Method for inhibiting cracks of high-entropy alloy coating and application
By placing an intermediate layer made of high-entropy alloy main material elements between the base material and the high-entropy alloy coating, the stress is transformed, solving the problem of cracks in the high-entropy alloy coating and improving the performance and applicability of the coating.
Patent Information
- Application Number
- CN202410906849.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-15
AI Technical Summary
High-entropy alloy coatings are prone to cracks during the laser cladding process, which affects their performance. The existing preheating treatment method heats the entire substrate, resulting in reduced mechanical properties and limited applicability.
An intermediate layer is provided between the base material and the high-entropy alloy coating. The metal elements in the intermediate layer are selected from the main components of the high-entropy alloy. They are prepared by laser cladding to convert tensile stress into compressive stress, reduce coating stress, and improve adhesion. Focus.
Effectively inhibits the occurrence of cracks in high-entropy alloy coatings, improves friction resistance, and expands the scope of applications without affecting the structural structure and mechanical properties of the base material.
Smart Images

Figure HDA0004932376130000011 
Figure HDA0004932376130000012 
Figure HDA0004932376130000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high entropy alloy coatings, and in particular relates to a method and application of suppressing cracks in high entropy alloy coatings. Background Art
[0002] Laser Cladding (LC) is a method of adding different cladding materials to the surface of a substrate and using a high-energy laser beam to fuse the cladding materials with the substrate surface. Laser cladding technology has a high degree of automation, has almost no restrictions on cladding materials, and produces coatings with excellent performance. It is widely used in aerospace, molds, ships and other fields.
[0003] High-entropy alloys (HEAs) are composed of multiple elements in equal or nearly equal molar ratios, ensuring that each element does not occupy an absolute dominant position, breaking the design concept of traditional alloys. Therefore, high-entropy alloys have four major effects: high entropy effect, lattice distortion effect, diffusion hysteresis effect and cocktail effect. These effects jointly improve the performance of high-entropy alloys and give them unique physical and chemical properties, including high strength, high hardness, high wear resistance, corrosion resistance, high temperature oxidation resistance, etc., breaking through the performance limits of traditional alloys, and are expected to be used in aerospace, marine equipment and other fields, bringing unlimited possibilities for the application of high-entropy alloys.
[0004] However, during the process of forming high entropy alloys using laser cladding technology, cracks and other defects are often formed due to solidification shrinkage, thermal stress, and high entropy effect, which seriously affect the performance of high entropy alloy coatings. Therefore, how to suppress the generation of cracks in high entropy alloy coatings has become the key to realizing the application of high entropy alloy coatings using laser cladding technology.
[0005] In conventional operation, flame heating is generally used to preheat the substrate and high entropy alloy coating, converting the tensile stress between the substrate surface and the high entropy alloy coating into compressive stress to eliminate stress cracks. However, this operation method heats the entire substrate, which can easily induce changes in the matrix structure and reduce its mechanical properties; moreover, this operation method is less applicable to larger materials, and open flame heating also limits the scope of use of this operation method, resulting in its inability to be applied on a large scale. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a method and application for inhibiting cracks in a high entropy alloy coating. The method provided by the present invention prepares an intermediate layer between a substrate and a high entropy alloy coating, which can inhibit the generation of cracks in the high entropy alloy coating.
[0007] The present invention provides a method for inhibiting cracks in a high entropy alloy coating, comprising the following steps:
[0008] providing an intermediate layer between the substrate and the high entropy alloy coating;
[0009] The high entropy alloy coating comprises a high entropy alloy main material;
[0010] The metal element of the intermediate layer is selected from one of the main constituent elements of the high entropy alloy.
[0011] Preferably, the main material of the high entropy alloy includes AlCoCrFeNiTi.
[0012] Preferably, the intermediate layer comprises BNi 2 One of a nickel layer, a nickel layer and a Fe layer; the thickness of the intermediate layer is 1 to 3 mm.
