higher material refractive index, which can effectively reduce the coating thickness and improve the preparation efficiency.

[0008] Compared with traditional magnetron optics and electron beam evaporation optical processes, in the optical coating process of large-angle anti-reflection film in the 1510nm-1575nm band according to the present invention, the method of medium-frequency magnetron sputtering plus RF ion source post-oxidation has the characteristics of high precision and high controllability, and can achieve precise control of the coating layer to ensure the stability and reliability of the process; it has higher film forming energy and film forming rate, can improve the stacking density and compactness of the film layer, can effectively increase the refractive index of high-refractive materials, and reduce material absorption. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 It is a schematic structural diagram of the magnetron sputtering equipment used in the optical coating process of the large-angle anti-reflection film in the 1510nm-1575nm band according to the present disclosure.

[0010] Figure 2 It is a flow chart of the optical coating process of the large-angle anti-reflection film in the 1510nm-1575nm band according to the present disclosure.

[0011] Figures 3 to 5 yes Figure 2 The single-layer film spectral data in the film system data captured by the magnetron sputtering equipment in the flowchart, wherein at least four single-layer films with a thickness of 1 / 4 wavelength of three types of films Nb2O5 / SiO2 / Si are respectively deposited on the cleaned BK7 optical glass according to steps S1 to S5, and then the spectral data of the material is tested by a spectrophotometer.

[0012] Figure 6 and Figure 7 is based on Figure 2 The flowchart is a test data chart of the reflectivity of the substrate at 40° incident angle and 66° incident angle in the 1510nm-1575nm band after the entire film system is plated on the SK2 substrate. DETAILED DESCRIPTION

[0013] The accompanying drawings show embodiments of the present disclosure, and it will be understood that the disclosed embodiments are merely examples of the present disclosure, and the present disclosure can be implemented in various forms. Therefore, the specific details disclosed herein should not be interpreted as limiting, but merely as the basis for the claims and as a representative basis for teaching ordinary technicians in the field to implement the present disclosure in various ways.

[0014] [Optical coating process of large-angle anti-reflection film in the 1510nm-1575nm band]

[0015] Reference Figures 1 to 5 According to the optical coating process of the 1510nm-1575nm band large-angle anti-reflection film disclosed in the present invention, the steps include:

[0016] S1, cleaning the surface of the substrate;

[0017] S2, a pair of medium frequency Nb2O5 targets, a pair of medium frequency Si targets, and an RF ion source are selected for the process chamber of the magnetron sputtering equipment, wherein the pair of medium frequency Nb2O5 targets, the pair of medium frequency Si targets, and the RF ion source are all lower than the rotating table at the top of the process chamber,

[0018] S3, fix the base on the lower surface of the rotating table, and evacuate the process chamber to less than 9.0×10 -5 Pa;

[0019] S4, cleaning the surface of the substrate using an RF ion source;

[0020] S5, magnetron sputtering equipment captures Nb2O5 / SiO2 / Si film system data, when a pair of medium frequency Nb2O5 targets are used to deposit Nb2O5 film layers, Ar gas is introduced at the position of a pair of medium frequency Nb2O5 targets, and oxygen is introduced at the RF ion source and maintained to be vacuumed, when a pair of medium frequency Si targets are used to deposit SiO2 film layers, Ar gas is introduced at the position of a pair of medium frequency Si targets, and oxygen is introduced at the RF ion source and maintained to be exhausted in the process chamber, when a pair of medium frequency Si targets are used to deposit Si film layers, Ar gas is introduced at the position of a pair of medium frequency Si targets, oxygen is not introduced at the RF ion source, but Ar gas is introduced and maintained to be exhausted in the process chamber;

[0021] S6, the rotating table drives the substrate to rotate, and based on the Nb2O5 / SiO2 / Si film system data, the rotation of the target corresponding to the plated film layer in the pair of intermediate frequency Nb2O5 targets and the pair of intermediate frequency Si targets is started, and the intermediate frequency power supply and RF ion source corresponding to the pair of intermediate frequency Nb2O5 targets and the pair of intermediate frequency Si targets are started at the same time, and the introduction or non-introduction of Ar gas and the introduction or non-introduction of oxygen are controlled accordingly, and the process chamber is exhausted to maintain the flow pressure of the process chamber;

[0022] S7, after the entire film system is plated according to the film system data, the intermediate frequency power supply and the RF ion source are turned off, the introduction of Ar gas and oxygen is stopped, the exhaust of the process chamber is stopped, and the rotation of the turntable is stopped.

