Thermal control sunshade cloth and preparation method thereof
By providing a base cloth layer, light absorbing layer, first optical coating and second optical coating in the sunshade cloth, the sunlight reflectivity is improved and the existing sunshade cloth reflection is solved by using components such as aluminum powder, resin and titanium dioxide. The problem of insufficient rate improves the insulation and comfort of the sunshade cloth.
Patent Information
- Application Number
- CN202411487171.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-11-22
AI Technical Summary
The sunlight reflectivity of the sunshade cloth on the market is relatively low, resulting in the heating and cooling load of the building, and the comfort level decreases.
The base cloth layer, the light absorbing layer, the first optical coating and the second optical coating are arranged in sequence, and the sunlight reflectivity is increased by controlling the composition of the coating, including the light absorbing coating, the first optical coating and the second optical coating, respectively Components such as aluminum powder, resin, titanium dioxide and sheet-like wide band gap filler are used to increase reflectivity and reduce transmittance.
It significantly improves the reflectivity of the sunlight, reduces the transmittance of the sunlight, improves the comfort and insulation effect of the sunshade cloth, and is suitable for a variety of sunshade applications.
Smart Images

Figure CN118996865A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sunshade materials, and in particular to a thermal control sunshade cloth and a preparation method thereof. Background Art
[0002] The sunshade cloth sold on the market generally includes a base cloth, a silver coating, a titanium dioxide coating, a calcium carbonate coating, a barium sulfate coating, etc.; in order to achieve full shading of the sunshade cloth, it is also necessary to additionally superimpose a foam coating or a black glue coating. Even so, the solar reflectivity of the obtained full shading sunshade cloth is relatively low, between 70% and 85%, and 15% to 30% of sunlight still passes through, resulting in a decrease in comfort. When used in buildings, it will lead to an increase in the temperature inside the building and the air-conditioning cooling load. Summary of the invention
[0003] In view of this, an object of the present invention is to provide a thermal control sunshade cloth and a preparation method thereof. The thermal control sunshade cloth provided by the present invention has high solar reflectivity and low solar transmittance.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The present invention provides a heat-controlled sunshade cloth, comprising a base cloth layer, a light-absorbing layer, a first optical coating layer, a second optical coating layer and an anti-fouling layer which are stacked in sequence; The coating used in the light absorbing layer is a light absorbing coating; The coating material used in the first optical coating is a first optical coating material; The coating material used in the second optical coating is a second optical coating material; The light-absorbing paint comprises aluminum powder and resin; The first optical coating comprises titanium dioxide and resin; The second optical coating comprises the following components in percentage by mass: Resin 15~30%, dispersant 0.5~3%, defoamer 0.5~3%, directional arrangement additive 2%, lamellar wide bandgap filler 10~40%, granular wide bandgap filler 10~40% and the rest solvent; The particle size of the granular wide bandgap filler is 5nm~10μm; The flaky wide bandgap filler comprises a flaky wide bandgap material and a coating layer wrapping the flaky wide bandgap material, wherein the coating layer is made of TiO2, SiO2 or Al2O3; The sheet-like wide bandgap material has a thickness of 5-500 nm, a diameter of 3-50 μm, and a diameter / thickness ratio of 10-100.
[0005] Preferably, the types of the flaky wide bandgap material and the granular wide bandgap filler independently include one or more of calcium carbonate, barium sulfate, aluminum oxide, silicon dioxide, magnesium oxide and boron nitride.
[0006] Preferably, the alignment aid comprises cellulose and / or modified polyamide wax.
[0007] Preferably, the resin independently includes acrylic resin and / or polyurethane resin; the elastic modulus of the resin is ≤10 MPa, and the elongation is ≥300%; the resin is colorless, transparent or milky white.
[0008] Preferably, the base fabric layer is made of a polymer material, and the polymer material includes one of polyester, cotton, plastic fiber, polyvinyl chloride or polyethylene-vinyl acetate. The thickness of the base fabric layer is 20-500 μm.