[0013] Preferably, the high entropy alloy coating further comprises an additive; the additive is dispersed in the main material of the high entropy alloy;
[0014] The auxiliary agent is a mixture of ceramic particles and lubricating materials;
[0015] Preferably, the ceramic particles include one or more of oxides, carbides, nitrides and borides; the oxides include aluminum oxide and / or zirconium oxide, the carbides include one or more of silicon carbide, tungsten carbide and titanium carbide, and the nitrides include aluminum nitride and / or silicon nitride;
[0016] The lubricating material includes one of graphite, calcium fluoride, molybdenum disulfide and tungsten sulfide.
[0017] Preferably, the mass of the auxiliary agent is 0-3% of the mass of the main material of the high entropy alloy, and is not 0%;
[0018] The mass of the ceramic particles is 0-2% of the mass of the main material of the high entropy alloy, and is not 0%; the mass of the lubricating material is 0-1% of the mass of the main material of the high entropy alloy, and is not 0%.
[0019] Preferably, the preparation of the intermediate layer is carried out in a vacuum atmosphere or a protective atmosphere; the vacuum degree of the vacuum atmosphere is 5-10 Pa; the protective atmosphere is nitrogen or argon; the preparation method of the intermediate layer is laser cladding;
[0020] The parameters of the laser cladding include: laser power of 0.8-1 kW; scanning speed of 240-300 mm / min; powder feeding amount of 8-12 g / min; and overlap rate of 35-45%.
[0021] Preferably, the raw material for preparing the intermediate layer includes powder;
[0022] The powder includes BNi 2 One of powder, Ni powder and Fe powder;
[0023] The particle size of the powder is 100-300 meshes.
[0024] Preferably, the preparation of the high entropy alloy coating is carried out in a vacuum atmosphere or a protective atmosphere; the vacuum degree of the vacuum atmosphere is 5-10 Pa; the protective atmosphere is nitrogen or argon;
[0025] The preparation method of the high entropy alloy coating comprises one of laser cladding, magnetron sputtering, flame spraying, arc spraying and plasma spraying.
[0026] Preferably, the substrate comprises H13 mold steel and / or H11 mold steel.
[0027] The present invention provides a method for inhibiting cracks in a high entropy alloy coating, comprising the following steps: an intermediate layer is provided between a substrate and the high entropy alloy coating; the high entropy alloy coating comprises a high entropy alloy main material; and a metal element of the intermediate layer is selected from one of the constituent elements of the high entropy alloy main material.
[0028] The main reason for cracks in high entropy alloy coatings is that stress is generated due to different thermal expansion coefficients of different materials, resulting in cracks. The present invention can convert the tensile stress generated by the substrate and the high entropy alloy coating during laser cladding into compressive stress by arranging an intermediate layer between the substrate and the high entropy alloy coating, and release the stress to the intermediate layer, thereby reducing the stress in the high entropy alloy coating, thereby achieving the purpose of suppressing the generation of cracks in the high entropy alloy coating. Moreover, since the material of the intermediate layer is selected from one of the metal constituent elements of the main material of the high entropy alloy, the intermediate layer and the high entropy alloy coating can be fused with each other without affecting their adhesion. The method provided by the present invention will not affect the organizational structure and mechanical properties of the substrate, greatly improves the anti-friction performance of the high entropy alloy coating, and has a wide range of application space.
[0029] The results of the examples show that the surface of the high entropy alloy coating without the intermediate layer is full of cracks (see Figure 4 , the red stripes in the figure are cracks), while the surface of the high entropy alloy coating used to prepare the intermediate layer is white, and there are basically no cracks (see Figure 1 ), indicating that the method provided by the present invention is effective and can effectively inhibit the generation of cracks in the high entropy alloy coating. The wear depth of the high entropy alloy coating without the intermediate layer is very deep, while the high entropy alloy coating with the intermediate layer is basically free of wear, and the wear amount is reduced by 30%. The hardness is higher than that of the high entropy alloy coating without the intermediate layer. The increase or unchanged hardness indicates that the high entropy alloy coating has basically no cracks and excellent performance.
