Main-grid-free assembly prepared by graphical bearing film and preparation method thereof
By wrapping the low-temperature welding tape with a patterned bearing film and strengthening the series connection of the battery, the problem of cell string offset and reliability verification during the lamination process of the main gate photovoltaic cell is solved, and the light transmittance and reduced silver paste are achieved. The effect of dosage.
Patent Information
- Application Number
- CN202411321881.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-23
AI Technical Summary
During the lamination process, existing main gateless photovoltaic cells cannot effectively contact the cell, resulting in cell string offset and reliability verification problems. The cost of silver paste is high, so the amount of silver paste needs to be reduced and the search for alternatives is needed.
A patterned bearing film is used to wrap the low-temperature welding tape around the front and back of the battery string, and a "well" font cut is formed through laser cutting to ensure good contact between the battery cell and the adhesive film, avoid lamination and delamination, and pass infrared low-temperature heat Welding reinforcement bonding of welding tape and battery cell.
Effectively reinforce the connection between the welding tape and the battery cell, prevent the film from penetrating in the molten state, improve component reliability verification, reduce the amount of silver paste, improve light transmittance, and reduce the risk of filling reduction.
Smart Images

Figure CN119092574A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of solar photovoltaic technology, and in particular to a main grid-free component prepared by a patterned carrier film and a preparation method thereof. Background Art
[0002] As the efficiency of silicon-based solar cells has reached a certain bottleneck, finding ways to reduce costs has become a goal for major companies for a long time in the future. Usually, the main grid of photovoltaic cells usually uses silver paste, which is expensive. Therefore, it is very important to reduce the consumption of silver paste. Based on the perspective of reducing the absolute value of silver paste usage and seeking silver substitutes, more and more researchers are focusing on the research and development of main grid-free batteries. Main grid-free batteries eliminate the original main grid silver paste and use welding strips to collect fine grid currents and realize battery interconnection. In the prior art, dispensing or laminating methods are usually used. However, the laminating method usually covers the entire mask material on the battery cell and then fixes it through other processes. This treatment will make the battery cell and the adhesive film unable to contact well. During lamination, the battery string will have a large offset and there is a risk of parallel connection, and the subsequent reliability verification will also have a certain impact.
[0003] To this end, the applicant has carried out certain graphic processing on the mask material so that part of the battery cell is exposed and in full contact with the adhesive film, thereby eliminating the risk of battery strings being offset and connected in parallel during the lamination process and improving the reliability verification of the components. Summary of the invention
[0004] In view of the above problems, the present invention provides a main-grid-free component prepared by a graphic carrier film that strengthens the connection between the welding strip and the battery cell, avoids delamination in the full coating state, and improves the reliability verification of the component.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a main-grid-free component prepared by a patterned carrier film, the main-grid-free component structure is transparent glass, an upper adhesive film, an upper patterned carrier film, an OBB battery string, a lower patterned carrier film, a lower adhesive film, and a backplane from the light-receiving surface to the outer surface, the OBB battery string is composed of a plurality of array-arranged main-grid-free battery cells, adjacent battery cells of the OBB battery string are connected in parallel by several groups of low-temperature welding tapes, the two ends of the low-temperature welding tapes are respectively connected to the light-receiving surface of one battery cell and the backlight surface of the next battery cell, the low-temperature welding tapes located at the two ends of the OBB battery string are led outward, the upper patterned carrier film and the lower patterned carrier film are patterned by laser cutting or automatic cutting to cut off the block carrier film, and the cut pattern is in the shape of a "well", and the upper patterned carrier film and the lower patterned carrier film are pasted and fixed to the front and back sides of the OBB battery string.
[0006] Furthermore, both the upper patterned carrier film and the lower patterned carrier film are composed of a light absorption layer, an ultraviolet light conversion layer, and an adhesive layer formed by coextrusion of multiple layers.
[0007] Furthermore, the film thickness of the upper patterned carrier film and the lower patterned carrier film is set to 0.05 - 0.5 mm.