[0009] Preferably, the light-absorbing coating comprises the following components in percentage by mass: 20-50% aluminum powder and the remainder resin; the particle size of the aluminum powder is 1-20 μm, and the thickness of the light-absorbing layer is 3-15 μm.
[0010] Preferably, the pigment-to-base ratio of the first optical coating is 1.0-2.5, and the thickness of the first optical coating is 15-30 μm.
[0011] Preferably, the thickness of the second optical coating is 40-120 μm.
[0012] Preferably, the antifouling coating used in the antifouling layer comprises the following components in mass percentage: 1-4% hydrophobic nano-silicon dioxide, 1-5% organic silicon anti-graffiti agent, 1-5% slip agent, and the remainder of surface resin; the surface resin comprises polyurethane resin and / or acrylic resin, the elastic modulus of the surface resin is ≤10MPa, the elongation is ≥300%, and the surface resin is colorless, transparent or milky white; The thickness of the antifouling layer is 5-20 μm.
[0013] The present invention also provides a method for preparing the thermal control sunshade cloth described in the above technical solution, comprising the following steps: A light absorbing layer, a first optical coating layer, a second optical coating layer and an anti-fouling layer are sequentially stacked on the base fabric layer.
[0014] The invention provides a heat-control sunshade cloth.
[0015] The heat-control sunshade cloth of the present invention is provided with a light-absorbing layer, a first optical coating, a second optical coating and an antifouling layer which are stacked in sequence, and the material composition of the second optical coating is controlled, so that the solar reflectivity of the heat-control sunshade cloth is improved and the solar transmittance is reduced. The high solar reflectivity of the heat-control sunshade cloth provided by the present invention enables it to be well applied to indoor and outdoor sunshades, parasols, tents, sunshade awnings, sunshade hats, clothes, car sunshade canopies, car sunshade gears, sunshade car clothes and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A schematic diagram of the structure of the thermal control sunshade cloth provided by the present invention; Figure 2 This is a graph of the solar reflectivity and solar transmittance (also called transmittance) of the thermal control sunshade cloth obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0017] Figure 1 The schematic diagram of the structure of the heat control sunshade cloth provided by the present invention is shown below in combination with Figure 1 The thermal control sunshade cloth provided by the present invention is described in detail.
[0018] The present invention provides a heat-controlled sunshade cloth, comprising a base cloth layer, a light-absorbing layer, a first optical coating layer, a second optical coating layer and an anti-fouling layer which are stacked in sequence; The coating used in the light absorbing layer is a light absorbing coating; The coating material used in the first optical coating is a first optical coating material; The coating material used in the second optical coating is a second optical coating material; The light-absorbing paint comprises aluminum powder and resin; The first optical coating comprises titanium dioxide and resin; The second optical coating comprises the following components in percentage by mass: Resin 15~30%, dispersant 0.5~3%, defoamer 0.5~3%, directional arrangement additive 2%, lamellar wide bandgap filler 10~40%, granular wide bandgap filler 10~40% and the rest solvent; The particle size of the granular wide bandgap filler is 5nm~10μm; The flaky wide bandgap filler comprises a flaky wide bandgap material and a coating layer wrapping the flaky wide bandgap material, wherein the coating layer is made of TiO2, SiO2 or Al2O3; The sheet-shaped wide bandgap material has a thickness of 5-500 nm, a diameter of 3-50 μm, and a diameter / thickness ratio of 10-100.
[0019] In the present invention, unless otherwise specified, the raw materials used are preferably commercially available products.