[0023] In the optical coating process of the large-angle anti-reflection film in the 1510nm-1575nm band according to the present disclosure, as verified by the subsequent test process, the optical coating of the large-angle (AOI=40-66°) anti-reflection film (Rs, Rp<1.0%) in the 1510nm-1575nm band can be achieved, thereby effectively improving the anti-reflection performance of optical devices.

[0024] In the optical coating process of the large-angle anti-reflection film in the 1510nm-1575nm band according to the present disclosure, three types of Nb2O5 / SiO2 / Si thin films are obtained by using two target materials, Nb2O5 target and Si target. This film system structure utilizes the transmission characteristics of single crystal silicon in the infrared band and the higher material refractive index, which can effectively reduce the coating thickness and improve the preparation efficiency.

[0025] Compared with traditional magnetron optics and electron beam evaporation optical processes, in the optical coating process of large-angle anti-reflection film in the 1510nm-1575nm band according to the present invention, the method of medium-frequency magnetron sputtering plus RF ion source post-oxidation has the characteristics of high precision and high controllability, and can achieve precise control of the coating layer to ensure the stability and reliability of the process; it has higher film forming energy and film forming rate, can improve the stacking density and compactness of the film layer, can effectively increase the refractive index of high-refractive materials, and reduce material absorption.

[0026] In one example, in step S1 , the substrate BK7 optical glass is used to collect single-layer film data, and the SK2 optical glass is used for the final sample.

[0027] In one example, in step S1, the substrate is first cleaned by ultrasonic wave. Specifically, the substrate is cleaned by ultrasonic wave vibration in pure water, with the ultrasonic wave frequency of 50KHz, temperature of 45°C and power of 400W.

[0028] In one example, in step S2, the purity of the Nb2O5 target and the Si target is 5N.

[0029] In one example, in step S4, the process parameters for RF ion source cleaning are: 100 sccm argon gas is introduced into the RF ion source, the cleaning time is 3 minutes, the RF ion source power is set to 4KW, the forward power is 3.994KW, and the reverse power is 6W.

[0030] In step S5, the process of acquiring the Nb2O5 / SiO2 / Si film system data captured by the magnetron sputtering device includes the following sub-steps:

[0031] Sa, at least four single-layer films with a thickness of 1 / 4 wavelength of three kinds of films of Nb2O5 / SiO2 / Si are deposited on the cleaned BK7 substrate, and then the spectral data of the materials are tested by a spectrophotometer;

[0032] Sb, using TFC to calculate the refractive index data of the three film layers in the required band through spectral data;

[0033] Sc, using TFC to simulate the overall reflectivity Rs and Rp < 1.0% at an incident angle of 40-66° and a wavelength range of 1510nm-1575nm on the SK2 substrate, and obtain the data of the Nb2O5 / SiO2 / Si film system;

[0034] Sd, import the obtained Nb2O5 / SiO2 / Si film system data into the control system of the magnetron sputtering coating machine.

[0035] Further, in step Sc, the Nb2O5 / SiO2 / Si film system data is that 13 film layers of Nb2O5 / SiO2 / Si / Nb2O5 / SiO2 / Nb2O5 / Si / Nb2O5 / Si / SiO2 / Si / Nb2O5 / SiO2 are deposited on the substrate in sequence, and the thickness of the first Nb2O5 film layer is The thickness of the second SiO2 film The thickness of the third Si film layer The thickness of the fourth Nb2O5 film The thickness of the fifth SiO2 film layer The thickness of the sixth Nb2O5 film The thickness of the seventh Si film layer The thickness of the eighth Nb2O5 film The thickness of the ninth Si film layer Thickness of the tenth SiO2 film layer The thickness of the eleventh Si film layer The thickness of the twelfth Nb2O5 film The thickness of the thirteenth SiO2 film layer

[0036] Further, in one example, in step S6, the rotation speed of the rotating table is 250rpm; based on the Nb2O5 / SiO2 / Si film system data, when each Nb2O5 film layer is plated: the power of the medium frequency power supply of a pair of Nb2O5 targets is 12KW; the flow rate of Ar gas at a pair of Nb2O5 targets is 200sccm, the flow rate of oxygen at the RF ion source is 100sccm, the RF ion source power is set to 4KW, the forward power is 3.992KW, and the reverse power is 8W; the deposition rate of the Nb2O5 film layer is The flow pressure is 2.2×10 -1 Pa. Corresponding to the Nb2O5 / SiO2 / Si film system data, the number of deposition turns of the first Nb2O5 film layer is 1263; the number of deposition turns of the fourth Nb2O5 film layer is 961; the number of deposition turns of the sixth Nb2O5 film layer is 3867; the number of deposition turns of the eighth Nb2O5 film layer is 3317; and the number of deposition turns of the twelfth Nb2O5 film layer is 2957.

