Visible light superhard composite coating material, preparation method and device and anti-reflection film
By controlling the content of titanium and silicon elements in vacuum coating technology, the TiSiON coating material is formed, and the problem of insufficient hardness of traditional anti-reflective films is solved, and the anti-reflective film with high hardness and low refractive index is achieved, which improves scratch resistance.
Patent Information
- Application Number
- CN202411089386.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The scratch-resistant and wear-resistant properties of traditional anti-reflective films cannot meet the requirements of modern display systems. It is necessary to develop anti-reflective films with high hardness and good wear resistance to improve the scratch resistance of the film layer.
Using vacuum coating technology, titanium material and silicon material are co-evaporated by reactive gas to control the content proportion of titanium and silicon elements to improve the hardness and refractive index of the coating material, and form TiSiON coating material for the preparation of high hardness and low hardness. Refractive index film.
By controlling the content of titanium and silicon elements, the hardness and refractive index of the coating material are improved, and TiSiON coating material with a hardness of more than 1500HV and a refractive index between 1.49 and 2.09 is prepared to meet the high hardness and wear resistance requirements of the display system. , improves the scratch resistance of the film layer.
Smart Images

Figure CN118979221A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical fields of optical coating materials, anti-reflection films and vacuum coatings, and in particular to a visible light super-hard composite coating material and a preparation method, device and anti-reflection film. Background Art
[0002] With the rapid development of display technology, more and more digital products with display screens have been integrated into people's lives. For example, smart phones, tablets and other products are playing an increasingly important role in our study and work. In order to improve the utilization rate of energy, it is necessary to deposit an anti-reflection film on the surface of the display screen. With the update and iteration of the display system, the anti-scratch and wear-resistant performance of the traditional anti-reflection film is far from meeting the use requirements of the display system. It is urgent to develop an anti-reflection film with high hardness and good wear resistance to meet the use requirements of the display system.
[0003] Based on this, a new technical solution is needed to improve the scratch resistance of the film layer. Summary of the invention
[0004] In view of this, the embodiments of this specification provide a visible light super-hard composite coating material and a preparation method, device, and anti-reflection film.
[0005] The embodiments of this specification provide the following technical solutions:
[0006] The embodiment of the present specification provides a method for preparing a visible light superhard composite coating material, comprising: using a titanium material, a silicon material and a reaction gas as raw materials, and co-evaporating the titanium material and the silicon material in a vacuum coating machine; wherein the titanium material and the silicon material are co-evaporated and deposited on a coating substrate by the reaction gas, so as to obtain a coating material containing a titanium element Ti, a silicon element Si and a reaction element; the titanium material and the silicon material are separated by a partition and placed inside the vacuum coating machine, so that under the separation of the partition, the titanium material and the silicon material are co-evaporated and deposited on the coating substrate respectively;
[0007] In the co-evaporation deposition process, according to the first condition that the hardness of the coating material needs to meet, the first rate of the titanium material in the co-evaporation deposition is controlled so that the content ratio of the titanium element Ti in the coating material meets the requirements corresponding to the first condition, and according to the second condition that the refractive index of the coating material needs to meet, the second rate of the silicon material in the co-evaporation deposition is controlled so that the content ratio of the silicon element Si in the coating material meets the requirements corresponding to the second condition.
[0008] The embodiments of the present specification also provide a visible light superhard composite coating material, which is a coating material prepared by the above-mentioned visible light superhard composite coating material preparation method.
[0009] The embodiment of this specification also provides a visible light superhard composite coating material preparation device, comprising:
[0010] A partition is erected at the bottom of the vacuum coating machine;
[0011] Dual electron guns are respectively located on both sides of the partition, each electron gun correspondingly serving as an evaporation source for evaporating titanium material or an evaporation source for evaporating silicon material;
[0012] The controller is connected to the electron gun and is used to control a first rate of the titanium material in the co-evaporation deposition according to a first condition that the hardness of the coating material needs to meet, so that the content of the titanium element Ti in the coating material meets the requirement corresponding to the first condition; and control a second rate of the silicon material in the co-evaporation deposition according to a second condition that the refractive index of the coating material needs to meet, so that the content of the silicon element Si in the coating material meets the requirement corresponding to the second condition.