[0020] The heat-controlled sunshade cloth provided by the present invention includes a base fabric layer, and the material of the base fabric layer is preferably a polymer material, and the polymer material preferably includes one of polyester, cotton cloth, plastic fiber, polyvinyl chloride (PVC) or polyethylene-vinyl acetate (PEVA). In the present invention, the thickness of the base fabric layer is preferably 20~500μm, more preferably 100~500μm, and specifically can be 100μm, 200μm, 300μm, 400μm or 500μm. In the present invention, the base fabric layer is a carrier of other coatings.
[0021] The heat-controlled sunshade cloth provided by the present invention includes a light-absorbing layer, and the coating used in the light-absorbing layer is a light-absorbing coating, and the light-absorbing coating includes aluminum powder and resin. In the present invention, the light-absorbing coating preferably includes the following components in mass percentage: 20-50% aluminum powder and the rest resin. In the present invention, the particle size of the aluminum powder is preferably 1-20 μm, specifically 5 μm, 10 μm, 15 μm or 20 μm. In the present invention, the resin preferably includes acrylic resin and / or polyurethane resin; the elastic modulus of the resin is preferably ≤10 MPa, and the elongation is preferably ≥300%; the resin is preferably colorless, transparent or milky white. In the present invention, the mass percentage of aluminum powder in the light-absorbing coating is further preferably 25-40%, specifically 20%, 25%, 30%, 35%, 38%, 40%, 45% or 50%. In the present invention, the thickness of the light-absorbing layer is preferably 3-15 μm, specifically 3 μm, 5 μm, 8 μm, 10 μm or 15 μm. In the present invention, the main function of the light absorbing layer is to block light and reduce the transmittance of sunlight.
[0022] The thermal control sunshade cloth provided by the present invention includes a first optical coating, and the coating used in the first optical coating is a first optical coating; the first optical coating includes titanium dioxide and a resin. In the present invention, the color-to-base ratio of the first optical coating is preferably 1.0~2.5, and can be specifically 1, 1.5, 2 or 2.5. In the present invention, the resin is preferably consistent with the type and requirements of the resin in the light-absorbing coating, which will not be repeated here. In the present invention, the particle size of the titanium dioxide is preferably 0.2~0.4μm. In the present invention, the first optical coating preferably also includes a flame retardant with a mass percentage of 3~8%, and the mass percentage of the flame retardant can be specifically 3%, 5% or 8%. In the present invention, the flame retardant is preferably a halogen-free environmentally friendly phosphate flame retardant, and the model of the halogen-free environmentally friendly phosphate flame retardant is specifically preferably 9000B, 6000-5 or FR-105. In the present invention, the thickness of the first optical coating is preferably 15-30 μm, preferably 20-30 μm, and specifically can be 15 μm, 20 μm, 25 μm or 30 μm. In the present invention, the first optical coating can cover the light absorbing layer, increase the reflectivity, and further reduce the sunlight transmittance.
[0023] The thermal control sunshade cloth provided by the present invention includes a second optical coating, and the coating used in the second optical coating is a second optical coating; the second optical coating includes the following components in mass percentage: 15-30% resin, 0.5-3% dispersant, 0.5-3% defoaming agent, 2% directional arrangement auxiliary agent, 10-40% flaky wide bandgap filler, 10-40% granular wide bandgap filler and 10-30% solvent.
[0024] In the present invention, the mass percentage of the resin in the second optical coating can be specifically 10%, 15%, 20%, 25% or 30%; the type and requirements of the resin are consistent with the type and requirements of the resin in the light-absorbing coating described in the above technical solution, and will not be repeated here.
[0025] In the present invention, in the second optical coating, the mass percentage of the dispersant may be 0.5%, 1%, 1.5%, 2%, 2.5% or 3%. In the present invention, the dispersant preferably includes a dispersant for solvent-based coatings or a dispersant for water-based coatings, and the dispersant for solvent-based coatings preferably includes one or more of BYK163, BYK025, BYK161, BYK108, TEGO Dispers 676 and TEGO Dispers 655; the dispersant for water-based coatings preferably includes one or more of NXZ, SN5040, AC93, SN5027 and BYK190.