[0030] The present invention also provides the use of the method for inhibiting cracks in the high entropy alloy coating described in the above scheme in the preparation of the high entropy alloy coating. The high entropy alloy coating prepared by the method provided by the present invention has excellent performance and no cracks; and is suitable for a variety of substrates and can be used in a variety of extreme environmental conditions, greatly expanding the application range of the high entropy alloy coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The flaw detection image of the high entropy alloy coating prepared in Example 1;
[0032] Figure 2 This is the SEM-EDS image of the high entropy alloy prepared in Example 1;
[0033] Figure 3 This is a wear morphology diagram of the high entropy alloy prepared in Example 1;
[0034] Figure 4 The flaw detection image of the high entropy alloy coating prepared in Comparative Example 1;
[0035] Figure 5 This is the SEM-EDS image of the high entropy alloy prepared in Comparative Example 1;
[0036] Figure 6 This is a wear morphology diagram of the high entropy alloy prepared in Comparative Example 1;
[0037] Figure 7 This is the wear morphology of the substrate H13 mold steel in blank test example 1. DETAILED DESCRIPTION
[0038] The present invention provides a method for inhibiting cracks in a high entropy alloy coating, comprising the following steps:
[0039] providing an intermediate layer between the substrate and the high entropy alloy coating;
[0040] The high entropy alloy coating comprises a high entropy alloy main material;
[0041] The metal element of the intermediate layer is selected from one of the main constituent elements of the high entropy alloy.
[0042] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0043] In the present invention, the substrate preferably comprises H13 die steel and / or H11 die steel, more preferably H13 die steel.
[0044] In the present invention, the substrate is preferably a plate, and the size of the plate is preferably 200×50×20 mm. Before preparing the intermediate layer, the present invention preferably pre-treats the substrate, and the pre-treatment preferably includes polishing, cleaning and sandblasting in sequence. In the present invention, the polishing is preferably sandpaper polishing, and the sandpaper polishing preferably includes polishing with 240#, 400#, 800#, 1200# and 2000# sandpaper in sequence until there are no scratches visible to the naked eye on the surface of the substrate. In the present invention, the cleaning is preferably alcohol cleaning. In the present invention, the particle size of the abrasive used in the sandblasting is preferably 1 to 2 mm.
[0045] In the present invention, the high entropy alloy coating comprises a high entropy alloy main material. In the present invention, the high entropy alloy main material preferably comprises AlCoCrFeNiTi. In the present invention, the metal element of the intermediate layer is selected from one of the constituent elements of the high entropy alloy main material. In the present invention, the intermediate layer preferably comprises BNi 2 One or more of a layer, a Ni layer and a Fe layer, more preferably BNi 2 In the present invention, the thickness of the intermediate layer is preferably 1 to 3 mm.
[0046] In the present invention, the step of preparing the intermediate layer preferably includes: spreading the raw materials for preparing the intermediate layer on the surface of the substrate, and performing laser cladding to obtain the intermediate layer.
[0047] In the present invention, the raw material for preparing the intermediate layer preferably includes powder. In the present invention, the powder preferably includes BNi 2 One or more of powder, Ni powder and Fe powder, more preferably BNi 2 Powder. In the present invention, the particle size of the powder is preferably 100-300 mesh, more preferably 100-200 mesh. The present invention selects the same metal element as the main component element of the high entropy alloy as the raw material for preparing the intermediate layer, so that the intermediate layer and the high entropy alloy coating can be fused with each other, and there is no problem of peeling of the high entropy alloy coating and the intermediate layer or substrate.
[0048] In the present invention, the preparation of the intermediate layer is preferably carried out in a vacuum atmosphere or a protective atmosphere, the vacuum degree of the vacuum atmosphere is preferably 5-10Pa, and the protective atmosphere is preferably nitrogen or argon. In the present invention, the method of laying the raw materials for preparing the intermediate layer on the surface of the substrate is preferably coaxial powder feeding. In the present invention, the method for preparing the intermediate layer is preferably laser cladding. In the present invention, the parameters of the laser cladding include: the laser power is preferably 0.8-1kW, more preferably 0.9-1kW; the scanning speed is preferably 240-300mm / min, more preferably 240-280mm / min; the powder feeding amount is preferably 8-12g / min, more preferably 8-10g / min; the overlap rate is preferably 35-45%.