[0037] Further, in one example, in step S6, the rotation speed of the rotating table is 250rpm; based on the Nb2O5 / SiO2 / Si film system data, when each SiO2 film layer is plated: the power of the medium frequency power supply of a pair of Si targets is 6KW; the flow rate of Ar gas at a pair of Si targets is 200sccm, the flow rate of oxygen at the RF ion source is 100sccm, the RF ion source is set to 4KW, the forward power is 3.994KW, and the reverse power is 6W; the deposition rate of the SiO2 film layer is The flow pressure is 2.2×10 -1 Pa. Corresponding to the Nb2O5 / SiO2 / Si film system data, the deposition number of the second SiO2 film layer is 1294; the deposition number of the fifth SiO2 film layer is 4169; the deposition number of the tenth SiO2 film layer is 1435; and the deposition number of the thirteenth SiO2 film layer is 4036.

[0038] Further, in one example, in step S6, the rotation speed of the rotating table is 250rpm; based on the Nb2O5 / SiO2 / Si film system data, when each Si film layer is plated: the power of the medium frequency power supply at a pair of Si targets is 10KW; the flow rate of the Ar gas at a pair of Si targets is 200sccm; the flow rate of the Ar gas at the RF ion source is 100sccm; the power of the RF ion source is set to 4KW, the forward power is 3.998KW, and the reverse power is 2W; the deposition rate of the Si film layer is The flow pressure is 2.0×10 -1 Pa. Corresponding to the data of the Nb2O5 / SiO2 / Si film system, the deposition number of the third Si film layer is 2510; the deposition number of the seventh Si film layer is 1164; the deposition number of the ninth Si film layer is 639; and the deposition number of the eleventh Si film layer is 502.

[0039] [test]

[0040] Example 1

[0041] Reference Figure 1 and Figure 2 , Example 1 adopts the following steps:

[0042] S1, cleaning the surface of the substrate, the substrate is SK2 optical glass, and the substrate is cleaned by ultrasonic vibration in pure water, the ultrasonic frequency is 50KHz, the temperature is 45°C, and the power is 400W;

[0043] S2, a pair of medium frequency Nb2O5 targets, a pair of medium frequency Si targets, and an RF ion source are selected for the process chamber of the magnetron sputtering equipment, the pair of medium frequency Nb2O5 targets, the pair of medium frequency Si targets, and the RF ion source are all lower than the rotating table at the top of the process chamber, and the purity of the Nb2O5 target and the Si target is 5N;

[0044] S3, fix the base on the lower surface of the rotating table, and evacuate the process chamber to 5.0×10 -5 Pa;

[0045] S4, using an RF ion source to clean the surface of the substrate, the process parameters of the RF ion source cleaning are: 100 sccm of argon gas is introduced into the RF ion source, the cleaning time is 3 minutes, the RF ion source power is set to 4KW, the forward power is 3.994KW, and the reverse power is 6W;

[0046] S5, magnetron sputtering equipment captures Nb2O5 / SiO2 / Si film system data, when a pair of medium frequency Nb2O5 targets are used to deposit Nb2O5 film layers, Ar gas is introduced at the position of a pair of medium frequency Nb2O5 targets, oxygen is introduced at the RF ion source, and the process chamber is kept exhausted; when a pair of medium frequency Si targets are used to deposit SiO2 film layers, Ar gas is introduced at the position of a pair of medium frequency Si targets, oxygen is introduced at the RF ion source, and the process chamber is kept exhausted; when a pair of medium frequency Si targets are used to deposit Si film layers, Ar gas is introduced at the position of a pair of medium frequency Si targets, oxygen is not introduced at the RF ion source, but Ar gas is introduced, and the process chamber is kept exhausted;