[0026] In the present invention, in the second optical coating, the mass percentage of the defoamer can be 0.5%, 1%, 1.5%, 2%, 2.5% or 3%. In the present invention, the defoamer preferably includes an organosilicon defoamer, a polyether defoamer, a polyether-modified organosilicon defoamer or a mineral oil defoamer. In the present invention, the specific model of the organosilicon defoamer is BYK077 or D912R.
[0027] In the present invention, the alignment aid in the second optical coating preferably includes cellulose and / or modified polyamide wax, and more preferably cellulose. In the present invention, the cellulose is preferably CAB-381-0.5, and the modified polyamide wax is preferably Arkema CRAYVALLAC SUPER.
[0028] In the present invention, in the second optical coating, the mass percentage of the flaky wide bandgap filler can be specifically 10%, 13%, 15%, 20%, 25%, 30%, 33%, 35% or 40%. In the present invention, the flaky wide bandgap filler includes a flaky wide bandgap material and a coating layer that wraps the flaky wide bandgap material. In the present invention, the material of the coating layer is TiO2, SiO2 or Al2O3; the coating layer has a high refractive index; the thickness of the coating layer is preferably 100-300nm, specifically 100nm, 200nm or 300nm. In the present invention, the type of the flaky wide bandgap material preferably includes one or more of calcium carbonate, barium sulfate, aluminum oxide, silicon dioxide, magnesium oxide and boron nitride. In the present invention, the thickness of the flaky wide bandgap material is 5-500nm. In the present invention, the diameter of the flaky wide bandgap material is 3-50μm, preferably 5-10μm, specifically 5μm, 10μm or 50μm. In the present invention, the diameter / thickness of the sheet-like wide bandgap material is 10-100, preferably 15-30, specifically 10, 15, 30 or 100. The present invention has no particular limitation on the specific preparation method of the sheet-like wide bandgap filler, and can be prepared by methods well known to those skilled in the art, such as wet coating, vapor deposition or solid coating. The preparation method of the sheet-like wide bandgap filler is described below by taking wet coating as an example. The flaky wide bandgap material is dispersed in water to obtain a suspension having a concentration of 5wt%. The suspension is heated to 80°C, and then a 2mol / L TiCl4 solution is added dropwise to the suspension. The pH value is adjusted to 6 using a NaOH solution, and the stirring speed is controlled to 500rpm. The reacted solution is centrifuged after standing for 2h, and the solid is washed with deionized water. The centrifugal washing steps are repeated many times until the supernatant is neutral. The obtained solid is then dried in an oven at 120°C for 3h, and then calcined in a high-temperature furnace at 950°C for 3h to obtain a flaky wide bandgap filler with titanium dioxide coated on the surface.
[0029] In the present invention, in the second optical coating, the mass percentage of the granular wide bandgap filler is preferably 17-33%, specifically 10%, 15%, 17%, 20%, 25%, 30%, 33%, 35% or 40%. In the present invention, the particle size of the granular wide bandgap filler is 5nm-10μm, preferably 6nm-500nm, specifically 6nm, 10nm, 20nm, 100nm, 500nm or 1000nm. In the present invention, the type of the granular wide bandgap filler preferably includes one or more of calcium carbonate, barium sulfate, aluminum oxide, silicon dioxide, magnesium oxide and boron nitride, specifically aluminum oxide is preferred.
[0030] In the present invention, the second optical coating further comprises a residual solvent, and the mass percentage of the solvent is preferably 20%, and specifically can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 25% or 30%. In the present invention, when the second optical coating is a solvent-based coating, the solvent preferably comprises one or more of ethanol, ethyl acetate, butanone, propylene glycol methyl ether, a mixture of dibasic esters, butyl acetate, toluene, xylene, propylene glycol methyl ether acetate, dimethyl carbonate, N,N-dimethylformamide and propylene glycol; when the second optical coating is a water-based coating, the solvent is preferably water.
