High-speed acousto-optic modulation composite waveguide structure and preparation method thereof

The composite waveguide structure is formed through stacked deposition of AlN and AlScN, which solves the problems of poor lattice matching between the optical waveguide and the piezoelectric film and surface acoustic wave leakage in the AlN acousto-optic modulator, and realizes CMOS-compatible, low-cost acousto-optic modulation. The device design improves the acousto-optic modulation efficiency.

CN118778299APending Publication Date: 2024-10-15XIDIAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411157499.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-10-15

Smart Images

  • Figure CN118778299A_ABST
    Figure CN118778299A_ABST
Patent Text Reader

Abstract

The invention discloses a high-speed acousto-optic modulation composite waveguide structure and a preparation method thereof, and mainly solves the problems that in an existing aluminum nitride-based acousto-optic modulator, the acoustic surface wave intensity is low, and optical mode propagation is affected by crystal structure defects in a scandium-doped aluminum nitride optical waveguide. According to the scheme, a silicon substrate, a silicon dioxide buried layer and a waveguide modulation region are arranged from bottom to top, and the silicon dioxide buried layer is subjected to cavity digging treatment or replaced by a Bragg reflection cavity; wherein the waveguide modulation area comprises a composite structure, an interdigital transducer and a covering protection layer, and the composite structure is formed by laminating and depositing a waveguide made of aluminum nitride and a piezoelectric layer doped with aluminum nitride; the covering protection layer covers the upper surface of the composite structure. Good lattice matching of the optical waveguide and the piezoelectric film can be achieved, the CMOS compatible characteristic is achieved, and the size and cost of the acousto-optic modulator are remarkably reduced under the conditions that the sound field and the light field are well coupled and the acousto-optic modulation efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of aluminum nitride photonic integrated circuits, and relates to a composite waveguide structure formed by aluminum nitride grown on an insulator and doped aluminum nitride, specifically a high-speed acousto-optic modulation composite waveguide structure and a preparation method thereof, which can be used for high-speed modulation of on-chip photoelectric signals. Background Art

[0002] With the rapid development of the field of microelectronics, the integration of chips is getting higher and higher, the electrical interconnection of chips is getting denser and denser, the thermal management of chips is becoming more and more difficult, and the process yield and reliability of chips are gradually declining. In addition, the method of using electrical signal processing requires frequent conversion between photoelectricity, which consumes a lot of energy and has the problem of low photoelectric conversion efficiency. Optical communication has the advantages of low transmission loss, strong anti-electromagnetic interference ability, fast data transmission speed, and low heat loss. In this case, more and more people are turning their attention to optical communication. The optical modulator is the core component of short-distance optical communication technology. By loading the external signal onto the optical carrier, the phase of the optical carrier is modulated. Among optical modulators, the acousto-optic modulator is an optical device that loads the acoustic wave signal onto the optical carrier for modulation. Compared with the electro-optic modulator, it can provide higher modulation frequency, larger extinction ratio, better temperature stability, and lower driving power. It is expected to replace the electro-optic modulator in certain working environments and realize on-chip acousto-optic integration and acousto-optic modulation.

[0003] In a bulk acoustic wave (BAW) acousto-optic modulator, acoustic waves are generated by the inverse piezoelectric effect of a crystal several centimeters thick and interact with light waves propagating in the crystal. This control method has poor binding capacity for photon and phonon energy, resulting in weak acousto-optic interaction in the medium. Compared with bulk materials, photonic integrated circuits can well confine surface acoustic waves (SAW) and light waves in a thin film, achieve high acousto-optic overlap within the wavelength scale, and significantly enhance the coupling between the acoustic field and the light field. Only a very small driving power is required to achieve a very good acousto-optic effect, thereby realizing a miniaturized, high-performance, and low-cost integrated acousto-optic modulator. With the rapid development of thin film piezoelectric materials, integrated acousto-optic modulators have been realized on multiple piezoelectric material platforms, such as aluminum nitride (AlN) and lithium niobate (LN).

[0004] An acousto-optic modulator is a device that converts high-speed radio frequency electrical signals into modulated optical signals through the elastic-optic effect. The specific working principle is: the radio frequency source sends out an electrical signal, which is loaded onto the interdigital electrodes of the interdigital transducer IDT. Through the inverse piezoelectric effect of the piezoelectric film, the electrical signal is converted into an acoustic vibration sound signal of the same frequency, which propagates on the surface or body of the medium in the form of an acoustic wave. When the vibration signal is transmitted to the optical waveguide, the stress generated by the deformation causes the refractive index of the waveguide to change, thereby modulating the phase of the optical signal propagating in the waveguide, and achieving the purpose of efficient electro-optical conversion. At present, an important factor restricting the development of acousto-optic modulators is the selection of high-performance piezoelectric films, which requires piezoelectric films to have high piezoelectric coefficients, CMOS process compatibility, small film thickness, and good lattice matching with optical waveguides. At present, the research on acousto-optic modulators mainly focuses on LN and AlN piezoelectric films. The optical waveguide and piezoelectric film are mainly combined by heterogeneous integration or homogeneous integration on the same substrate material and placed adjacently. Since LN cannot be deposited at low temperature, the use of LN as a piezoelectric film is incompatible with CMOS technology and is expensive, which cannot meet the needs of low-cost mass production. Although AlN can be deposited into polycrystalline films with nearly single-crystal performance at low temperature (350°C) through magnetron sputtering, it is difficult to apply it in the field of acousto-optic modulators due to its extremely small piezoelectric coefficient.