[0047] S6, the rotating table drives the substrate to rotate, and based on the Nb2O5 / SiO2 / Si film system data, the rotation of the target corresponding to the plated film layer in the pair of intermediate frequency Nb2O5 targets and the pair of intermediate frequency Si targets is started, and the intermediate frequency power supply and RF ion source corresponding to the pair of intermediate frequency Nb2O5 targets and the pair of intermediate frequency Si targets are started at the same time, and the introduction or non-introduction of Ar gas and the introduction or non-introduction of oxygen are controlled accordingly, and the process chamber is exhausted to maintain the flow pressure of the process chamber;

[0048] S7, after the entire film system is plated according to the film system data, the intermediate frequency power supply and the RF ion source are turned off, the introduction of Ar gas and oxygen is stopped, the exhaust of the process chamber is stopped, and the rotation of the turntable is stopped;

[0049] Among them, in step S5, the process of acquiring the Nb2O5 / SiO2 / Si film system data captured by the magnetron sputtering equipment includes the following sub-steps:

[0050] Sa, at least four single-layer films of 1 / 4 wavelength thickness of three types of Nb2O5 / SiO2 / Si were deposited on the cleaned BK7 substrate, and then the optical properties of the materials were tested by spectrophotometer.

[0051] Spectral data, such as Figures 3 to 5 As shown;

[0052] Sb, using TFC to calculate the refractive index of the three layers in the required band through spectral data

[0053] According to, as shown in the following table;

[0054]

[0055] Sc, using TFC to simulate the overall reflectivity Rs and Rp <1.0% on the SK2 substrate at an incident angle of 40-66° and a wavelength range of 1510nm-1575nm, the data of the Nb2O5 / SiO2 / Si film system are obtained, as shown in the following table.

[0056]

[0057] Among them, in step S6,

[0058] The rotation speed of the rotating table was 250 rpm;

[0059] Based on the Nb2O5 / SiO2 / Si film system data, when each Nb2O5 film layer is deposited: the power of the medium frequency power supply of a pair of Nb2O5 targets is 12KW; the flow rate of Ar gas at a pair of Nb2O5 targets is 200sccm, the flow rate of oxygen at the RF ion source is 100sccm, the RF ion source power is set to 4KW, the forward power is 3.992KW, and the reverse power is 8W; the deposition rate of the Nb2O5 film layer is The flow pressure is 2.2×10 -1 Pa; corresponding to the Nb2O5 / SiO2 / Si film system data, the number of deposition cycles of the first Nb2O5 film layer is 1263; the number of deposition cycles of the fourth Nb2O5 film layer is 961; the number of deposition cycles of the sixth Nb2O5 film layer is 3867; the number of deposition cycles of the eighth Nb2O5 film layer is 3317; the number of deposition cycles of the twelfth Nb2O5 film layer is 2957;

[0060] Based on the Nb2O5 / SiO2 / Si film system data, when each SiO2 film layer is deposited: the power of the medium frequency power supply of a pair of Si targets is 6KW; the flow rate of Ar gas at a pair of Si targets is 200sccm, the flow rate of oxygen at the RF ion source is 100sccm, the RF ion source power is set to 4KW, the forward power is 3.994KW, and the reverse power is 6W; the deposition rate of the SiO2 film layer is

[0061] The flow pressure is 2.2×10 -1 Pa; corresponding to the Nb2O5 / SiO2 / Si film system data, the number of deposition turns of the second SiO2 film layer is 1294 turns; the number of deposition turns of the fifth SiO2 film layer is 4169 turns; the number of deposition turns of the tenth SiO2 film layer is 1435 turns; the number of deposition turns of the thirteenth SiO2 film layer is 4036 turns.

[0062] Based on the Nb2O5 / SiO2 / Si film system data, when each Si film layer is deposited: the power of the medium frequency power supply at a pair of Si targets is 10KW; the flow rate of Ar gas at a pair of Si targets is 200sccm; the flow rate of Ar gas at the RF ion source is 100sccm; the RF ion source power is set to 4KW, the forward power is 3.998KW, and the reverse power is 2W; the deposition rate of the Si film layer is The flow pressure is 2.0×10 -1 Pa; corresponding to the Nb2O5 / SiO2 / Si film system data, the number of deposition turns of the third Si film layer is 2510 turns; the number of deposition turns of the seventh Si film layer is 1164 turns; the number of deposition turns of the ninth Si film layer is 639 turns; the number of deposition turns of the eleventh Si film layer is 502 turns.