[0031] In the present invention, the second optical coating preferably also includes a flame retardant with a mass percentage of 3-8%, specifically 3%, 5% or 8%; the flame retardant is preferably a halogen-free environmentally friendly phosphate flame retardant, and the model of the halogen-free environmentally friendly phosphate flame retardant is specifically preferably 9000B, 6000-5 or FR-105.
[0032] In the present invention, the thickness of the second optical coating is preferably 40-120 μm, and specifically preferably 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm or 120 μm.
[0033] The thermal control sunshade provided by the present invention includes an antifouling layer. In the present invention, the antifouling coating used in the antifouling layer preferably includes the following components in mass percentage: hydrophobic nano-silicon dioxide 1-4%, silicone anti-graffiti agent 1-5%, slip agent 1-5%, and the remainder of surface resin. In the present invention, the particle size of the hydrophobic nano-silicon dioxide is preferably 20nm~200nm. In the present invention, the specific model of the silicone anti-graffiti agent is BYK3700, TEGO5000 or SSL-350. In the present invention, the slip agent preferably includes one or more of polyethylene wax, polyamide wax, silicone micropowder and polytetrafluoroethylene (PTFE) micropowder. In the present invention, the surface resin preferably includes one or more of polyurethane resin, acrylic resin, fluorocarbon resin and silicone resin, specifically polyurethane resin, the elastic modulus of the surface resin is preferably ≤10MPa, the elongation is preferably ≥300%, and the surface resin is preferably colorless, transparent or milky white. In the present invention, the thickness of the antifouling layer is preferably 5-20 μm, specifically 5 μm, 8 μm, 10 μm, 15 μm or 20 μm. In the present invention, the antifouling layer mainly plays the role of waterproofing, anti-fouling and protecting the second optical coating.
[0034] The present invention also provides a method for preparing the thermal control sunshade cloth described in the above technical solution, comprising the following steps: A light absorbing layer, a first optical coating layer, a second optical coating layer and an anti-fouling layer are sequentially stacked on the base fabric layer.
[0035] In the present invention, the method for setting the light absorbing layer preferably includes: applying a light absorbing coating, and performing subsequent operations after drying. In the present invention, the drying temperature is preferably 80-120°C; the drying time is preferably controlled by the vehicle speed, and the vehicle speed is preferably 5-30 m / min.
[0036] In the present invention, the method for setting the first optical coating preferably includes: applying the first optical coating, and performing subsequent operations after drying. In the present invention, the drying temperature is preferably 80-120°C; the drying time is preferably controlled by the vehicle speed, and the vehicle speed is preferably 5-30 m / min.
[0037] In the present invention, the method for setting the second optical coating preferably includes: applying the second optical coating, and performing subsequent operations after drying. In the present invention, the drying temperature is preferably 80-120°C; the drying time is preferably controlled by the vehicle speed, and the vehicle speed is preferably 5-30 m / min.
[0038] In the present invention, the method for setting the antifouling layer preferably includes: applying the antifouling coating, and performing subsequent operations after drying. In the present invention, the drying temperature is preferably 80-120°C; the drying time is preferably controlled by the vehicle speed, and the vehicle speed is preferably 5-30 m / min.
[0039] In the present invention, the preparation of the thermal control sunshade cloth is preferably carried out on a 2-coating 2-drying scraper device, and the specific process is: setting the temperature of the oven to 80~120℃, the vehicle speed to 5~30m / min, coating the light-absorbing coating and the first optical coating on the base fabric layer, and then rolling it up; then coating the second optical coating and anti-fouling coating, and rolling it up.
[0040] The thermal control sunshade cloth and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0041] The formulations and performance characteristics of the embodiments and comparative examples are shown in Tables 1 and 2.