[0005] At present, the acousto-optic modulator with AlN as the piezoelectric layer has a piezoelectric coefficient d 33 The problem is that the intensity of the surface acoustic wave generated is weak, and it is impossible to achieve good coupling between the sound field and the light field, and the coupling efficiency is low. With the continuous development of piezoelectric material modification and doping technology, AlN can significantly improve its piezoelectric coefficient by element doping, such as scandium-doped aluminum nitride AlScN, which can reduce the piezoelectric coefficient of AlN to d 33Increased by 3-5 times. In addition, the Sc element is doped in AlN in a substitutional manner. When AlN is used as an optical waveguide and AlScN is integrated as a piezoelectric film, the lattice matching degree at the interface between the two is high, and the problem of internal stress caused by lattice mismatch affecting device performance will not occur at the interface. Therefore, the research on AlN acousto-optic modulators has made great progress. The existing AlN acousto-optic modulator uses AlScN as a piezoelectric film and Si as an optical waveguide, which can achieve a larger modulation bandwidth and modulation frequency. However, since the optical waveguide and the piezoelectric film are heterogeneously integrated together, the lattice structures of the two are different, and there is a lattice mismatch at the interface. The two are prone to internal stress at the interface during the growth process, which affects the performance of the device, and it is difficult to miniaturize the device size and the cost is high. In addition, AlScN acousto-optic modulators are also currently being studied. By etching the AlScN material into a ridge structure, it can be used as both a piezoelectric film and a ridge waveguide to propagate light modes, achieving a good match between the piezoelectric film and the optical waveguide lattice. However, AlScN material has many crystal structure defects, and the propagation of light modes is very sensitive to defects. AlScN is not a good choice as an optical waveguide in an acousto-optic modulator, which seriously affects the propagation of light modes. Summary of the invention

[0006] The present invention aims to address the deficiencies of the prior art and propose a high-speed acousto-optic modulation composite waveguide structure and a preparation method thereof, which are used to solve the technical problems that the poor lattice matching between the optical waveguide and the piezoelectric film in the current AlN acousto-optic modulator leads to incompatibility with the CMOS process and difficulty in device size miniaturization, the crystal structure defects of AlScN as an optical waveguide seriously affect the propagation of the optical mode, and the surface acoustic wave generated in the AlScN piezoelectric layer is easy to leak downward, resulting in low acoustic-optic coupling efficiency. Firstly, by adopting AlN and AlScN stacked deposition growth to form a composite waveguide structure, the optical mode is mainly confined in the AlN optical waveguide, and the AlScN piezoelectric layer is mainly used to generate strong surface acoustic waves. The two perform their respective functions, and the optical mode will not be affected by the crystal structure defects in the AlScN piezoelectric layer. Secondly, AlScN is obtained by substitutional doping of Sc elements in AlN. AlN and AlScN have similar lattice structures. Through the stacked deposition growth of the two, good lattice matching between the optical waveguide and the piezoelectric layer is achieved, which has CMOS compatibility characteristics and is easy to miniaturize the device size. Finally, by hollowing out a cavity in the SiO2 buried layer or replacing the SiO2 buried layer with a Bragg reflection cavity formed by overlapping high acoustic impedance materials and low acoustic impedance materials layer by layer, the surface acoustic wave generated in the AlScN piezoelectric layer is suppressed from leaking downward or the leaked surface acoustic wave is reflected back, thereby achieving good coupling between the surface acoustic wave and the optical mode and improving the acoustic-optical coupling efficiency. The present invention can achieve good lattice matching between the optical waveguide and the piezoelectric film, has CMOS compatibility, is easy to achieve device size miniaturization, significantly reduces the size and cost of the acousto-optic modulator, achieves good coupling between the acoustic field and the optical field, improves the efficiency of the acousto-optic modulation, has good commercial application prospects, and provides a basic solution for the development of large-scale low-cost integrated acousto-optic modulators.

[0007] In order to solve the above problems, the technical solution proposed by the present invention is as follows:

[0008] A high-speed acousto-optic modulation composite waveguide structure, comprising, from bottom to top, a silicon substrate 1, a silicon dioxide buried layer 2, and a waveguide modulation region 3;

[0009] The silicon dioxide buried layer 2 is hollowed out to contain a cavity 21;

[0010] The waveguide modulation region 3 includes a composite structure 31, an interdigital transducer 32 and a covering protective layer 33; the composite structure 31 is composed of a waveguide 311 and a piezoelectric layer 312, wherein the waveguide 311 is made of aluminum nitride film material, and the piezoelectric layer 312 is made of doped aluminum nitride film material;

[0011] The composite structure 31 is located above the silicon dioxide buried layer 2, and the composite structure 31 includes a waveguide 311 and a piezoelectric layer 312 in close contact;

[0012] The interdigital transducer 32 is located on one side of the waveguide 311 and is located on the upper surface of the piezoelectric layer 312 and above the cavity 21;

[0013] The covering protection layer 33 is located above the waveguide 311 and covers the upper surfaces of the waveguide 311 and the piezoelectric layer 312 .