[0013] The embodiments of the present specification also provide an anti-reflection film, including a substrate and a film layer, wherein the film layer is attached to the substrate, wherein the film layer is a coating structure formed on the substrate by the above-mentioned visible light superhard composite coating material.
[0014] Compared with the prior art, the beneficial effects that can be achieved by at least one of the above technical solutions adopted in the embodiments of this specification include at least:
[0015] In the present application, titanium material and silicon material are co-evaporated and deposited onto a coating substrate respectively by reaction gases, and the titanium material and silicon material are evaporated and deposited onto the coating substrate respectively under the separation of a partition, so as to control a first rate of the titanium material in the co-evaporation deposition, and control a second rate of the silicon material in the co-evaporation deposition so that the content ratio of the titanium element Ti in the coating material satisfies a first condition of hardness requirement, and so that the content ratio of the silicon element Si in the coating material satisfies a second condition of refractive index requirement, that is, the hardness of the coating material is increased by controlling the content ratio of the titanium element Ti in the coating material to increase, and the refractive index of the coating material is decreased by controlling the content ratio of the silicon element Si in the coating material to increase; wherein the coating substrate can be an anti-reflection film substrate, and the coating material can be used to prepare an anti-reflection film on the anti-reflection film substrate, so as to obtain an anti-reflection film that meets multiple requirements such as refractive index, hardness, wear resistance and scratch resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 It is a schematic diagram of the co-evaporation structure of the present application;
[0018] Figure 2 is a refractive index dispersion distribution curve diagram of the TiSiON film layer obtained in the embodiment of the present application;
[0019] Figure 3 This is a graph showing the extinction coefficient distribution of the TiSiON film obtained in the embodiment of the present application.
[0020] Figure numerals: 1. first monitoring probe; 2. second monitoring probe; 3. third monitoring probe; 4. coating substrate; 5. partition; 6. first inflation port; 7. second inflation port; 8. evaporation source of titanium material; 9. evaporation source of silicon material. DETAILED DESCRIPTION
[0021] The embodiments of the present application are described in detail below with reference to the accompanying drawings.
[0022] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.
[0023] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.
[0024] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0025] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the examples can be practiced without these specific details.
[0026] The applicant has conducted in-depth research and improvement on anti-reflection films and coating materials and found that: Currently, for the visible light range, high refractive index superhard materials usually use silicon nitride Si 3 N 4 , whose hardness can reach more than 2000HV; low refractive index materials usually include silicon dioxide SiO 2 and magnesium fluoride MgF 2 However, the hardness of these two materials is low, about 900HV, which leads to the overall low hardness of the prepared anti-reflection film, which cannot meet the high hardness requirements of the display system. Therefore, the development of ultra-hard low-refractive index materials is the key to improving the hardness of the anti-reflection film.
[0027] Based on this, the technical solutions provided by the embodiments of the present application are described below in conjunction with the accompanying drawings.
[0028] The present specification provides a method for preparing a visible light superhard composite coating material. Figure 1 As shown, it includes: using titanium material, silicon material and reaction gas as raw materials, co-evaporating the titanium material and silicon material in a vacuum coating machine; wherein the titanium material and silicon material are co-evaporated and deposited on the coating substrate 4 by the reaction gas, so as to obtain a coating material containing titanium element Ti, silicon element Si and reaction elements; the titanium material and silicon material are separated by a partition 5 and placed inside the vacuum coating machine, so that under the separation of the partition 5, the titanium material and the silicon material are evaporated and deposited on the coating substrate 4 respectively. The partition 5 serves as an isolation baffle.
[0029] In the co-evaporation deposition process, according to the first condition that the hardness of the coating material needs to meet, the first rate of the titanium material in the co-evaporation deposition is controlled so that the content ratio of the titanium element Ti in the coating material meets the requirements corresponding to the first condition; and according to the second condition that the refractive index of the coating material needs to meet, the second rate of the silicon material in the co-evaporation deposition is controlled so that the content ratio of the silicon element Si in the coating material meets the requirements corresponding to the second condition. Among them, the coating material can be a visible superhard new nano-composite low-refractive index coating material. The coating substrate can be an anti-reflection film substrate, and the coating material can be used to prepare an anti-reflection film, that is, the anti-reflection film contains the coating material.