[0042] raw material In the light-absorbing coating for preparing the light-absorbing layer, the mass percentage of aluminum powder is 30%, and the remainder is polyurethane resin. The particle size of the aluminum powder and the thickness of the light-absorbing layer are shown in Tables 1 and 2.
[0043] In the first optical coating for preparing the first optical coating, the particle size of titanium dioxide is 0.2-0.4 μm, the flame retardant is 9000B purchased from Doer Chemical Co., Ltd., and the balance is polyurethane resin. The pigment-to-base ratio, the amount of flame retardant added, and the thickness of the first optical coating are shown in Tables 1 and 2.
[0044] The second optical coating for preparing the second optical coating includes the following components in mass percentage: 25% resin, 1% dispersant, 1% defoamer, 2% oriented arrangement aid, 18% lamellar wide bandgap filler, 35% granular wide bandgap filler, and the flame retardant is added according to Table 1 and Table 2, and the balance is solvent, wherein the resin is acrylic resin, the dispersant is BYK163; the defoamer is an organosilicon defoamer, model BYK077; the oriented arrangement aid is cellulose, model CAB-381-0.5; the granular wide bandgap filler is aluminum oxide, and the particle size is 0.1 μm; the solvent is butyl acetate, and the flame retardant is 9000B purchased from Doer Chemical Co., Ltd.; the amount of flame retardant added and the thickness of the second optical coating are shown in Table 1 and Table 2.
[0045] Among them, the lamellar wide bandgap filler is a lamellar wide bandgap material with titanium dioxide coated on the surface, and the preparation method is as follows: wet coating: prepare a lamellar wide bandgap filler suspension with a concentration of 5wt%, heat it to 80°C, and then add 2 mol / L TiCl4 solution dropwise to the suspension, use NaOH solution to adjust the pH value to 6, control the stirring speed to 500rpm, let the reacted solution stand for 2h and then centrifuge it, wash the solid with deionized water, repeat the centrifugal washing steps many times until the supernatant is neutral, dry it in a 120°C oven for 3h, and then calcine it at 950°C in a high-temperature furnace for 3h to obtain a lamellar wide bandgap filler with titanium dioxide coated on the surface.
[0046] In the antifouling coating for preparing the antifouling coating, the particle size of the hydrophobic nano-silica is 20nm~200nm, the model of the silicone anti-graffiti additive is BYK3700, the lubricant is polyethylene wax, and the balance is polyurethane resin. The addition amount of the hydrophobic nano-silica, the addition amount of the silicone anti-graffiti additive, the addition amount of the lubricant and the thickness of the antifouling coating are shown in Tables 1 and 2.
[0047] The optical performance test method is: GB / T 2680-2021.
[0048] Other performance tests: GB / T 1733-1993 is used to test water resistance, GB / T 5454-1997 is used to test limiting oxygen index, GB / T 10707-2008 is used to test flame retardancy, ASTM D1308 is used to test stain resistance, and GB / T 6742-2007 is used to test flexibility.