[0014] A method for preparing a high-speed acousto-optic modulation composite waveguide structure comprises the following steps:

[0015] S1. Pre-treating the silicon wafer to obtain a pre-treated Si substrate;

[0016] S2. Forming a SiO2 buried layer on the pretreated Si substrate by plasma enhanced chemical vapor deposition PECVD growth or thermal oxidation process;

[0017] S3. The portion deposited on the upper surface of the SiO2 buried layer is polished by chemical mechanical polishing CMP;

[0018] S4. Growing an AlScN layer having a preferred c-axis orientation on the layer obtained in step S3 by magnetron sputtering;

[0019] S5. Continue to grow an AlN layer on the AlScN layer by magnetron sputtering, and coat the grown AlN layer with a photoresist for photolithography, and then etch it by inductively coupled plasma-reactive ion etching ICP-RIE technology to obtain an AlN waveguide structure on the top of the AlScN layer;

[0020] S6. Depositing a covering protective layer on the composite structure composed of AlScN and AlN by atomic layer deposition or magnetron sputtering process;

[0021] S7. coating a photoresist on the substrate covered with the protective layer and performing photolithography, depositing a metal electrode by electron beam evaporation or magnetron sputtering, and performing metal patterning and stripping to obtain an interdigitated electrode;

[0022] S8. Continue to apply photoresist and perform photolithography, and cover the protective layer by inductively coupled plasma-reactive ion etching ICP-RIE technology or wet etching, so that the interdigital electrodes are exposed to the air;

[0023] S9. Continue to apply photoresist and perform photolithography, and sequentially etch the AlScN layer covering the protective layer until the silicon dioxide buried layer by inductively coupled plasma-reactive ion etching ICP-RIE technology to obtain a release groove structure;

[0024] S10. placing the structure obtained in steps S1-S9 in an HF acid solution or a buffered oxide etchant, and removing the silicon dioxide buried layer under the waveguide modulation region through the release groove structure, thereby making the waveguide modulation region suspended;

[0025] S11. Complete the preparation process and obtain a high-speed acousto-optic modulator with a composite waveguide structure.

[0026] Compared with the prior art, the present invention has the following advantages:

[0027] First, since the present invention uses AlN and AlScN to form a composite waveguide structure, the optical waveguide and the piezoelectric film have a high lattice matching degree, and the CMOS process compatibility of the two is achieved, which facilitates device size miniaturization and reduces manufacturing costs.

[0028] Second, since the present invention digs a cavity in the SiO2 buried layer, the downward leakage of the surface acoustic wave generated by the AlScN piezoelectric layer is suppressed, thereby achieving good coupling between the surface acoustic wave and the optical mode.

[0029] Thirdly, since the SiO2 buried layer is replaced by a Bragg acoustic reflection cavity in the present invention, the surface acoustic wave leaking downward is reflected back to the AlScN piezoelectric layer by the Bragg reflection cavity, thereby improving the acoustic-optical coupling efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the overall structure of the present invention;

[0031] Figure 2 is a schematic diagram of the composite waveguide structure of the present invention;

[0032] Figure 3 It is a schematic diagram of simulation results of the present invention;

[0033] Figure 4 It is a schematic diagram of the high-speed acousto-optic modulation composite waveguide structure provided in Embodiment 3 of the present invention;

[0034] Figure 5 Schematic diagram of the high-speed acousto-optic modulation composite waveguide structure provided in Embodiment 4 of the present invention;

[0035] Figure 6 Schematic diagram of the high-speed acousto-optic modulation composite waveguide structure provided in Embodiment 5 of the present invention;

[0036] Figure 7 is a schematic structural diagram of a Bragg reflection cavity layer in the present invention;

[0037] Figure 8 is a schematic diagram of a waveguide delay line constructed based on the waveguide structure of the present invention;

[0038] Fig. 9 is a schematic diagram of a micro-ring modulator constructed based on the waveguide structure of the present invention;

[0039] Fig.10 Schematic diagram of a Mach-Zehnder MZ modulator constructed based on the waveguide structure of the present invention;

[0040] Fig.11 It is a schematic diagram of a one-dimensional photonic crystal nanobeam resonant cavity modulator constructed based on the waveguide structure of the present invention. DETAILED DESCRIPTION

[0041] The present invention will be further described below in conjunction with the accompanying drawings.

[0042] Embodiment 1: Refer to the attached Figure 1-7 The high-speed acousto-optic modulation composite waveguide structure provided in this embodiment includes, from bottom to top, a silicon substrate 1, a silicon dioxide buried layer 2, and a waveguide modulation region 3;

[0043] The silicon dioxide buried layer 2 is hollowed out to contain a cavity 21. The silicon dioxide buried layer 2 can also be replaced by a Bragg reflection cavity layer 4 formed by alternately stacking low acoustic impedance material 41 and high acoustic impedance material 42, wherein the thickness of the low acoustic impedance material 41 is λ IDT· v L-DBR / 4v p , the thickness of the high acoustic impedance material 42 is λ IDT· v H-DBR / 4v p , where λ IDT is the period of the IDT 32, v L-DBR and v H-DBR are the acoustic velocities in the low acoustic impedance material 41 and the high acoustic impedance material 42, respectively, and v P is the acoustic velocity in the piezoelectric layer 312 .