[0049] After the intermediate layer is obtained, the present invention prepares a high entropy alloy coating on the surface of the intermediate layer.
[0050] Before preparing the high entropy alloy coating, the present invention preferably pre-treats the surface of the intermediate layer, and the pre-treatment preferably includes polishing, cleaning and sandblasting in sequence. In the present invention, the polishing is preferably sandpaper polishing, and the sandpaper polishing preferably includes polishing with 240#, 400#, 800#, 1200# and 2000# sandpaper in sequence until there are no visible scratches on the surface of the intermediate layer. In the present invention, the cleaning is preferably alcohol cleaning. In the present invention, the particle size of the abrasive used in the sandblasting is preferably 1 to 2 mm.
[0051] In the present invention, the high entropy alloy coating preferably also includes an additive, which, as a reinforcing phase, is uniformly dispersed in the high entropy alloy main material, giving the high entropy alloy coating higher mechanical properties, lubrication properties and wear resistance. In the present invention, the additive is preferably a mixture of ceramic particles and lubricating materials. In the present invention, the mass of the additive is preferably 0 to 3% of the mass of the high entropy alloy main material, and is not 0, more preferably 0.5 to 1.5%, and further preferably 0.8 to 1.2%.
[0052] In the present invention, the ceramic particles preferably include one or more of oxides, carbides, nitrides and borides. In the present invention, the oxides preferably include aluminum oxide and / or zirconium oxide; the carbides preferably include one or more of silicon carbide, tungsten carbide and titanium carbide; the nitrides preferably include aluminum nitride and / or silicon nitride. In the present invention, the mass of the ceramic particles is preferably 0 to 2% of the mass of the main material of the high entropy alloy, and is not 0, more preferably 0.5 to 1.5%, and further preferably 0.8 to 1.2%. In the present invention, the lubricating material preferably includes one of graphite, calcium fluoride, molybdenum disulfide and tungsten sulfide, and is more preferably one of graphite, calcium fluoride and molybdenum disulfide. In the present invention, the mass of the lubricating material is preferably 0 to 1% of the mass of the main material of the high entropy alloy, and is not 0, and is more preferably 0.5 to 0.8%.
[0053] In the present invention, the preparation method of the high entropy alloy coating preferably includes one of laser cladding, magnetron sputtering, flame spraying, arc spraying and plasma spraying, and laser cladding is more preferred.
[0054] In the present invention, the preparation step of the high entropy alloy coating preferably includes: spreading the high entropy alloy main material and auxiliary agent on the surface of the intermediate layer, performing laser cladding, and obtaining the high entropy alloy coating.
[0055] In the present invention, the preparation of the high entropy alloy coating is preferably carried out in a vacuum atmosphere or a protective atmosphere, the vacuum degree of the vacuum atmosphere is preferably 5-10Pa, and the protective atmosphere is preferably nitrogen or argon. In the present invention, the method of paving the high entropy alloy main material and auxiliary agent on the surface of the intermediate layer is preferably coaxial powder feeding. In the present invention, the parameters of laser cladding used to prepare the high entropy alloy coating include: the laser power is preferably 0.9-1.6kW, more preferably 0.9-1.2kW; the scanning speed is preferably 240-300mm / min, more preferably 240-260mm / min; the powder feeding amount is preferably 20-28g / min, more preferably 24-28g / min; the overlap rate is preferably 35-45%.
[0056] The present invention prepares the intermediate layer and the high entropy alloy coating in a vacuum atmosphere or a protective atmosphere, thereby reducing the contact between the intermediate layer and the high entropy alloy coating and air, ensuring that the metal is not affected by oxidation before and after cladding, thereby ensuring the excellent performance of the intermediate layer and the high entropy alloy coating.
[0057] The present invention adopts the method of laser cladding to prepare the intermediate layer and the high entropy alloy coating. On the one hand, the preparation of the intermediate layer and the high entropy alloy coating can complete all preparation steps on the same equipment, which is simple to operate and reduces the influence of the external environment and unknown variables on the performance of the intermediate layer and the high entropy alloy coating. On the other hand, the high entropy alloy coating prepared by laser cladding has a good appearance and morphology, no cracks, and no obvious changes in hardness and strength, which overcomes the problem that the high entropy alloy coating is prone to cracks.