[0030] In one embodiment, a first monitoring probe is used to monitor a first rate of the titanium material in co-evaporation deposition, and a second monitoring probe is used to monitor a second rate of the silicon material in co-evaporation deposition; wherein the first monitoring probe and the titanium material are arranged on one side of the partition 5, and the second monitoring probe and the silicon material are arranged on the other side of the partition 5, and the connection line between the first monitoring probe and the evaporation source 9 of the silicon material passes through the partition 5, and similarly, the connection line between the second monitoring probe and the evaporation source 8 of the titanium material passes through the partition 5, so that during the co-evaporation deposition, the first monitoring probe does not collect the deposition parameters corresponding to the silicon material, and the second monitoring probe does not collect the deposition parameters corresponding to the titanium material.
[0031] In one embodiment, the first rate monitored by the first monitoring probe is 0.2 nm / s to 0.4 nm / s; and / or the second rate monitored by the second monitoring probe 2 is 0.8 nm / s to 1.4 nm / s.
[0032] In one embodiment, the method for preparing the coating material further includes: monitoring the deposition rate and / or deposition thickness of the coating material film layer by a third monitoring probe.
[0033] In one embodiment, the deposition rate monitored by the third monitoring probe is 0.9-1.5 nm / s; and / or the deposition thickness monitored by the third monitoring probe is 500-700 nm, wherein when the monitored deposition thickness exceeds 700 nm, the co-evaporation process is stopped.
[0034] In one embodiment, the first reaction gas is oxygen and the second reaction gas is nitrogen, so that the titanium material forms Ti(ON) containing titanium element Ti, oxygen element O and nitrogen element N during evaporation deposition, and the silicon material forms Si(ON) containing silicon element Si, oxygen element O and nitrogen element N during evaporation deposition; wherein oxygen is filled into the first side space where the titanium material is located, and nitrogen is filled into the second side space where the silicon material is located, and the first side space and the second side space are the corresponding spaces on both sides of the partition 5 respectively. 2 and oxygen O 2The purity of the four basic materials must be above 99.999%; the formed coating material is TiSiON coating material, and the content ratio of oxygen element O and the content ratio of nitrogen element N in the coating material are controlled by controlling the amount of oxygen and nitrogen charged.
[0035] In one embodiment, the nitrogen filling amount is 35 sccm to 45 sccm, and the oxygen filling amount is 45 sccm to 60 sccm.
[0036] In one embodiment, the co-evaporation deposition process adopts any one of the following methods: electron beam thermal evaporation, magnetron sputtering, ion beam sputtering. That is, the preparation method of the present application is: electron beam thermal evaporation, magnetron sputtering, ion beam sputtering, etc.
[0037] In one embodiment, a radio frequency ion-assisted deposition process may be used in electron beam thermal evaporation. The ion source parameters of the radio frequency ion-assisted deposition process include a voltage of 850 V to 950 V and a current of 800 mA to 1000 mA.
[0038] In one embodiment, before the co-evaporation process, the electron guns corresponding to the titanium material and the silicon material are fully pre-melted, and the deposition process is started after the error between the power of the electron gun and the power during deposition falls within a preset range; the preset range can be a range that satisfies the following conditions: before the formal film formation, the electron gun is fully pre-melted, and the power of the electron gun is ensured to be close to the power during deposition, so that when the deposition is officially started, the detection rates of the first monitoring probe 1, the second monitoring probe 2 and the third monitoring probe 3 quickly reach the set value and remain relatively stable, thereby achieving stability of the deposition process.
[0039] And / or, before the co-evaporation treatment, the substrate of the coating material is cleaned and wiped with an alcohol-ether mixture.
[0040] And / or, before the co-evaporation treatment, the vacuum chamber is evacuated, and when the vacuum degree reaches a first vacuum degree, the substrate of the coating material is pre-treated by ion cleaning, and the ion source parameters used for ion cleaning are 1200V voltage, 950mA current, and cleaning for 5-10 minutes. The first vacuum degree can be 5.0×10 -4 Pa.