[0063] Figure 6 and Figure 7 is based on Figure 2 The flow chart shows the test data of the reflectivity of the substrate at 40° and 66° incident angles in the 1510nm-1575nm band after the entire film system is plated on the SK2 substrate.

[0064] from Figure 6 and Figure 7 It can be seen that in the 1510nm-1575nm band (AOI=40-66°), the reflectivities Rs and Rp are <1.0%.

[0065] The above detailed description is used to describe multiple exemplary embodiments, but this document is not intended to be limited to the explicitly disclosed combinations. Therefore, unless otherwise stated, the various features disclosed herein can be combined together to form multiple additional combinations that are not shown for the sake of simplicity.

Claims

1. An optical coating process for a large-angle anti-reflection film in the 1510nm-1575nm band, comprising the steps of: S1, cleaning the surface of the substrate; S2, a pair of medium frequency Nb2O5 targets, a pair of medium frequency Si targets, and an RF ion source are selected for the process chamber of the magnetron sputtering equipment, wherein the pair of medium frequency Nb2O5 targets, the pair of medium frequency Si targets, and the RF ion source are all lower than the rotating table at the top of the process chamber, S3, fix the base on the lower surface of the rotating table, and evacuate the process chamber to less than 9.0×10 -5 Pa; S4, cleaning the surface of the substrate using an RF ion source; S5, magnetron sputtering equipment captures Nb2O5 / SiO2 / Si film system data, when a pair of medium frequency Nb2O5 targets are used to deposit Nb2O5 film layers, Ar gas is introduced at the position of a pair of medium frequency Nb2O5 targets, oxygen is introduced at the RF ion source, and the process chamber is kept exhausted; when a pair of medium frequency Si targets are used to deposit SiO2 film layers, Ar gas is introduced at the position of a pair of medium frequency Si targets, oxygen is introduced at the RF ion source, and the process chamber is kept exhausted; when a pair of medium frequency Si targets are used to deposit Si film layers, Ar gas is introduced at the position of a pair of medium frequency Si targets, oxygen is not introduced at the RF ion source, but Ar gas is introduced, and the process chamber is kept exhausted; S6, the rotating table drives the substrate to rotate, and based on the Nb2O5 / SiO2 / Si film system data, the rotation of the target corresponding to the plated film layer in the pair of intermediate frequency Nb2O5 targets and the pair of intermediate frequency Si targets is started, and the intermediate frequency power supply and RF ion source corresponding to the pair of intermediate frequency Nb2O5 targets and the pair of intermediate frequency Si targets are started at the same time, and the introduction or non-introduction of Ar gas and the introduction or non-introduction of oxygen are controlled accordingly, and the process chamber is exhausted to maintain the flow pressure of the process chamber; S7, after the entire film system is plated according to the film system data, the intermediate frequency power supply and the RF ion source are turned off, the introduction of Ar gas and oxygen is stopped, the exhaust of the process chamber is stopped, and the rotation of the turntable is stopped.

2. The optical coating process of the 1510nm-1575nm band wide angle anti-reflection film according to claim 1, characterized in that: In step S1, the sample substrate is SK2 optical glass and BK7 optical glass is used to collect single-layer film data.

3. The optical coating process of the 1510nm-1575nm wide-angle anti-reflection film according to claim 1, characterized in that: In step S1 , the substrate is first cleaned using ultrasonic waves.

4. The optical coating process of the 1510nm-1575nm band wide angle anti-reflection film according to claim 1, characterized in that: In step S2, the purity of the Nb2O5 target and the Si target is 5N.

5. The optical coating process of the 1510nm-1575nm wide-angle anti-reflection film according to claim 1, characterized in that: In step S4, the process parameters for RF ion source cleaning are: 100 sccm argon gas is introduced into the RF ion source, the cleaning time is 3 minutes, the RF ion source power is set to 4KW, the forward power is 3.994KW, and the reverse power is 6W.