[0044] The waveguide modulation region 3 includes a composite structure 31, an interdigital transducer 32 and a covering protective layer 33; the composite structure 31 is composed of a waveguide 311 and a piezoelectric layer 312, wherein the waveguide 311 is made of aluminum nitride film material, and the piezoelectric layer 312 is made of doped aluminum nitride film material;

[0045] The composite structure 31 is located above the silicon dioxide buried layer 2, and the composite structure 31 includes a waveguide 311 and a piezoelectric layer 312 in close contact; in this embodiment, the piezoelectric layer 312 is made of doped aluminum nitride material, wherein the doping element is scandium Sc or boron B, and the doping element is doped into the aluminum nitride by substitutional doping, and the doping ratio is 0 to 45%; the thickness of the waveguide 311 is greater than the thickness of the piezoelectric layer 312, wherein the thickness of the waveguide 311 is greater than 100nm, and the thickness of the piezoelectric layer 312 is greater than 10nm.

[0046] Furthermore, the waveguide 311 is a strip-structure waveguide 313 or a ridge-structure waveguide 314. When the waveguide 311 is a strip-structure waveguide 313, it is located between the piezoelectric layer 312 and the cover protective layer 33 in the waveguide modulation region 3, and is in close contact with the piezoelectric layer 312 and the cover protective layer 33, respectively. When the waveguide 311 is a ridge-structure waveguide 314, it is covered by the piezoelectric layer 315 and the cover protective layer 33, and the waveguide is located below the piezoelectric layer 315 and in close contact with it; the piezoelectric layer 315 is located below the cover protective layer 33 and in close contact with it.

[0047] The interdigital transducer 32 is located on one side of the waveguide 311 and is located on the upper surface of the piezoelectric layer 312 and above the cavity 21;

[0048] The covering protective layer 33 is located above the waveguide 311, covering the upper surface of the waveguide 311 and the piezoelectric layer 312; the optical refractive index of the covering protective layer 33 is less than the optical refractive index of the waveguide 311, and the thickness is less than the thickness of the waveguide 311; the material of the covering protective layer 33 is Si3N4, TiN, Al2O3 or SiO2, etc. In this embodiment, the covering protective layer 33 preferably uses a low-refractive-index TiN single-layer thin film material with a larger film thickness, or a high-refractive-index Si3N4 single-layer thin film material with a smaller film thickness.

[0049] Embodiment 2: Refer to the attached Figure 1-11 The overall structure of the composite waveguide proposed in this embodiment is the same as that in the first embodiment. Now, its structural design, technical principle and specific application are further described:

[0050] 1. Specific structure:

[0051] Reference Figure 1 In this embodiment, a high-speed acousto-optic modulation composite waveguide structure is proposed, in which an AlN waveguide and an AlScN piezoelectric film form a composite structure that is deposited and grown on top of an insulator SiO2 buried layer, and the SiO2 buried layer is hollowed out to limit the downward leakage of surface acoustic waves. An IDT is grown on top of the AlScN piezoelectric film, and an RF source transmits an electrical signal that is loaded on the IDT. The function of generating surface acoustic waves is achieved through the combined action of the IDT and the AlScN piezoelectric film. A covering protective layer is deposited and grown on top of the composite structure, and the thickness of the layer is less than that of the AlN waveguide, and is used to protect the AlScN piezoelectric film and prevent the intrusion of impurities and gases (such as O2, etc.) from affecting the quality of the AlScN piezoelectric film. Figure 2As shown in the figure, limiting the thickness of the AlScN film to less than 0.1μm can achieve the concentration of the light mode in the AlN waveguide. The light mode is transmitted in the composite waveguide structure formed by the AlN waveguide and the AlScN piezoelectric film, and the surface acoustic wave is transmitted to the composite waveguide structure. Through the coupling of the light field and the acoustic field, the light field is modulated, which has a huge development space in waveguide delay lines, microring modulators, Mach-Zehnder MZ modulators, and nanobeam resonant cavity modulators.

[0052] The present invention includes a silicon substrate, a silicon dioxide buried layer and a waveguide modulation region. The silicon dioxide buried layer is hollowed out or replaced by a Bragg reflection cavity to suppress the downward leakage of surface acoustic waves. The waveguide modulation region is located above the silicon dioxide buried layer or the Bragg reflection cavity layer, and plays the role of generating surface acoustic waves and limiting the transmission light field. At the same time, it can realize the role of acousto-optic modulation of the light field and modulate the phase of the light field mode. The waveguide modulation region specifically includes a composite structure, an interdigital transducer and a covering protective layer.