[0041] And / or, before the co-evaporation process, the vacuum chamber is evacuated and heated, and the deposition process is started when the baking temperature reaches the set temperature and the vacuum degree is stabilized at the second vacuum degree. The set temperature can be 100°C, and the second vacuum degree can be 3.0×10 -4 Pa.
[0042] This application adopts vacuum co-deposition technology to 2 and O 2 As the reaction gas, titanium material and silicon material are deposited simultaneously, and N2 and O 2 By adjusting the flow rate, the deposition rate of titanium and silicon materials, and the deposition temperature, vacuum degree, ion-assisted and other process parameters, a new type of ultra-hard composite low-refractive index coating material TiSiON is obtained. Preparation of TiSiON nanocomposite materials: Open the electron guns corresponding to titanium and silicon materials at the same time, evaporate and deposit titanium particles and silicon particles, N 2 Filling amount 35sccm~45sccm, O 2 The filling amount is 45sccm~60sccm. By adjusting the electron gun power of titanium material and silicon material, the monitoring rate of the first monitoring probe 1 is 0.2nm / s~0.4nm / s, the monitoring rate of the second monitoring probe 2 is 0.8nm / s~1.4nm / s, and the monitoring rate of the third monitoring probe 3 is about 0.9nm / s~1.5nm / s. When the deposition thickness monitored by the third monitoring probe 3 is 500~700nm, the electron gun, gas filling and other systems are turned off to stop film deposition. The radio frequency ion assisted deposition process is used in the entire deposition process, and the ion source parameters are voltage 850V~950V and current 800mA~1000mA. Refractive index and hardness of TiSiON nanocomposite materials on N 2 and O 2 The flow rate is not sensitive, but the hardness increases with the increase of Ti relative content, and varies between 1500HV and 1600HV. The refractive index decreases with the increase of Si relative content, and varies between 2.09 and 1.49. 2 The relative content has a great influence on the extinction coefficient in the 350nm-450nm band. 2 As the relative content increases, the extinction coefficient gradually decreases. At 400nm, the extinction coefficient is 12x10 -4 ~0.2x10 -4 Because the four elements undergo chemical reactions, the reaction energy and degree of different elements are different, all of which are obtained through actual experiments. This application uses three probes for separate monitoring to ensure the rationality of monitoring, and sets an isolation baffle to achieve relatively independent monitoring of Ti (ON) and Si (ON), realizing co-evaporation and film thickness monitoring.
[0043] The embodiments of the present specification also disclose a visible light superhard composite coating material, which is a coating material prepared by any coating material preparation method of the embodiments of the present specification.
[0044] In one embodiment, the wavelength range of the coating material is 350nm-800nm; wherein the hardness of the coating material is 1500HV-1600HV, and / or the refractive index of the coating material is 2.09-1.49. The hardness here can be used as the first condition mentioned in the text, and the refractive index here can be used as the second condition mentioned in the text.
[0045] In one embodiment, the coating material is a TiSiON thin film material, wherein the silicon element Si content accounts for 28% to 30%, the titanium element Ti content accounts for 5% to 7%, the nitrogen element N content accounts for 7%-9%, and the oxygen element O content accounts for 56% to 58%. The titanium element Ti content ratio here can be used as the corresponding requirement to meet the first condition, and the silicon element Si content ratio here can be used as the corresponding requirement to meet the second condition.
[0046] In one embodiment, in the wavelength range of 350 nm to 450 nm, the extinction coefficient of the coating material decreases as the relative content of oxygen increases, wherein the extinction coefficient at 400 nm falls within 12×10 -4 ~0.2×10 -4 .
[0047] The present application adopts vacuum coating technology to prepare TiSiON ultra-hard low-refractive index coating material. Through process adjustment, the composite nano-TiSiON low-refractive index material can vary between 1.49 and 2.09 at a wavelength of 550nm, and the hardness can reach more than 1700HV. The nitrogen content of TiSiON material is 7%-9%, the oxygen content is 56%-58%, the silicon content is 28%-30%, and the titanium content is 5%-7%. The refractive index at a wavelength of 550nm can vary between 1.49 and 2.09, and the hardness can reach more than 1500HV. The wavelength range is 350nm to 800nm, and the refractive index wavelength of 550nm can vary between 1.49 and 2.09, and the hardness range is 1500 to 1600HV.