[0008] Furthermore, the overall length and width of the upper patterned carrier film and the lower patterned carrier film are both less than or equal to the length and width of a half-cell. The width of the horizontal lines is set to 1 - 6 mm, the number of horizontal lines is set according to the number of solder tapes on a single cell, the length is set to be less than or equal to the width of a half-cell, the number of vertical lines is between 2 - 6, the width is set to 5 - 30 mm, and the length is set to be less than or equal to the length of a half-cell.
[0009] Furthermore, for the OBB cell string, the sub-grid lines in the welding solder tape area are thickened and widened, or the main grid lines are thinned to be the same width as the fine grid lines, so that the low-temperature solder tape is welded to the cell, and the solder tape coating on the low-temperature solder tape forms an alloy with the sub-grid lines of the cell.
[0010] Furthermore, the diameter of the low-temperature solder tape is set between 0.15 mm and 0.35 mm.
[0011] A preparation method of a main-gridless component prepared with a patterned carrier film. The method is as follows: First, the patterned carrier film cuts the块状 carrier film into a pattern by laser cutting or an automatic cutter. The cut pattern is in a "well" shape. Then, the patterned carrier film wraps the low-temperature fine solder tape by infrared low-temperature thermal welding and pastes and fixes it on the front and back of the OBB cell string. On the film laminating platform, the patterned carrier film is attached to both the upper and lower sides of the OBB cell string. Then, the OBB cell string after film lamination and the pressing tooling are integrally transported to the infrared heating area. By controlling the heating temperature at about 120 °C, the patterned carrier film shrinks and melts due to heat and adheres to the OBB cell string. Finally, from the light-receiving surface to the outer surface, it is in turn a transparent glass, an upper adhesive film, an upper patterned carrier film, an OBB cell string, a lower patterned carrier film, a lower adhesive film, and a backsheet, and enters the laminator for lamination and forming.
[0012] Furthermore, the patterned carrier film is composed of a biological matrix resin, polyethylene, ethylene-vinyl acetate copolymer, and terpene resin.
[0013] Furthermore, the low-temperature solder tape coating is made of any one or a combination of tin-lead-bismuth, tin-lead-bismuth-silver, tin-bismuth-silver, and tin-lead materials, and the melting point is below 150 °C.
[0014] From the above description of the structure of the present invention, compared with the prior art, the present invention has the following advantages:
[0015] 1. The graphic carrier film is used to wrap the low-temperature thin welding ribbon through infrared low-temperature heat welding and stick it to the front and back of the battery string. It can effectively strengthen the connection between the welding ribbon and the battery cell, protect the welding ribbon and the battery cell secondary grid line alloying, so that the current of the series battery string can flow well, and it can also isolate the contact between the welding ribbon and the adhesive film, preventing the adhesive film from penetrating into the welding ribbon and the battery cell in a molten state, which directly leads to the phenomenon of filling decrease.
[0016] 2. The patterned carrier film has incisions at corresponding positions, so that most of the battery cells can be in good contact with the adhesive film, preventing the battery string from shifting due to the melting flow of the film during the lamination process, and avoiding the delamination phenomenon after lamination in the full-film state, thereby further improving the reliability verification of the components. At the same time, the transmittance of the incident light to the battery will decrease to a certain extent, and the transmittance will be higher than that of the full-film state. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0018] Figure 1 A cross-sectional view of a main-grid-free component prepared by a patterned carrier film according to the present invention;
[0019] Figure 2 This is a structural diagram of the upper graphic carrier film covering the OBB battery string of the present invention. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0021] Example
[0022] refer to Figure 1 , Figure 2, a main-grid-free component prepared by a patterned carrier film, wherein the main-grid-free component structure is transparent glass 4, upper adhesive film 3, upper patterned carrier film 2, OBB battery string 1, lower patterned carrier film 5, lower adhesive film 6, backplane 7 from the light-receiving surface to the outer surface, the OBB battery string 1 is composed of a plurality of battery cells arranged in an array without a main grid, and the adjacent battery cells of the OBB battery string are connected in parallel by a plurality of groups of low-temperature welding strips 8, the battery cell is 182 mm long and 91 mm wide, and the two ends of the low-temperature welding strip 8 are respectively connected to the light-receiving surface of one battery cell and the light-receiving surface of the next battery cell. The backlight surface of the battery cell is connected, and the low-temperature welding strips 8 located at both ends of the OBB battery string 1 are led outward. The upper patterned carrier film 2 and the lower patterned carrier film 5 are patterned by laser cutting or automatic cutting. The block carrier film is cut out, and the cutting pattern is in the shape of a "well". There are 20 lines, 88mm in length, 3mm in width, and 8.65mm in gap. The number of vertical lines is set to 2, with a length of 180mm, a width of 15mm, and a gap of 30.3mm. The upper patterned carrier film 2 and the lower patterned carrier film 5 are pasted and fixed on the front and back of the OBB battery string 1.