[0053] 2. Technical Principle

[0054] Reference Figure 1 , the radio frequency source sends out an electrical signal which is loaded on the interdigital electrodes of the IDT, and a surface acoustic wave is generated through the inverse piezoelectric effect of the AlScN piezoelectric film. The signal propagates along the surface of the AlScN film to the composite waveguide structure formed by the AlN waveguide and the AlScN piezoelectric film, thereby realizing the phase modulation of the optical mode in the composite waveguide structure. The surface acoustic wave is suppressed from leaking downward by hollowing out a cavity in the SiO2 buried layer or replacing the SiO2 buried layer with a Bragg reflection cavity. Among them, the Bragg reflection cavity is formed by alternating layer-by-layer stacking of high acoustic impedance materials (such as Ta2O5, HfO2, W, etc.) and low acoustic impedance materials (such as SiO2, etc.). The material of the layer in direct contact with the Si substrate and the AlScN film in the Bragg reflection cavity is SiO2, such as Figure 7 As shown, the Bragg reflection cavity is set to 7 layers. The thickness of the low acoustic impedance material is λ IDT ·v L-DBR / 4v p , the thickness of the high acoustic impedance material is λ IDT ·v H-DBR / 4v p , where λ IDT is the interdigital transducer period, v L-DBR and v H-DBR are the acoustic velocities in low acoustic impedance materials and high acoustic impedance materials, respectively, and v pis the acoustic velocity in the AlScN piezoelectric film. When the sound wave leaks downward and interacts with the periodic structure in the Bragg reflection cavity, the sound wave of a specific wavelength that meets the Bragg condition can be strongly reflected. The relevant parameters of the Bragg reflection cavity are designed according to the wavelength of the surface acoustic wave to achieve the effect of reflecting the surface acoustic wave back to the piezoelectric layer and inhibiting its downward leakage. As the core structure of the present invention, the composite waveguide structure deposited and grown on the insulator SiO2 achieves the following functions: 1) The AlScN film has piezoelectricity, and the piezoelectric coefficient d 33 1) The AlScN material is 3-5 times that of AlN and can generate higher intensity surface acoustic waves; 2) AlScN material is obtained by doping AlN material with Sc element, and has the characteristics of optical waveguide. It can form a composite waveguide structure with AlN waveguide to better confine the light mode in the optical waveguide structure; 3) AlScN and AlN have a high lattice matching degree, and will not generate internal stress at the contact between the two, affecting the device performance; 4) AlN and AlScN are both CMOS process compatible materials. By adopting the structure of AlN and AlScN stacked growth, it is easy to shrink the device size, reduce production costs, and is conducive to commercial applications.

[0055] 3. Specific applications

[0056] In terms of commercial applications, based on the high-speed acousto-optic modulator composite waveguide structure proposed in this embodiment, the acousto-optic modulator manufactured by changing the shape of the AlN waveguide has huge development space in the waveguide delay line, micro-ring modulator, Mach-Zehnder MZ modulator, nano-beam resonant cavity modulator and other acousto-optic modulators. Figure 8 As shown in the figure, it is a top view and a cross-sectional view of the waveguide delay line. The acousto-optic modulator can achieve the change of the optical mode phase. Fig.10 As shown in the figure, it is a top view and a cross-sectional view of the Mach-Zehnder MZ modulator. The acousto-optic modulator performs phase modulation through one of the waveguide arms of the MZ double-arm waveguide, which can realize the conversion of the "0" and "1" of the output optical signal, thereby changing the intensity of the output optical mode. Fig. 9 and 11 The figure shows the top view and cross-sectional view of the microring modulator and nanobeam resonant cavity modulator, respectively, which modulate the phase of the optical mode through the action of surface acoustic waves. Both are microcavity acousto-optic modulators. The AlN waveguide has a high optical quality factor and can achieve better acousto-optic overlapping effect. The nanobeam microcavity modulator has a more compact structure and is easy to integrate on-chip acousto-optics.

[0057] Embodiment 3: The composite waveguide structure proposed in this embodiment is the same as that in Embodiment 1 or 2. Figure 4 A specific example of the present invention using a silicon dioxide buried layer containing a cavity and a strip-type structure waveguide is given:

[0058] The composite waveguide structure provided in this embodiment includes a silicon substrate 1, a silicon dioxide buried layer 2 and a waveguide modulation region 3. The silicon dioxide buried layer 2 is hollowed out and contains a cavity 21, which is used to suppress the downward leakage of surface acoustic waves. The waveguide modulation region 3 includes a composite structure 31, a forked finger transducer 32 and a covering protective layer 33. The waveguide modulation region 3 is located above the silicon dioxide buried layer 2, and plays the role of generating surface acoustic waves and limiting the transmission light field. At the same time, it can realize the role of acousto-optic modulation of the light field and modulate the phase of the light field mode. The composite structure 31 is composed of a waveguide 313 and a piezoelectric layer 312. The waveguide 313 is located between the piezoelectric layer 312 and the covering protective layer 33 in the waveguide modulation region 3, and is in close contact with the piezoelectric layer 312 and the covering protective layer 33 respectively; the piezoelectric layer 312 is in close contact with the silicon dioxide buried layer 2. The covering protective layer 33 is located above the composite structure 31 and is in close contact with the composite structure 31. The IDT 32 is located at the upper right of the piezoelectric layer 312 and is in close contact with the piezoelectric layer 312 .