[0048] The present specification also discloses a device for preparing a visible light superhard composite coating material, comprising:
[0049] The partition 5 is erected at the bottom of the vacuum coating machine.
[0050] The dual electron guns are respectively located on both sides of the partition 5, and each electron gun corresponds to an evaporation source 8 for evaporating titanium material or an evaporation source 9 for evaporating silicon material.
[0051] The controller is connected to the electron gun and is used to control a first rate of the titanium material in the co-evaporation deposition according to a first condition that the hardness of the coating material needs to meet, so that the content of the titanium element Ti in the coating material meets the requirement corresponding to the first condition; and control a second rate of the silicon material in the co-evaporation deposition according to a second condition that the refractive index of the coating material needs to meet, so that the content of the silicon element Si in the coating material meets the requirement corresponding to the second condition.
[0052] In one embodiment, the coating material preparation device also includes: a first monitoring probe and a second monitoring probe connected to the controller; the first monitoring probe is used to monitor a first rate of the titanium material in the co-evaporation deposition; the second monitoring probe is used to monitor a second rate of the silicon material in the co-evaporation deposition.
[0053] The first monitoring probe and the titanium material are arranged on one side of the partition 5, the second monitoring probe and the silicon material are arranged on the other side of the partition 5, and the connection line between the first monitoring probe and the evaporation source 9 of the silicon material passes through the partition 5, and the connection line between the second monitoring probe and the evaporation source 8 of the titanium material passes through the partition 5, so that during the co-evaporation deposition, the first monitoring probe does not collect the deposition parameters corresponding to the silicon material, and the second monitoring probe does not collect the deposition parameters corresponding to the titanium material. The first monitoring probe and the titanium material are arranged on the same side of the partition 5, and the second monitoring probe and the silicon material are arranged on the same side of the partition 5.
[0054] In one embodiment, the first rate monitored by the first monitoring probe is 0.2 nm / s to 0.4 nm / s; and / or the second rate monitored by the second monitoring probe 2 is 0.8 nm / s to 1.4 nm / s.
[0055] In one embodiment, the coating material preparation device further includes: a third monitoring probe connected to the controller, which is used to monitor the deposition rate and / or deposition thickness of the coating material film layer.
[0056] In one embodiment, the deposition rate monitored by the third monitoring probe is 0.9-1.5 nm / s; and / or the deposition thickness monitored by the third monitoring probe is 500-700 nm, wherein when the monitored deposition thickness exceeds 700 nm, the co-evaporation process is stopped.
[0057] In one embodiment, the vacuum coating machine includes a 1300 type vacuum coating machine.
[0058] The present application also provides a method for preparing a new type of ultra-hard nano-composite low-refractive index coating material. Figure 1 , Figure 2 as well as Figure 3 For detailed explanation, a 1300 type vacuum coating machine is used, which is equipped with dual electron guns, radio frequency ion assisted evaporation system, three sets of multi-probe quartz crystal monitoring system and low temperature pump + dry pump oil-free exhaust system.
[0059] Using dual electron gun co-evaporation technology, a new type of TiSiON nanocomposite material was prepared on a K9 substrate with a diameter of 30 mm and a thickness of 2 mm. The evaporation schematic diagram is shown in the figure. Figure 1 shown.
[0060] The two sets of electron gun evaporation sources evaporate titanium material and silicon material respectively, and the first gas filling port 6 is filled with N 2, the second filling port 7 is filled with O 2 The third monitoring probe 3 monitors the deposition rate and thickness of the TiSiON material, the first monitoring probe 1 monitors the deposition rate and thickness of Ti(ON), and the second monitoring probe 2 monitors the deposition rate and thickness of Si(ON). The isolation baffle is used to prevent the deposition rate of Ti(ON) from affecting the second monitoring probe 2 and the deposition rate of Si(ON) from affecting the first monitoring probe 1. The third monitoring probe 3 monitors the deposition rate and thickness of the TiSiON film layer. The height of the isolation baffle requires that the line connecting the first monitoring probe 1 and the evaporation source 9 of the silicon material pass through the isolation baffle, and similarly, the line connecting the second monitoring probe 2 and the evaporation source 8 of the titanium material pass through the isolation baffle, that is, the height of the isolation baffle satisfies that the second monitoring probe 2 cannot collect deposition parameters when Ti(ON) evaporates, and the first monitoring probe 1 cannot collect deposition parameters when Si(ON) evaporates.
