Hydrophilic catalyst layer for fuel cell and preparation method of hydrophilic catalyst layer
Modifying the catalytic layer through plasma treatment technology solves the problem of large mass transfer resistance under low-humidity conditions caused by the hydrophobicity of the surface of the fuel cell catalytic layer, achieving better water management capabilities and improved performance.
Patent Information
- Application Number
- CN202410749621.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
The surface of the existing fuel cell catalytic layer is hydrophobic, which results in high mass transfer resistance under low-humidity conditions and reduces the adaptability and performance of the membrane electrode.
Plasma treatment technology is used to modify the surface of the catalytic layer. Through the combination of ultrasonic waves and plasma, functional groups are introduced and surface etching is performed to change the surface properties of the catalytic layer, making it hydrophilic and reducing mass transfer and drainage resistance.
It improves the performance of membrane electrodes under low-humidity conditions, enhances proton transport capabilities, reduces ohmic polarization and mass transfer polarization, and improves the overall performance of the fuel cell.
Smart Images

Figure CN118782808A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a hydrophilic catalyst layer for a fuel cell and a preparation method thereof. Background Art
[0002] A fuel cell is an electrochemical energy converter that converts the chemical energy in the fuel directly into direct current. The working principle is that hydrogen is catalytically oxidized on the anode side to form H + After that, it reacts with the oxygen on the cathode side to generate water through catalytic reaction. Due to its environmentally friendly, zero-emission, high efficiency, no noise and light weight, it has been widely developed and applied in the fields of automobiles, forklifts, buses, etc.
[0003] The catalyst layer is the core component of the fuel cell. The electrochemical reaction for energy conversion occurs on the surface of the catalyst layer. Therefore, the catalyst layer must not only have enough catalytic active sites, but also have a sufficiently small mass transfer resistance, and water transport in the catalyst layer has a crucial impact on the mass transfer resistance. Good water management capabilities require that the proton membrane be well hydrated at low current density in the fuel cell to enhance the proton transfer capacity; and promote drainage at high current density to prevent the battery from flooding.
[0004] The surfaces of current fuel cell catalyst layers are relatively hydrophobic and sensitive to humidity changes, especially under low humidity conditions where the mass transfer resistance is very large. This greatly hinders the performance of the membrane electrode and reduces the adaptability of the membrane electrode to low humidity conditions. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a hydrophilic catalyst layer for a fuel cell and a preparation method thereof. The purpose of the present invention is to propose a method for changing the hydrophilicity and hydrophobicity of the catalyst layer surface for a fuel cell catalyst layer, which can not only enhance the performance of the membrane electrode under low humidity conditions, but also has simple operation and low cost.
[0006] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:
[0007] In a first aspect, an embodiment of the present invention provides a method for preparing a hydrophilic catalyst layer for a fuel cell, comprising the following steps:
[0008] Step S1, sequentially mixing a platinum-based catalyst, ultrapure water, an organic alcohol and a perfluorosulfonic acid ionomer solution, and placing the mixture in an ultrasonic generator for ultrasonic treatment to obtain a uniformly dispersed catalyst slurry;
[0009] Step S2, coating the catalyst slurry obtained in step S1, and drying for 2-3 minutes to obtain a catalyst layer with a hydrophobic surface;
[0010] Step S3, subjecting the catalyst layer obtained in step S2 to plasma surface modification treatment, wherein the contact angle of the catalyst layer after the treatment is between 10° and 80°.
[0011] Further, in step S1, the solid content of the catalyst slurry is 1-30%, the I / C is 0.8-1.1 by mass ratio, and the water-to-alcohol ratio is 3-6:1;
[0012] The power of the ultrasonic generator is 10-10000W, and the ultrasonic treatment time is 10-300min.
[0013] Furthermore, in step S2, the catalyst slurry is coated on the PTFE substrate or the PEM or the GDL material, and the coating method includes one of wire rod coating, ultrasonic spray coating and slit coating.
[0014] Further, in step S3, the power of the plasma emission device is 1-1000W, and the plasma treatment time is 1-600min;
[0015] The process gas introduced during plasma treatment includes one or more of oxygen, nitrogen, argon, air, argon-hydrogen mixed gas and CF4.
[0016] Furthermore, the catalyst is a platinum-based catalyst or a non-platinum-based catalyst, wherein the platinum-based catalyst includes Pt / C, PtCo / C, PtNi / C and PtCoMn / C, and the non-platinum-based catalyst includes FeN / C and Pd / C.
[0017] In a second aspect, an embodiment of the present invention provides a hydrophilic catalyst layer for a fuel cell, which is made by the preparation method described in the first aspect.
[0018] The technical solution provided by the embodiment of the present invention has the following beneficial effects:
[0019] Plasma is a collection of neutral particles, ions and electrons. Plasma treatment is to first apply an electric field to the process gas (air, nitrogen, argon, oxygen, etc.) to ionize it into plasma, and then use the properties of these active components to carry out oxidation, reduction, cracking, cross-linking and other reactions to change the surface properties of the sample and optimize the surface performance of the material.