[0059] Embodiment 4: The composite waveguide structure proposed in this embodiment is the same as that in Embodiment 1 or 2. Figure 5 A specific example of the present invention using a silicon dioxide buried layer containing a cavity and a ridge structure waveguide is given:

[0060] Reference Figure 5 The composite waveguide structure provided in this embodiment includes a silicon substrate 1, a silicon dioxide buried layer 2 and a waveguide modulation region 3. The silicon dioxide buried layer 2 is hollowed out and contains a cavity 21, which is used to suppress the downward leakage of surface acoustic waves. The waveguide modulation region 3 includes a composite structure 31, a forked finger transducer 32 and a covering protective layer 33. The waveguide modulation region 3 is located above the silicon dioxide buried layer 2, and plays the role of generating surface acoustic waves and limiting the transmission light field. At the same time, it can realize the role of acousto-optic modulation of the light field and modulate the phase of the light field mode. The composite structure 31 is composed of a waveguide 314 and a piezoelectric layer 312, and the waveguide 314 is covered by a piezoelectric layer 315 and a covering protective layer 33, wherein the waveguide 314 is located below the piezoelectric layer 315, and the two are in close contact, and the piezoelectric layer 315 is located below the covering protective layer 33, and the two are in close contact. The forked finger transducer 32 is located at the upper right of the piezoelectric layer 312 and is in close contact with the piezoelectric layer 312.

[0061] Embodiment 5: The composite waveguide structure proposed in this embodiment is the same as that in Embodiment 1 or 2. Figure 6 and Figure 7 A specific example of the present invention using a waveguide containing a Bragg reflection cavity layer and a strip structure is given:

[0062] Reference Figure 6 and Figure 7The composite waveguide structure provided in this embodiment includes a silicon substrate 1, a Bragg reflection cavity layer 4 and a waveguide modulation region 3. The Bragg reflection cavity 4 is formed by alternating layer-by-layer stacking of a low acoustic impedance material 41 and a high acoustic impedance material 42. The Bragg reflection cavity 4 is mainly used to reflect the surface acoustic wave leaking downward back to the waveguide modulation region 3. The waveguide modulation region 3 includes a composite structure 31, an interdigital transducer 32 and a covering protective layer 33. The waveguide modulation region 3 is located above the Bragg reflection cavity 4, and plays a role in generating surface acoustic waves and limiting the transmission light field. At the same time, it can realize the role of acousto-optic modulation of the light field and modulate the phase of the light field mode. The composite structure 31 is composed of a waveguide 313 and a piezoelectric layer 312. The waveguide 313 is located between the piezoelectric layer 312 and the covering protective layer 33 in the waveguide modulation region 3, and is in close contact with the piezoelectric layer 312 and the covering protective layer 33 respectively; the piezoelectric layer 312 is in close contact with the silicon dioxide buried layer 2. The cover protection layer 33 is located above the composite structure 31 and is in close contact with the composite structure 31. The interdigital transducer 32 is located above and to the right of the piezoelectric layer 312 and is in close contact with the piezoelectric layer 312.

[0063] The present invention enhances the intensity of the generated surface acoustic waves by adopting a composite waveguide structure, thereby achieving good coupling between the acoustic field and the light field and improving the coupling efficiency. At the same time, the lattice structures of AlN and AlScN are similar, and the heterogeneous integration of the two has good lattice matching, and no internal stress is generated at the contact point between the two to affect the performance of the device. In addition, AlN and AlScN are both CMOS compatible materials, and the formed composite waveguide structure can be miniaturized, so that the acousto-optic modulator develops in the direction of miniaturization and commercialization, which is conducive to the realization of monolithic acousto-optic integration.

[0064] Embodiment 6: The method provided in this embodiment is used to prepare a high-speed acousto-optic modulated composite waveguide structure containing a silicon dioxide buried layer in a cavity region, such as Figure 1 As shown, the specific implementation steps are as follows:

[0065] Step 1. Pre-treat the silicon wafer to obtain a pre-treated Si substrate; in this embodiment, the pre-treatment operation is completed by removing impurities and dust on the surface of the silicon wafer through ultrasonic cleaning, rinsing with plasma water, and drying with a nitrogen gun.

[0066] Step 2. forming a SiO2 buried layer on the pretreated Si substrate by plasma enhanced chemical vapor deposition (PECVD) growth or thermal oxidation process;

[0067] Step 3: Grinding the portion deposited on the upper surface of the SiO2 buried layer by chemical mechanical polishing (CMP);

[0068] Step 4. Growing a c-axis preferentially oriented AlScN layer on the layer obtained in step S3 by magnetron sputtering;

[0069] Step 5. Continue to grow an AlN layer on the AlScN layer by magnetron sputtering, and coat the grown AlN layer with photoresist for photolithography, and then etch it by inductively coupled plasma-reactive ion etching ICP-RIE technology to obtain an AlN waveguide structure on the AlScN layer;

[0070] Step 6. Depositing a covering protective layer on the composite structure composed of AlScN and AlN by using an atomic layer deposition or magnetron sputtering process;

[0071] Step 7. Coating a photoresist on the substrate covered with the protective layer and performing photolithography, depositing metal electrodes by electron beam evaporation or magnetron sputtering, and performing metal patterning and stripping to obtain interdigitated electrodes;

[0072] Step 8. Continue to apply photoresist and perform photolithography, and cover the protective layer by inductively coupled plasma-reactive ion etching ICP-RIE technology or wet etching, so that the interdigital electrodes are exposed to the air;

[0073] Step 9. Continue to apply photoresist and perform photolithography, and etch the AlScN layer, the covering protective layer, and the silicon dioxide buried layer in sequence by inductively coupled plasma-reactive ion etching (ICP-RIE) technology to obtain a release groove structure;

[0074] Step 10. Place the structure obtained in steps S1-S9 in an HF acid solution or a buffered oxide etchant, and remove the silicon dioxide buried layer under the waveguide modulation region through the release groove structure, so that the waveguide modulation region is suspended;

[0075] Step 11. Complete the preparation process and obtain a high-speed acousto-optic modulation composite waveguide structure.