[0023] The upper patterned carrier film 2 and the lower patterned carrier film 5 are both composed of a light absorption layer, an ultraviolet light conversion layer and an adhesive layer formed by multi-layer co-extrusion. The film thickness of the upper patterned carrier film 2 and the lower patterned carrier film 5 is set to 0.2 mm.
[0024] The OBB battery string 1 uses thickened and widened secondary grid lines in the welding welding strip area, or thinned main grid lines to the same width as the fine grid lines, so that the low-temperature welding strip is welded to the battery cell, and the welding strip coating on the low-temperature welding strip 8 forms an alloy with the secondary grid lines of the battery cell. The diameter of the low-temperature welding strip 8 is set at 0.25mm.
[0025] The method for preparing a main-grid-free component prepared by the patterned carrier film is as follows: first, the patterned carrier film is patterned and cut out of a block carrier film by laser cutting or an automatic cutter, and the cut pattern is in the shape of a "well", and then the patterned carrier film is wrapped with a low-temperature fine welding tape by infrared low-temperature heat welding and pasted and fixed on the front and back sides of the OBB battery string, and the patterned carrier film is pasted on the upper and lower sides of the OBB battery string on the laminating platform, and then the laminated OBB battery string and the pressing tool are transported to the infrared heating zone as a whole, and the heating temperature is controlled at about 120°C so that the patterned carrier film shrinks and melts due to the heat and is pasted together with the OBB battery string, and finally, from the light-receiving surface to the outer surface, transparent glass, upper adhesive film, upper patterned carrier film, OBB battery string, lower patterned carrier film, lower adhesive film, and backplane enter the laminator for lamination.
[0026] The patterned carrier film is composed of bio-matrix resin, polyethylene, ethylene-vinyl acetate copolymer and terpene resin.
[0027] The low-temperature solder strip coating is made of any one or more combinations of tin-lead-bismuth, tin-lead-bismuth-silver, tin-bismuth-silver, and tin-lead materials, and has a melting point below 150° C.
[0028] The present invention uses a graphic carrier film to wrap the low-temperature thin solder strip through infrared low-temperature heat welding and stick it to the front and back of the battery string, which can effectively strengthen the connection between the solder strip and the battery cell, protect the solder strip and the battery cell secondary grid line from alloying, so that the current of the series battery string can flow well, and can also isolate the contact between the solder strip and the adhesive film, preventing the adhesive film from penetrating into the solder strip and the battery cell in a molten state, which directly causes the filling to decrease. The graphic carrier film has incisions at corresponding positions, so that most of the battery cells can be in good contact with the adhesive film, preventing the battery string from being displaced due to the molten flow of the adhesive film during the lamination process, avoiding the phenomenon of delamination after lamination in a fully covered state, thereby further improving the reliability verification of the component, and at the same time, the transmittance of the incident light to the battery will decrease to a certain extent, and the transmittance will be higher than that of the full film.