[0020] The present invention uses plasma to bombard the surface of the catalyst layer under vacuum conditions, so that the chemical bonds of the molecules on the surface of the catalyst layer are opened and combined with free radicals in the plasma. Depending on the process gas, specific functional groups (-COOH, CO, -OH, NH2-) are added to the surface of the catalyst layer. The introduction of functional groups, especially oxygen-containing functional groups, plays a significant role in improving the surface energy and wettability of the material. And during the plasma treatment process, a certain degree of plasma etching will occur, that is, the plasma reacts with the carbon on the surface of the catalyst layer to generate volatile gases for removal. Because the plasma treatment only reacts physically and chemically with the surface layer of the material, and the action depth is tens to hundreds of nanometers in the surface layer, the etching that occurs will not affect the inherent properties of the material, but some of the pores it produces increase the catalytic active sites at the three-phase interface while reducing the gas transmission and drainage resistance, which can effectively improve the performance of PEMFC. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The actual pictures of the contact angles of the catalytic layers of Example 1, Comparative Example 1 and Comparative Example 4 are shown.
[0022] Figure 2 The battery performance diagram is obtained by using the catalytic layers of Example 1, Comparative Example 1 and Comparative Example 4. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0024] Example 1
[0025] A method for preparing a hydrophilic catalyst layer for a fuel cell comprises the following steps:
[0026] Step S1, mixing a TKK-Pt / C catalyst (Pt content 50%), ultrapure water, n-propanol and Nafion D520 perfluorosulfonic acid resin solution to form a catalyst mixture with a solid content of 5%, wherein the water-to-alcohol ratio is 4:1 by mass ratio, and I / C=1; wherein I represents the mass of the solute in the ionomer Nafion D520 perfluorosulfonic acid resin solution, and C represents the mass of the carbon carrier in the catalyst;
[0027] Step S2, dispersing the catalyst mixture with an ultrasonic cell crusher, with an ultrasonic power of 100 W and an ultrasonic time of 40 minutes, and using cooling water to control the ultrasonic temperature at 10° C. during the ultrasonic treatment to obtain a catalyst slurry;
[0028] Step S3, coating the catalyst slurry, and drying on a heating platform at 60° C. for 2 minutes to obtain an original catalyst layer;
[0029] Step S4, placing the prepared catalyst layer into a plasma treatment chamber, connecting the air cylinder, processing power of 500 W, and processing time of 3 min.
[0030] Example 2
[0031] A method for preparing a hydrophilic catalyst layer for a fuel cell comprises the following steps:
[0032] Step S1, mixing a TKK-PtCo / C catalyst (Pt and Co contents of 47% and 5%), ultrapure water, isopropanol and Nafion D2020 perfluorosulfonic acid resin solution to form a catalyst mixture with a solid content of 6%, wherein the water-to-alcohol ratio is 4:1 by mass ratio, and I / C=1; wherein I represents the mass of the solute in the ionomer Nafion D2020 perfluorosulfonic acid resin solution, and C represents the mass of the carbon carrier in the catalyst;
[0033] Step S2, dispersing the catalyst mixture with an ultrasonic cell crusher, with an ultrasonic power of 200 W and an ultrasonic time of 30 minutes, and using cooling water to control the ultrasonic temperature at 10° C. during the ultrasonic treatment to obtain a catalyst slurry;
[0034] Step S3, coating the catalyst slurry, and drying on a heating platform at 60° C. for 2 minutes to obtain an original catalyst layer;
[0035] Step S4, placing the prepared catalyst layer into a plasma treatment chamber, connecting the N2 bottle, processing power of 300 W, and processing time of 10 min.
[0036] Example 3
[0037] A method for preparing a hydrophilic catalyst layer for a fuel cell comprises the following steps:
[0038] Step S1, mixing a TKK-PtCoMn / C catalyst (Pt, Co, Mn contents of 47%, 3.6%, 1.2%), ultrapure water, n-butanol and Aquivion D79 perfluorosulfonic acid resin solution to form a catalyst mixture with a solid content of 5%, wherein the water-to-alcohol ratio is 4:1 by mass ratio, and I / C=1; wherein I represents the mass of the solute in the ionomer Aquivion D79 perfluorosulfonic acid resin solution, and C represents the mass of the carbon carrier in the catalyst;
[0039] Step S2, dispersing the catalyst mixture with an ultrasonic cell crusher, with an ultrasonic power of 300 W, using cooling water to control the ultrasonic temperature to 10° C. during the ultrasonic treatment, and the ultrasonic time for 10 minutes;
[0040] Step S3, coating the catalyst slurry, and drying on a heating platform at 60° C. for 2 minutes to obtain an original catalyst layer;
[0041] Step S4, placing the prepared catalyst layer into a plasma treatment chamber, connecting an Ar bottle, treating with a power of 50 W and a treatment time of 20 min.