[0049] Table 1 Example formulation and performance test results
[0050] The difference between Example 2 and Example 1 is that the light absorbing layer has a thickness of 3 μm and the antifouling layer has a thickness of 15 μm. The difference between Example 3 and Example 1 is that the base fabric layer uses a PET film, the light absorbing layer thickness is set to 10 μm, the color-to-base ratio of the first optical coating is 1, and the antifouling layer thickness is set to 8 μm. The difference between Example 4 and Example 1 is that the base fabric layer uses cotton cloth, the aluminum powder particle size in the light absorbing coating of the light absorbing layer is 5 μm, the light absorbing layer coating thickness is 10 μm, the first optical coating color-to-base ratio is set to 1.5, and the antifouling layer thickness is 8 μm. The difference between Example 5 and Example 1 is that the color-to-base ratio of the first optical coating is set to 2.5, the thickness is 30 μm, and the flame retardant addition ratio is 3wt%; the thickness of the second optical coating is set to 60 μm, the flame retardant addition ratio is 3wt%; the antifouling layer thickness is 15 μm. The difference between Example 6 and Example 1 is that the thickness of the first optical coating is set to 30μm, and the flame retardant addition ratio is 3wt%; the thickness of the second optical coating is 70μm, the flame retardant addition ratio is 3wt%, and the antifouling layer thickness is 15μm. The difference between Example 7 and Example 1 is that the base fabric layer uses PVC with a thickness of 200μm, the aluminum powder particle size is 20μm in the light-absorbing coating of the raw material for preparing the light-absorbing layer, and the thickness of the light-absorbing layer is 10μm; the thickness of the first optical coating is set to 30μm, and the flame retardant addition ratio is 3wt%; the thickness of the second optical coating is set to 80μm, the flame retardant addition ratio is set to 3wt%, and the antifouling layer thickness is 15μm. The difference between Example 8 and Example 1 is that the thickness of the base fabric layer is 300μm, the thickness of the first optical coating is 30μm, the flame retardant addition ratio is 3wt%; the thickness of the second optical coating is 100μm, the flame retardant addition ratio is set to 3wt%; the antifouling layer thickness is 20μm. The difference between Example 9 and Example 1 is that the base fabric layer is made of PEVA with a thickness of 500 μm, the thickness of the second optical coating is 120 μm, and the thickness of the anti-fouling layer is 10 μm.
[0051] Table 2 Comparative example formulation and performance test results
[0052] The difference between Comparative Example 1 and Example 1 is that the coating thickness of the light-absorbing layer becomes thinner, the shading effect becomes worse, and part of the sunlight is transmitted; the thickness of the first optical coating becomes thinner, resulting in a decrease in the visible light reflectivity. The difference between Comparative Example 2 and Example 1 is that the pigment-to-base ratio of the first optical coating becomes lower, resulting in a poor coverage of the light-absorbing layer by the first optical coating, and a decrease in the sunlight reflectivity of the sunshade cloth. The difference between Comparative Example 3 and Example 1 is that the thickness of the first optical coating becomes thinner, resulting in a poor coverage of the light-absorbing layer by the first optical coating, an increase in the visible light absorption of the first optical coating, and a decrease in the sunlight reflectivity of the sunshade cloth. The difference between Comparative Example 4 and Example 1 is that the thickness of the first optical coating becomes thinner and the thickness of the second optical coating becomes thinner, resulting in a decrease in the sunlight reflectivity. The difference between Comparative Example 5 and Example 1 is that the thickness of the antifouling layer becomes thinner, the antifouling performance of the sunshade cloth becomes worse, the thickness of the first optical coating becomes thinner, resulting in a poor coverage of the light-absorbing layer by the first optical coating, an increase in the visible light absorption of the first optical coating, and a decrease in the sunlight reflectivity of the sunshade cloth. The difference between Comparative Example 6 and Example 1 is that no flame retardant is added to the first optical coating and the second optical coating, and the thickness of the first optical coating becomes thinner, resulting in the flame retardant grade and limiting oxygen index of the sunshade cloth failing to meet the flame retardant requirements. The difference between Comparative Examples 7, 8, 9, and 11 and Example 1 is that no first optical coating, no light absorbing layer, no first optical coating and light absorbing layer, and no second optical coating are provided, resulting in a decrease in the optical reflectivity of the sunshade cloth or partial transmission of sunlight. The difference between Comparative Example 10 and Example 1 is that the diameter of aluminum oxide in the light absorbing layer is too large, which does not have the proper shading effect, resulting in partial transmission of sunlight. The difference between Comparative Example 11 and Example 1 is that no second optical coating is provided. Since there is no main reflective layer, the reflectivity of the sunshade to sunlight drops sharply, and the heat insulation and shading effect becomes worse.