[0076] Embodiment 7: The method provided in this embodiment is used to prepare a high-speed acousto-optic modulated composite waveguide structure including a Bragg reflection cavity layer, such as Figure 6 As shown, the specific implementation steps are as follows:

[0077] Step a. Pre-treating the silicon wafer to obtain a pre-treated Si substrate;

[0078] Step b. On the pretreated Si substrate, a Bragg reflection cavity layer is obtained by alternately growing the Bragg reflection cavity layer layer by layer using plasma enhanced chemical vapor deposition (PECVD) and chemical vapor deposition (CVD);

[0079] Step c. growing an AlScN layer having a preferred c-axis orientation on the layer obtained in step S3 by magnetron sputtering;

[0080] Step d. Continue to grow an AlN layer on the AlScN layer by magnetron sputtering, and coat the grown AlN layer with a photoresist for photolithography, and then etch it using inductively coupled plasma - reactive ion etching ICP-RIE technology to obtain an AlN waveguide structure on top of the AlScN layer;

[0081] Step e. Depositing a covering protective layer on the composite structure composed of AlScN and AlN by atomic layer deposition or magnetron sputtering process;

[0082] Step f. coating a photoresist on the substrate covered with the protective layer and performing photolithography, depositing metal electrodes by electron beam evaporation or magnetron sputtering, and performing metal patterning and stripping to obtain interdigitated electrodes;

[0083] Step g. Continue to coat the photoresist for photolithography, and cover the protective layer by inductively coupled plasma - reactive ion etching ICP-RIE technology or wet etching, so that the interdigitated electrodes are exposed to the air;

[0084] Step h. Complete the preparation process to obtain a high-speed acousto-optic modulation composite waveguide structure.

[0085] The effect of the present invention is further described below in conjunction with simulation experiments.

[0086] 1. Simulation conditions:

[0087] The simulation of the present invention uses finite element software, and selects the electromagnetic wave and frequency domain (ewfd) physical field in the wave optics module to simulate the geometric structure (such as Figure 1 Modeling and simulation are performed as shown).

[0088] 2. Simulation content:

[0089] In this simulation, the thickness of the SiO2 layer is set to 2μm, the thickness of the AlScN layer is set to 0.1μm, and the thickness of the AlN strip waveguide is set to 0.7μm. The strip waveguide is set with a certain sidewall tilt angle, which is consistent with the actual etching process. By calling electromagnetic waves and frequency domain physical fields, the distribution of light modes in the structure is analyzed.

[0090] 3. Simulation results:

[0091] Reference Figure 3 The optical mode is mainly confined in the AlN strip waveguide, which means that after the composite waveguide is formed by AlN and AlScN, the optical mode is rarely distributed in AlScN, and the optical mode is only slightly affected by the crystal structure defects in AlScN, thus realizing the low-loss transmission of the optical mode in the composite waveguide.

[0092] It can be seen that the present invention can effectively prevent the surface acoustic wave from leaking into the silicon dioxide buried layer, limit the surface acoustic wave to the waveguide modulation area to the greatest extent, and generate stronger surface acoustic waves; at the same time, the piezoelectric layer can act as a waveguide to a certain extent, and better limit the light mode; in addition, it has the characteristics of low cost, low power consumption, high speed, and CMOS process compatibility, and can greatly improve the performance of aluminum nitride-based acousto-optic modulators.

[0093] The above simulation analysis proves the correctness and effectiveness of the method proposed in the present invention.

[0094] Parts of the present invention that are not described in detail belong to common knowledge among those skilled in the art.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Obviously, for professionals in this field, after understanding the content and principles of the present invention, they may make various modifications and changes in form and details without departing from the principles and structures of the present invention. However, these modifications and changes based on the ideas of the present invention are still within the scope of protection of the claims of the present invention.

Claims

1. A high-speed acousto-optic modulated composite waveguide structure, It is characterized in that It includes, from bottom to top, a silicon substrate (1), a silicon dioxide buried layer (2), and a waveguide modulation region (3); The silicon dioxide buried layer (2) is hollowed out to contain a cavity (21); The waveguide modulation region (3) comprises a composite structure (31), an interdigital transducer (32) and a covering protective layer (33); the composite structure (31) is composed of a waveguide (311) and a piezoelectric layer (312), wherein the waveguide (311) is made of an aluminum nitride thin film material, and the piezoelectric layer (312) is made of a doped aluminum nitride thin film material; The composite structure (31) is located above the silicon dioxide buried layer (2), and the composite structure (31) includes a waveguide (311) and a piezoelectric layer (312) in close contact; The interdigital transducer (32) is located on one side of the waveguide (311), and is located on the upper surface of the piezoelectric layer (312) and above the cavity (21); The covering protection layer (33) is located above the waveguide (311) and covers the upper surfaces of the waveguide (311) and the piezoelectric layer (312).