[0058] The method for suppressing cracks in a high entropy alloy coating provided by the present invention is used to prepare a high entropy alloy coating, which has substantially no effect on the performance of the substrate. The prepared high entropy alloy coating has excellent performance, greatly expanding the application range of the high entropy alloy coating.
[0059] The technical solution of the present invention is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0060] Example 1
[0061] A method for suppressing cracks in laser cladding AlCoCrFeNiTi high entropy alloy coatings comprises the following steps:
[0062] Select a 200×50×20mm H13 steel plate, first grind its surface, then clean it with alcohol to remove surface oil, then sandblast the substrate surface, and blow dry the remaining sandblasting sand on the workpiece surface. Start to introduce protective gas argon, use coaxial powder feeding to lay BNi on the pre-treated clean steel plate surface 2 Powder, BNi prepared by laser cladding 2The main process parameters of the laser cladding preparation of the intermediate layer are: laser power of 0.8 kW, scanning speed of 250 mm / min, powder feeding amount of 10 g / min, overlap rate of 40%. The thickness of the intermediate layer obtained is 2 mm.
[0063] The obtained intermediate layer was polished, cleaned and sandblasted until there were no visible scratches on the surface. The protective gas argon was continued to be introduced, and the high entropy alloy main material AlCoCrFeNiTi was flattened on the surface of the pretreated intermediate layer by coaxial powder feeding. The main process parameters for preparing the high entropy alloy coating by laser cladding were: laser power of 1 kW, scanning speed of 280 mm / min, powder feeding amount of 28 g / min, overlap rate of 40%, and a high entropy alloy AlCoCrFeNiTi coating was obtained.
[0064] The high entropy alloy coating prepared in Example 1 was tested by using a colored penetrant flaw detector. The results are as follows: Figure 1 It can be seen that the high entropy alloy coating prepared in Example 1 is well formed and has no cracks on the surface.
[0065] According to the standard GB / T 230.1-2018, the hardness of the high entropy alloy coating prepared in Example 1 was tested using a microhardness tester, and the test result was: 731HV 0.2 .
[0066] The microstructure and element distribution of the high entropy alloy coating prepared in Example 1 were tested by scanning electron microscopy. The test results are as follows: Figure 2 As shown, from Figure 2 It can be seen that the atomic ratio of AlCoCrFeNiTi elements in the high entropy alloy coating is 1:1:1:1:1:1, which is the same as the proportion of each element in the main material of the high entropy alloy AlCoCrFeNiTi. It can be seen that the preparation of the intermediate layer does not affect the proportion of each element in the high entropy alloy coating, and the elements in the high entropy alloy coating do not change due to the addition of the intermediate layer.
[0067] According to the standard GB / T 17754-2012, the wear loss of the high entropy alloy coating prepared in Example 1 was tested by a friction and wear tester, and the load was set to 100N. The test result was: 2.1×10 8 μm 3 Wear morphology Figure 3 As shown, from Figure 3 It can be seen that: Figure 3 The medium orange color represents the coating surface, and the yellow color represents the wear scar area. The deepest wear scar of the high entropy alloy coating is 50-70 μm, which is lower than the wear depth of the substrate H13 steel of 120-130 μm. The addition of an intermediate layer in the present invention can effectively improve the wear resistance of the high entropy alloy coating, and can be used on the surface of mold steel to extend its service life.
[0068] Example 2
[0069] The only difference from Example 1 is that the middle layer is a Ni layer.
[0070] The test result is: hardness 735.2HV 0.2 , wear amount 2.14×10 8 μm 3 .