[0061] The specific preparation process is as follows:
[0062] 1. Use an alcohol-ether mixture to clean and wipe the K9 substrate, which is a sample and is also called a coating substrate 4.
[0063] 2. Place the wiped sample on the sample rack of the coating machine and evacuate the vacuum chamber. When the vacuum degree reaches 5.0×10 -4 When Pa, turn on the radio frequency ion source to perform ion cleaning pretreatment on the sample. The radio frequency ion source parameter voltage is 1200V, current is 950mA, and cleaning takes 5-10 minutes.
[0064] 3. After cleaning, wait for the baking temperature to reach the set 100°C and the vacuum degree to stabilize at 3.0×10 -4 Pa, the preparation of TiSiON nanocomposite materials was started, and the electron guns corresponding to the titanium material and the silicon material were turned on at the same time to evaporate and deposit titanium particles and silicon particles. 2 Filling amount 40sccm, O 2 The filling amount is 50sccm. By adjusting the electron gun power corresponding to the titanium material and the silicon material, the monitoring rate of the first monitoring probe 1 is 0.2nm / s, the monitoring rate of the second monitoring probe 2 is 0.9nm / s, and the monitoring rate of the third monitoring probe 3 is about 1.0nm / s. When the deposition thickness monitored by the third monitoring probe 3 is 500nm, the electron gun, the gas filling system and other systems are turned off to stop the film deposition. The radio frequency ion assisted deposition process is used in the entire deposition process, and the ion source parameters are voltage 900V and current 900mA. All parameters in this process can be adjusted, but the refractive index, extinction coefficient and hardness of the obtained sample are changed accordingly according to the adjustment.
[0065] 4. When the temperature of the vacuum chamber drops to 60°C, take out the sample for testing.
[0066] 5. The refractive index dispersion distribution of TiSiON in the visible light range is measured as follows Figure 2 As shown, the extinction coefficient distribution is as follows Figure 3 The hardness of the sample film layer is measured to be 1532HV, which can be used as a visible super-hard low-coating coating material. Figure 2 and Figure 3 The Wavelength in it represents the wavelength.
[0067] The embodiments of this specification also provide an anti-reflection film, including a substrate and a film layer, wherein the film layer is attached to the substrate, wherein the film layer is a coating structure formed on the substrate by a visible light superhard composite coating material as in any of the above embodiments. The substrate is an anti-reflection film substrate in a coating substrate. The film layer is a visible light anti-reflection film layer.
[0068] The new ultra-hard nano-composite low-refractive index material of the present application provides a visible low-refractive index coating material for film system design, which can solve the problem that the current low-refractive index coating materials in the visible light range have low hardness and cannot meet the requirements of the display system for anti-scratch properties. It can increase the hardness of the film layer and the anti-scratch performance of the product, and can be used as a visible transparent protective film.
[0069] In this specification, the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the embodiments described later, the description is relatively simple, and the relevant parts can be referred to the partial description of the previous embodiments.
[0070] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for preparing a visible light superhard composite coating material, characterized in that: include: Using titanium material, silicon material and reaction gas as raw materials, the titanium material and the silicon material are co-evaporated in a vacuum coating machine; wherein the titanium material and the silicon material are co-evaporated and deposited on a coating substrate by the reaction gas, so as to obtain a coating material containing titanium element Ti, silicon element Si and reaction elements; the titanium material and the silicon material are separated by a partition and placed inside the vacuum coating machine, so that under the separation of the partition, the titanium material and the silicon material are co-evaporated and deposited on the coating substrate respectively; In the co-evaporation deposition process, according to the first condition that the hardness of the coating material needs to meet, the first rate of the titanium material in the co-evaporation deposition is controlled so that the content ratio of the titanium element Ti in the coating material meets the requirements corresponding to the first condition, and according to the second condition that the refractive index of the coating material needs to meet, the second rate of the silicon material in the co-evaporation deposition is controlled so that the content ratio of the silicon element Si in the coating material meets the requirements corresponding to the second condition.