2. The structure according to claim 1, Features: The silicon dioxide buried layer (2) can be replaced by a Bragg reflection cavity layer (4) formed by alternately stacking a low acoustic impedance material (41) and a high acoustic impedance material (42) layer by layer, wherein the thickness of the low acoustic impedance material (41) is λ IDT· v L-DBR / 4v p , the thickness of the high acoustic impedance material (42) is λ IDT· v H-DBR / 4V P , where λ IDT is the period of the interdigital transducer (32), v L-DBR and v H-DBR are the acoustic velocities in the low acoustic impedance material (41) and the high acoustic impedance material (42), respectively, and v P is the acoustic velocity in the piezoelectric layer (312).

3. The structure according to claim 1, Features: The piezoelectric layer (312) is made of doped aluminum nitride material, wherein the doping element is scandium (Sc) or boron (B), and the doping element is doped into the aluminum nitride in a substitutional doping manner, with a doping ratio of 0 to 45%.

4. The structure according to claim 1, Features: The thickness of the waveguide (311) is greater than the thickness of the piezoelectric layer (312), wherein the thickness of the waveguide (311) is greater than 100 nm, and the thickness of the piezoelectric layer (312) is greater than 10 nm.

5. The structure according to claim 1, Features: The waveguide (311) is a strip-structure waveguide (313) or a ridge-structure waveguide (314).

6. The structure according to claim 5, Features: When the waveguide (311) is a strip-structured waveguide (313), it is located between the piezoelectric layer (312) and the covering protective layer (33) in the waveguide modulation region (3), and is in close contact with the piezoelectric layer (312) and the covering protective layer (33), respectively.

7. The structure according to claim 5, Features: When the waveguide (311) is a ridge structure waveguide (314), it is covered by a piezoelectric layer (315) and a covering protective layer (33), and the waveguide is located below the piezoelectric layer (315) and in close contact with the piezoelectric layer (315); the piezoelectric layer (315) is located below the covering protective layer (33) and in close contact with the covering protective layer (33).

8. The structure according to claim 1, Features: The optical refractive index of the covering protective layer (33) is less than the optical refractive index of the waveguide (311), and the thickness of the covering protective layer (33) is less than the thickness of the waveguide (311); the material selected for the covering protective layer (33) includes Si 3 N 4 、TiN、Al 2 O 3 and SiO 2 .

9. A method for preparing the structure according to claim 2, It is characterized in that The steps include: S1. Pre-treating the silicon wafer to obtain a pre-treated Si substrate; S2. Form SiO on the pretreated Si substrate by plasma enhanced chemical vapor deposition (PECVD) or thermal oxidation process 2 buried layer; S3. Deposition on SiO 2 The upper surface of the buried layer is polished by chemical mechanical polishing (CMP). S4. Growing a c-axis preferentially oriented AlScN layer on the layer obtained in step S3 by magnetron sputtering; S5. Continue to grow an AlN layer on the AlScN layer by magnetron sputtering, and coat the grown AlN layer with a photoresist for photolithography, and then etch it by inductively coupled plasma-reactive ion etching ICP-RIE technology to obtain an AlN waveguide structure on the top of the AlScN layer; S6. Depositing a covering protective layer on the composite structure composed of AlScN and AlN by atomic layer deposition or magnetron sputtering process; S7. coating a photoresist on the substrate covered with the protective layer and performing photolithography, depositing a metal electrode by electron beam evaporation or magnetron sputtering, and performing metal patterning and stripping to obtain an interdigitated electrode; S8. Continue to apply photoresist and perform photolithography, and cover the protective layer by inductively coupled plasma-reactive ion etching ICP-RIE technology or wet etching, so that the interdigital electrodes are exposed to the air; S9. Continue to apply photoresist and perform photolithography, and sequentially etch the AlScN layer covering the protective layer until the silicon dioxide buried layer by inductively coupled plasma-reactive ion etching ICP-RIE technology to obtain a release groove structure; S10. placing the structure obtained in steps S1-S9 in an HF acid solution or a buffered oxide etchant, and removing the silicon dioxide buried layer under the waveguide modulation region through the release groove structure, thereby making the waveguide modulation region suspended; S11. Complete the preparation process and obtain a high-speed acousto-optic modulation composite waveguide structure.

10. The method according to claim 9, It is characterized in that The high-speed acousto-optic modulation composite waveguide structure after replacing the silicon dioxide buried layer (2) with the Bragg reflection cavity layer (4) is prepared by the following operation: the SiO2 is formed by plasma enhanced chemical vapor deposition (PECVD) growth or thermal oxidation process as described in step S2. 2 The buried layer is replaced by a Bragg reflection cavity layer obtained by alternating growth of plasma enhanced chemical vapor deposition (PECVD) and chemical vapor deposition (CVD) layer by layer; at the same time, steps S3, S9 and S10 are not performed, and the other preparation steps remain unchanged.

Citation Information

Cited By

  • Aluminum nitride waveguide structure based on nitride layered coating and preparation method thereof

    CN119960109A