[0071] Example 3
[0072] The difference from Example 1 is that graphite and the high entropy alloy main material AlCoCrFeNiTi are evenly mixed, the mass of graphite is 0.8% of the mass of the high entropy alloy main material AlCoCrFeNiTi, the evenly mixed high entropy alloy coating powder is spread on the surface of the pretreated intermediate layer by coaxial powder feeding, and the main process parameters for preparing the high entropy alloy coating by laser cladding are: laser power of 1 kW, scanning speed of 280 mm / min, powder feeding amount of 28 g / min, overlap rate of 40%, and a high entropy alloy coating is obtained, and a high entropy alloy coating containing a graphite lubricating phase is prepared.
[0073] The test result is: hardness 845.2HV 0.2 , wear amount 1.5×10 8 μm 3 .
[0074] Example 4
[0075] The difference from Example 1 is that the molybdenum disulfide powder and the high entropy alloy main material AlCoCrFeNiTi are evenly mixed, the mass of the molybdenum disulfide powder is 0.8% of the mass of the high entropy alloy main material AlCoCrFeNiTi, and the evenly mixed high entropy alloy coating powder is spread on the surface of the pretreated intermediate layer by coaxial powder feeding. The main process parameters for preparing the high entropy alloy coating by laser cladding are: laser power of 1 kW, scanning speed of 280 mm / min, powder feeding amount of 28 g / min, overlap rate of 40%, and a high entropy alloy coating is obtained, and a high entropy alloy coating containing a molybdenum disulfide lubricating phase is prepared.
[0076] The test result is: hardness 800.1HV 0.2 , wear volume 1.68×10 8 μm 3 .
[0077] Comparative Example 1
[0078] The only difference from Example 1 is that no intermediate layer is prepared.
[0079] The high entropy alloy coating prepared in Comparative Example 1 was tested using a colored penetrant flaw detector. The results are as follows: Figure 4 As shown, it can be seen that the high entropy alloy coating prepared in Comparative Example 1 has cracks on almost the entire surface, and the red parts are all cracks that appear after being treated with a colored penetrant flaw detector.
[0080] According to the standard GB / T 230.1-2018, the hardness of the high entropy alloy coating prepared in Comparative Example 1 was tested using a microhardness tester, and the test result was: 720HV 0.2 .
[0081] The microstructure and element distribution of the high entropy alloy coating prepared in Comparative Example 1 were tested by scanning electron microscopy. The test results are as follows: Figure 5 As shown, from Figure 5 It can be seen that the atomic ratio of each element in the high entropy alloy coating is Al:Ti:Cr:Fe:Co:Ni=1:1:1:1:1:1:1.
[0082] According to the standard GB / T 17754-2012, the wear loss of the high entropy alloy coating prepared in Comparative Example 1 was tested by a friction and wear tester, and the load was set to 100N. The test result was: 2.7×10 8 μm 3 , wear morphology such as Figure 6 As shown, from Figure 6 It can be seen that the deepest wear depth of the high entropy alloy coating is between 100 and 120 μm.
[0083] Blank test example 1
[0084] Only the wear of the substrate H13 mold steel was tested. According to the standard GB / T 17754-2012, the wear of the substrate H13 mold steel was tested using a friction and wear tester. The load was set to 100N. The test result was: 2.9×10 8 μm 3 , wear morphology such as Figure 7 As shown, from Figure 7 It can be seen that the deepest wear depth of the H13 mold steel substrate is 120-130μm.
[0085] Comparison between Example 1 and Comparative Example 1: After the intermediate layer is prepared, the performance of the high entropy alloy coating does not decrease; cracks have a significant impact on wear performance, which is characterized by wear volume, and the smaller the wear volume, the more wear-resistant it is.
[0086] The deepest wear amount of the high entropy alloy coating obtained in Example 1 is 50-70 μm; the deepest wear amount of the high entropy alloy coating obtained in Comparative Example 1 is 100-120 μm; the deepest wear amount of the substrate H13 mold steel in Blank Test Example 1 is 120-130 μm; by comparison, it can be seen that the wear amount of the high entropy alloy coating in Comparative Example 1 is not much different from the wear amount of the substrate H13 mold steel, indicating that there is no intermediate layer, and the cracks generated on the high entropy alloy coating will seriously affect the wear performance of the high entropy alloy coating. The wear amount of the high entropy alloy coating in Example 1 is much lower than the wear amount in Comparative Example 1 and Blank Test Example 1, indicating that the addition of an intermediate layer can effectively improve the wear resistance of the high entropy alloy coating, and can be used on the surface of mold steel to extend the service life.