6. The optical coating process of the 1510nm-1575nm wide-angle anti-reflection film according to claim 2, characterized in that: In step S5, the process of acquiring the Nb2O5 / SiO2 / Si film system data captured by the magnetron sputtering device includes the following sub-steps: Sa, at least four single-layer films with a thickness of 1 / 4 wavelength of three kinds of films of Nb2O5 / SiO2 / Si are deposited on the cleaned BK7 substrate, and then the spectral data of the materials are tested by a spectrophotometer; Sb, using TFC to calculate the refractive index data of the three film layers in the required band through spectral data; Sc, using TFC to simulate the overall reflectivity Rs and Rp < 1.0% at an incident angle of 40-66° and a wavelength range of 1510nm-1575nm on the SK2 substrate, and obtain the data of the Nb2O5 / SiO2 / Si film system; Sd, import the obtained Nb2O5 / SiO2 / Si film system data into the control system of the magnetron sputtering coating machine.

7. The optical coating process of the 1510nm-1575nm wide-angle anti-reflection film according to claim 6, characterized in that: In step Sc, The data of Nb2O5 / SiO2 / Si film system is that 13 film layers are deposited on the substrate in sequence: Nb2O5 / SiO2 / Si / Nb2O5 / SiO2 / Nb2O5 / Si / Nb2O5 / Si / SiO2 / Si / Nb2O5 / SiO2. The thickness of the first Nb2O5 film The thickness of the second SiO2 film The thickness of the third Si film layer The thickness of the fourth Nb2O5 film The thickness of the fifth SiO2 film layer The thickness of the sixth Nb2O5 film The thickness of the seventh Si film layer The thickness of the eighth Nb2O5 film The thickness of the ninth Si film layer Thickness of the tenth SiO2 film layer The thickness of the eleventh Si film layer The thickness of the twelfth Nb2O5 film The thickness of the thirteenth SiO2 film layer 8. The optical coating process of the 1510nm-1575nm wide-angle anti-reflection film according to claim 7, characterized in that: In step S6, The rotation speed of the rotating table was 250 rpm; Based on the Nb2O5 / SiO2 / Si film system data, when coating each Nb2O5 film layer: The power of the medium frequency power supply for a pair of Nb2O5 targets is 12KW; The flow rate of Ar gas at a pair of Nb2O5 targets is 200sccm. The oxygen flow rate at the RF ion source is 100 sccm. The RF ion source was set to 4KW, with a forward power of 3.992KW and a reverse power of 8W; The deposition rate of Nb2O5 film is / lock up; The flow pressure is 2.2×10 -1 Pa; The number of deposition cycles of the first Nb2O5 film layer is 1263; The deposition number of the fourth Nb2O5 film layer is 961; The deposition number of the sixth Nb2O5 film layer is 3867; The deposition number of the eighth Nb2O5 film layer is 3317; The deposition number of the twelfth Nb2O5 film layer is 2957.

9. The optical coating process of the 1510nm-1575nm wide-angle anti-reflection film according to claim 7, characterized in that: In step S6, The rotation speed of the rotating table was 250 rpm; Based on the Nb2O5 / SiO2 / Si film system data, when coating each SiO2 film layer: The power of the medium frequency power supply for a pair of Si targets is 6KW; The flow rate of Ar gas at a pair of Si targets is 200 sccm. The oxygen flow rate at the RF ion source is 100 sccm. The RF ion source was set to 4KW, with a forward power of 3.994KW and a reverse power of 6W; The deposition rate of SiO2 film is / lock up; The flow pressure is 2.2×10 -1 Pa; The deposition number of the second SiO2 film layer is 1294; The deposition number of the fifth SiO2 film layer is 4169; The number of deposition turns of the tenth SiO2 film layer is 1435 turns; The deposition number of the thirteenth SiO2 film layer is 4036.

10. The optical coating process of the 1510nm-1575nm wide-angle anti-reflection film according to claim 7, characterized in that: In step S6, The rotation speed of the rotating table was 250 rpm; Based on the Nb2O5 / SiO2 / Si film system data, when coating each Si film layer: The power of the medium frequency power supply at a pair of Si targets is 10KW; The flow rate of Ar gas at a pair of Si targets is 200 sccm; The flow rate of Ar gas at the RF ion source was 100 sccm; The RF ion source was set to 4KW, with a forward power of 3.998KW and a reverse power of 2W; Deposition rate of Si film / lock up; The flow pressure is 2.0×10 -1 Pa; The deposition number of the third Si film layer is 2510; The number of deposition turns of the seventh Si film layer is 1164 turns; The deposition number of the ninth Si film layer is 639; The deposition number of the eleventh Si film layer is 502.