[0029] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A busbar-free component prepared by a patterned carrier film, characterized in that: The structure of the main-gridless component is, from the light-receiving surface to the outer surface, a transparent glass, an upper adhesive film, an upper patterned carrier film, an OBB cell string, a lower patterned carrier film, a lower adhesive film, and a backplane. The OBB cell string is composed of multiple cell pieces in a main-gridless form arranged in an array. Adjacent cell pieces of the OBB cell string are connected in parallel by several groups of low-temperature solder tapes. The two ends of the low-temperature solder tape are respectively connected to the light-receiving surface of one cell piece and the backlight surface of the next cell piece. The low-temperature solder tapes at both ends of the OBB cell string are led outwards. The upper patterned carrier film and the lower patterned carrier film are used to pattern and cut the block-shaped carrier film by means of laser cutting or an automatic cutter. The cut pattern is in the shape of a "well". The upper patterned carrier film and the lower patterned carrier film are pasted and fixed on the front and back of the OBB cell string.
2. A busbar-free component prepared by a patterned carrier film according to claim 1, characterized in that: Both the upper patterned carrier film and the lower patterned carrier film are composed of a light absorption layer, an ultraviolet light conversion layer, and an adhesive layer formed by multi-layer co-extrusion.
3. A busbar-free component prepared by a patterned carrier film according to claim 1, characterized in that: The film thickness of both the upper patterned carrier film and the lower patterned carrier film is set to 0.05 - 0.5 mm.
4. A busbar-free component prepared by a patterned carrier film according to claim 1, characterized in that: The overall length and width of both the upper patterned carrier film and the lower patterned carrier film are less than or equal to the length and width of a half cell piece. The width of the horizontal lines is set to 1 - 6 mm, the number of horizontal lines is set according to the number of solder tapes on a single cell, the length is set to be less than or equal to the width of a half cell piece, the number of its vertical lines is between 2 - 6, the width is set to 5 - 30 mm, and the length is set to be less than or equal to the length of a half cell piece.
5. A busbar-free component prepared by a patterned carrier film according to claim 1, characterized in that: For the OBB cell string, the sub-grid lines in the welded solder tape area are thickened and widened, or the main grid lines are thinned to be the same as the width of the fine grid lines, so that the low-temperature solder tape is welded to the cell piece, and the solder tape coating on the low-temperature solder tape forms an alloy with the sub-grid lines of the cell piece.
6. A busbar-free component prepared by a patterned carrier film according to claim 1, characterized in that: The diameter of the low-temperature solder tape is set at 0.15 mm - 0.35 mm.
7. A method for preparing the busbar-free assembly according to claim 1, characterized in that: The method is as follows: First, the patterned carrier film is used to pattern and cut the block-shaped carrier film by means of laser cutting or an automatic cutter. The cut pattern is in the shape of a "well". Then, the patterned carrier film wraps the low-temperature fine solder tape through infrared low-temperature thermal welding and is pasted and fixed on the front and back of the OBB cell string. On the film laminating platform, patterned carrier films are attached to both the upper and lower parts of the OBB cell string. Then, the OBB cell string after film lamination and the pressing tooling are integrally conveyed to the infrared heating area. By controlling the heating temperature at about 120 °C, the patterned carrier film is heated, shrunk, melted, and adhered to the OBB cell string. Finally, from the light-receiving surface to the outer surface, it is a transparent glass, an upper adhesive film, an upper patterned carrier film, an OBB cell string, a lower patterned carrier film, a lower adhesive film, and a backplane that enter the laminator for lamination and forming.
8. The method for preparing a busbar-free assembly according to claim 7, characterized in that: The patterned carrier film is composed of a biological matrix resin, polyethylene, ethylene-vinyl acetate copolymer, and terpene resin.
9. The method for preparing a busbar-free assembly according to claim 7, characterized in that: The coating of the low-temperature solder tape is made of any one or a combination of tin-lead-bismuth, tin-lead-bismuth-silver, tin-bismuth-silver, and tin-lead materials, and the melting point is below 150 °C.
Citation Information
Patent Citations
Photovoltaic module without main grid, preparation method thereof and welding strip welding method
CN114864721A
Photovoltaic module and preparation method thereof
CN116936665A
Main-grid-free assembly and preparation method thereof
CN117637890A
Battery string and battery assembly
CN117727819A
Composite film and gridless solar cell modules
CN218827159U
Cited By
Series welding method of photovoltaic cells and cell assembly
CN122340946A