[0053] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A thermal control sunshade cloth, characterized in that: It comprises a base fabric layer, a light absorbing layer, a first optical coating layer, a second optical coating layer and an antifouling layer which are stacked in sequence; The coating used in the light absorbing layer is a light absorbing coating; The coating material used in the first optical coating is a first optical coating material; The coating material used in the second optical coating is a second optical coating material; The light-absorbing paint comprises aluminum powder and resin; The first optical coating comprises titanium dioxide and resin; The second optical coating comprises the following components in percentage by mass: Resin 15~30%, dispersant 0.5~3%, defoamer 0.5~3%, directional arrangement additive 2%, lamellar wide bandgap filler 10~40%, granular wide bandgap filler 10~40% and the rest solvent; The particle size of the granular wide bandgap filler is 5nm~10μm; The flaky wide bandgap filler comprises a flaky wide bandgap material and a coating layer wrapping the flaky wide bandgap material, wherein the coating layer is made of TiO2, SiO2 or Al2O3; The sheet-shaped wide bandgap material has a thickness of 5-500 nm, a diameter of 3-50 μm, and a diameter / thickness ratio of 10-100.
2. The thermal control sunshade cloth according to claim 1, characterized in that: The types of the flaky wide bandgap material and the granular wide bandgap filler independently include one or more of calcium carbonate, barium sulfate, aluminum oxide, silicon dioxide, magnesium oxide and boron nitride.
3. The thermal control sunshade cloth according to claim 1, characterized in that: The alignment aid comprises cellulose and / or modified polyamide wax.
4. The thermal control sunshade cloth according to claim 1, characterized in that: The resin independently includes acrylic resin and / or polyurethane resin; the elastic modulus of the resin is ≤10MPa, and the elongation is ≥300%; the resin is colorless, transparent or milky white.
5. The thermal control sunshade cloth according to claim 1, characterized in that: The base fabric layer is made of a polymer material, which includes one of polyester, cotton, plastic fiber, polyvinyl chloride or polyethylene-vinyl acetate. The base fabric layer has a thickness of 20-500 μm.
6. The thermal control sunshade cloth according to claim 1, characterized in that: The light-absorbing coating comprises the following components in mass percentage: 20-50% aluminum powder and the remainder resin; the particle size of the aluminum powder is 1-20 μm, and the thickness of the light-absorbing layer is 3-15 μm.
7. The thermal control sunshade cloth according to claim 1, characterized in that: The pigment-to-base ratio of the first optical coating is 1.0-2.5, and the thickness of the first optical coating is 15-30 μm.
8. The thermal control sunshade cloth according to claim 1, characterized in that: The thickness of the second optical coating is 40-120 μm.
9. The thermal control sunshade cloth according to claim 1, characterized in that: The antifouling coating used in the antifouling layer includes the following components in percentage by mass: 1-4% hydrophobic nano-silicon dioxide, 1-5% organic silicon anti-graffiti agent, 1-5% slip agent, and the remainder of surface resin; the surface resin includes polyurethane resin and / or acrylic resin, the elastic modulus of the surface resin is ≤10MPa, the elongation is ≥300%, and the surface resin is colorless, transparent or milky white; The thickness of the antifouling layer is 5-20 μm.
10. The method for preparing the thermal control sunshade cloth according to any one of claims 1 to 9, characterized in that: The following steps are involved: A light absorbing layer, a first optical coating layer, a second optical coating layer and an anti-fouling layer are sequentially stacked on the base fabric layer.
Citation Information
Patent Citations
Heat insulation coating capable of reflecting solar heat rays
CN101121858A
Coating sunshade composite material with high reflectivity and preparation method thereof
CN102582170A
Light-scattering, light-absorbing and thermal-radiation regulating cloth and preparation method
CN105332284A
High-light-absorptivity solar heat-absorbing paint
CN105713502A
Light absorption reflective paint and film adopting same
CN106046883A
Cited By
Light coating heat-shielding umbrella cloth and preparation method thereof
CN122257269A