2. The method for preparing a visible light superhard composite coating material according to claim 1, characterized in that: The first rate of the titanium material in co-evaporation deposition is monitored by a first monitoring probe, and the second rate of the silicon material in co-evaporation deposition is monitored by a second monitoring probe; wherein the first monitoring probe and the titanium material are arranged on one side of the partition, the second monitoring probe and the silicon material are arranged on the other side of the partition, and the connection line between the first monitoring probe and the evaporation source of the silicon material passes through the partition, and similarly, the connection line between the second monitoring probe and the evaporation source of the titanium material passes through the partition, so that in co-evaporation deposition, the first monitoring probe does not collect deposition parameters corresponding to the silicon material, and the second monitoring probe does not collect deposition parameters corresponding to the titanium material.
3. The method for preparing a visible light superhard composite coating material according to claim 2, characterized in that: The first rate monitored by the first monitoring probe is 0.2 nm / s to 0.4 nm / s; and / or the second rate monitored by the second monitoring probe is 0.8 nm / s to 1.4 nm / s.
4. The method for preparing a visible light superhard composite coating material according to claim 1, characterized in that: The method for preparing the coating material further includes: monitoring the deposition rate and / or deposition thickness of the coating material by means of a third monitoring probe.
5. The method for preparing a visible light superhard composite coating material according to claim 4, characterized in that: The deposition rate monitored by the third monitoring probe is 0.9-1.5 nm / s; and / or the deposition thickness monitored by the third monitoring probe is 500-700 nm, wherein when the monitored deposition thickness exceeds 700 nm, the co-evaporation process is stopped.
6. The method for preparing a visible light superhard composite coating material according to claim 1, characterized in that: The reaction gas includes a first reaction gas and a second reaction gas; the first reaction gas is oxygen, and the second reaction gas is nitrogen, so that the titanium material forms Ti(ON) containing titanium element Ti, oxygen element O and nitrogen element N during evaporation deposition, and the silicon material forms Si(ON) containing silicon element Si, oxygen element O and nitrogen element N during evaporation deposition; wherein the oxygen is filled into the first side space where the titanium material is located, and the nitrogen is filled into the second side space where the silicon material is located, and the first side space and the second side space are the corresponding spaces on both sides of the partition respectively.
7. The method for preparing a visible light superhard composite coating material according to claim 6, characterized in that: The nitrogen filling amount is 35 sccm to 45 sccm, and the oxygen filling amount is 45 sccm to 60 sccm.
8. The method for preparing a visible light superhard composite coating material according to claim 1, characterized in that: The co-evaporation deposition process is carried out by any of the following methods: electron beam thermal evaporation, magnetron sputtering, and ion beam sputtering.
9. The method for preparing a visible light superhard composite coating material according to claim 8, characterized in that: The radio frequency ion-assisted deposition process is adopted in the electron beam thermal evaporation. The ion source parameters of the radio frequency ion-assisted deposition process include a voltage of 850V to 950V and a current of 800mA to 1000mA.
10. The method for preparing a visible light superhard composite coating material according to claim 1, characterized in that: Before the co-evaporation process, the electron guns corresponding to the titanium material and the silicon material are fully pre-melted, and the deposition process is started when the error between the power of the electron gun and the power during deposition falls within a preset range; and / or, before the co-evaporation treatment, the coated substrate is cleaned and wiped with an alcohol-ether mixture; And / or, before the co-evaporation treatment, the vacuum chamber is evacuated, and when the vacuum degree reaches a first vacuum degree, the coated substrate is pre-treated by ion cleaning, wherein the ion source parameters used for the ion cleaning are a voltage of 1200 V, a current of 950 mA, and the cleaning time is 5-10 minutes; And / or, before the co-evaporation process, the vacuum chamber is evacuated and heated, and the deposition process is started when the baking temperature reaches the set temperature and the vacuum degree is stabilized at the second vacuum degree.
11. A visible light superhard composite coating material, characterized in that: The coating material is prepared by the method for preparing a visible light superhard composite coating material as described in any one of claims 1 to 10.