[0087] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for inhibiting cracks in a high entropy alloy coating, characterized in that: The following steps are involved: providing an intermediate layer between the substrate and the high entropy alloy coating; The high entropy alloy coating comprises a high entropy alloy main material; The metal element of the intermediate layer is selected from one of the main constituent elements of the high entropy alloy.
2. The method for suppressing cracks in a high entropy alloy coating according to claim 1, characterized in that: The main material of the high entropy alloy includes AlCoCrFeNiTi.
3. The method for suppressing cracks in a high entropy alloy coating according to claim 2, characterized in that: The intermediate layer includes one of a BNi2 layer, a Ni layer and a Fe layer; and the thickness of the intermediate layer is 1 to 3 mm.
4. The method for suppressing cracks in a high entropy alloy coating according to claim 1, characterized in that: The high entropy alloy coating further comprises an additive; the additive is dispersed in the main material of the high entropy alloy; The auxiliary agent is formed by mixing ceramic particles and lubricating materials.
5. The method for suppressing cracks in a high entropy alloy coating according to claim 4, characterized in that: The ceramic particles include one or more of oxides, carbides, nitrides and borides; the oxides include aluminum oxide and / or zirconium oxide, the carbides include one or more of silicon carbide, tungsten carbide and titanium carbide, and the nitrides include aluminum nitride and / or silicon nitride; The lubricating material includes one of graphite, calcium fluoride, molybdenum disulfide and tungsten sulfide.
6. The method for suppressing cracks in a high entropy alloy coating according to claim 4, characterized in that: The mass of the auxiliary agent is 0-3% of the mass of the main material of the high entropy alloy, and is not 0%; The mass of the ceramic particles is 0-2% of the mass of the main material of the high entropy alloy, and is not 0%; the mass of the lubricating material is 0-1% of the mass of the main material of the high entropy alloy, and is not 0%.
7. The method for suppressing cracks in a high entropy alloy coating according to claim 1, characterized in that: The preparation of the intermediate layer is carried out in a vacuum atmosphere or a protective atmosphere; the vacuum degree of the vacuum atmosphere is 5-10 Pa; the protective atmosphere is nitrogen or argon; the preparation method of the intermediate layer is laser cladding; The parameters of the laser cladding include: laser power of 0.8-1 kW; scanning speed of 240-300 mm / min; powder feeding amount of 8-12 g / min; and overlap rate of 35-45%.
8. The method for suppressing cracks in a high entropy alloy coating according to claim 3, characterized in that: The raw materials for preparing the intermediate layer include powder; The powder material comprises one of BNi2 powder, Ni powder and Fe powder; The particle size of the powder is 100-300 meshes.
9. The method for suppressing cracks in a high entropy alloy coating according to claim 1 or 2, characterized in that: The high entropy alloy coating is prepared in a vacuum atmosphere or a protective atmosphere; the vacuum degree of the vacuum atmosphere is 5-10 Pa; the protective atmosphere is nitrogen or argon; The preparation method of the high entropy alloy coating comprises one of laser cladding, magnetron sputtering, flame spraying, arc spraying and plasma spraying.
10. The method for suppressing cracks in a high entropy alloy coating according to claim 1, characterized in that: The substrate includes H13 mold steel and / or H11 mold steel.
Citation Information
Patent Citations
Coating of copper-based surface intermetallic compound reinforced gradient high-entropy alloy and preparation method
CN113564577A
High-entropy alloy / hard ceramic synergistically reinforced composite coating and preparation method thereof
CN115029601A
High-entropy carbide ceramic material, carbide ceramic coating and preparation methods and use thereof
US20230183851A1
Cited By
Method for assisting high-temperature alloy TLP connection by adding high-entropy alloy nanoparticles to middle layer
CN119927400A
A method for TLP bonding of high-temperature alloy with interlayer added high-entropy alloy nanoparticles
CN119927400B