12. The visible light superhard composite coating material according to claim 11, characterized in that: The wavelength range of the coating material is 350nm-800nm; wherein the hardness of the coating material is 1500HV-1600HV, and / or the refractive index of the coating material is 2.09-1.
49.
13. The visible light superhard composite coating material according to claim 11, characterized in that: The coating material is TiSiON thin film material, in which the silicon element Si content accounts for 28% to 30%, the titanium element Ti content accounts for 5% to 7%, the nitrogen element N content accounts for 7%-9%, and the oxygen element O content accounts for 56% to 58%.
14. The visible light superhard composite coating material according to claim 13, characterized in that: In the 350nm to 450nm band, the extinction coefficient of the coating material decreases with the increase of the relative content of oxygen. At 400nm, the extinction coefficient falls within 12×10 -4 ~0.2×10 -4 .
15. A device for preparing a visible light superhard composite coating material, characterized in that: include: A partition is erected at the bottom of the vacuum coating machine; Dual electron guns are respectively located on both sides of the partition, each electron gun correspondingly serving as an evaporation source for evaporating titanium material or an evaporation source for evaporating silicon material; The controller is connected to the electron gun and is used to control a first rate of the titanium material in the co-evaporation deposition according to a first condition that the hardness of the coating material needs to meet, so that the content of the titanium element Ti in the coating material meets the requirement corresponding to the first condition; and control a second rate of the silicon material in the co-evaporation deposition according to a second condition that the refractive index of the coating material needs to meet, so that the content of the silicon element Si in the coating material meets the requirement corresponding to the second condition.
16. The device for preparing a visible light superhard composite coating material according to claim 15, characterized in that: The coating material preparation device also includes: a first monitoring probe and a second monitoring probe connected to the controller; the first monitoring probe is used to monitor a first rate of the titanium material in the co-evaporation deposition; the second monitoring probe is used to monitor a second rate of the silicon material in the co-evaporation deposition; The first monitoring probe and the titanium material are arranged on one side of the partition, and the second monitoring probe and the silicon material are arranged on the other side of the partition, and the connection line between the first monitoring probe and the evaporation source of the silicon material passes through the partition, and similarly, the connection line between the second monitoring probe and the evaporation source of the titanium material passes through the partition, so that during co-evaporation deposition, the first monitoring probe does not collect deposition parameters corresponding to the silicon material, and the second monitoring probe does not collect deposition parameters corresponding to the titanium material.
17. The device for preparing a visible light superhard composite coating material according to claim 16, characterized in that: The first rate monitored by the first monitoring probe is 0.2 nm / s to 0.4 nm / s; and / or the second rate monitored by the second monitoring probe is 0.8 nm / s to 1.4 nm / s.
18. The device for preparing a visible light superhard composite coating material according to claim 15, characterized in that: The coating material preparation device also includes: a third monitoring probe connected to the controller, which is used to monitor the deposition rate and / or deposition thickness of the coating material.
19. The device for preparing a visible light superhard composite coating material according to claim 18, characterized in that: The deposition rate monitored by the third monitoring probe is 0.9-1.5 nm / s; and / or the deposition thickness monitored by the third monitoring probe is 500-700 nm, wherein when the monitored deposition thickness exceeds 700 nm, the co-evaporation process is stopped.
20. The device for preparing a visible light superhard composite coating material according to any one of claims 15 to 19, characterized in that: The vacuum coating machine includes a 1300 type vacuum coating machine.
21. An anti-reflection film, characterized in that: It comprises a substrate and a film layer, wherein the film layer is attached to the substrate, wherein the film layer is a coating structure formed on the substrate by the visible light superhard composite coating material according to any one of claims 11 to 14.
Citation Information
Patent Citations
Plastic substrate hard antireflection film and coating method thereof
CN112251720A
Vacuum vapor deposition apparatus
JP2010196082A
Attenuated embedded phase shift photomask blanks
US20020119378A1
Silicon titanium oxide coating, coated article including silicon titanium oxide coating, and method of making the same
US20110081532A1
Optical coatings having a plurality of prescribed properties and methods of fabricating same
US5507870A
Cited By
Super-hard high-firmness optical protective film and preparation method thereof
CN121115184A