[0042] Example 4
[0043] A method for preparing a hydrophilic catalyst layer for a fuel cell comprises the following steps:
[0044] Step S1, mixing a homemade PtNi / C catalyst (Pt, Ni content of 47%, 5%), ultrapure water, glycerol and Solvay D72 solution to form a catalyst mixture with a solid content of 10%, wherein the water-to-alcohol ratio is 4:1 by mass ratio, and I / C=1; wherein I represents the mass of the solute in the ionomer Solvay D72 solution, and C represents the mass of the carbon carrier in the catalyst;
[0045] Step S2, dispersing the catalyst mixture with an ultrasonic cell crusher, with an ultrasonic power of 300 W, using cooling water to control the ultrasonic temperature to 10° C. during the ultrasonic treatment, and the ultrasonic time of 50 minutes;
[0046] Step S3, coating the catalyst slurry, and drying on a heating platform at 60° C. for 2 minutes to obtain an original catalyst layer;
[0047] Step S4, placing the prepared catalyst layer into the plasma treatment chamber, connecting the O2 bottle, processing power of 100 W, and processing time of 30 min.
[0048] Comparative Examples 1-3
[0049] Except that the fourth step does not include plasma treatment, the remaining steps are the same as those of the corresponding embodiments 1-3.
[0050] Comparative Example 4
[0051] The first three steps are the same as those in Example 4. The fourth step is to subject the prepared catalyst layer to high-temperature treatment at a temperature of 150° C. for 2 h.
[0052] The contact angle of the catalyst layer surface prepared by Examples 1-4 and Comparative Examples 1-4 is characterized. It can be clearly seen from the contact angle diagram in the attached figure that, compared with Comparative Example 1 which does not use plasma treatment and Comparative Example 4 which uses high temperature treatment, in Example 1 using the treatment method of the present invention, water droplets are better adsorbed and spread on the catalyst layer surface, that is, they have a smaller contact angle; the catalyst layer in Comparative Example 1 is highly hydrophobic, and the contact angle is also the largest; the contact angle of water droplets on the catalyst layer surface in Comparative Example 4 is slightly reduced compared to the untreated catalyst layer. The specific values of the contact angle are shown in Table 1.
[0053] Table 1 Contact angle values of the catalyst layer surface of Examples 1-4 and Comparative Examples 1-4
[0054]
[0055] The smaller contact angle indicates that the surface properties of the catalyst layer have changed. After the oxygen in the air is bombarded by accelerated electrons into oxygen ions and free radicals, it collides with the molecular chains on the surface of the catalyst layer to convert and recombine charges, forming a hydrophilic surface of active groups, thereby achieving the purpose of surface activation. The nitrogen in the air is bombarded by electrons into positively charged nitrogen ions, and the positive nitrogen ions will be attracted to the negative electrode plate. Since nitrogen particles are relatively heavy, they can bombard the surface of the sample with great force to form a rough surface. Argon uses ions in the plasma for pure physical bombardment, which forms a rough surface without producing oxides. As can be seen from Table 1, under the same catalyst layer, compared with the method of not being treated and using high-temperature treatment, the method of using plasma to treat the catalyst layer proposed in the present invention can effectively change the surface properties of the catalyst layer, and the size of the contact angle can be regulated by changing the process gas and the power and time of the treatment.
[0056] The ion-treated catalyst layer and PEM membrane were hot-pressed and transferred to prepare a membrane electrode (MEA) and assembled into a single cell for battery performance testing. The test conditions were: battery temperature 75°C, H2 was passed into the anode and humidified, relative humidity 40%, and the anode flow rate was 0.5L / min. The cathode was passed through humidified O2, relative humidity 40%, and the cathode flow rate was 1.5L / min. The cell performance was as shown in the attached Figure 2 In the battery performance diagram, under the same humidity conditions, compared with Example 1, Comparative Example 1 and Comparative Example 4, Example 1 has a very high power density in the entire current density range, wherein the ohmic polarization and mass transfer polarization are both relatively low, which is also a reflection of the hydrophilicity of the catalyst layer making the proton membrane wet.
[0057] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a hydrophilic catalyst layer for a fuel cell, characterized in that: The following steps are involved: Step S1, sequentially mixing a platinum-based catalyst, ultrapure water, an organic alcohol and a perfluorosulfonic acid ionomer solution, and placing the mixture in an ultrasonic generator for ultrasonic treatment to obtain a uniformly dispersed catalyst slurry; Step S2, coating the catalyst slurry obtained in step S1, and drying for 2-3 minutes to obtain a catalyst layer with a hydrophobic surface; Step S3, subjecting the catalyst layer obtained in step S2 to plasma surface modification treatment, wherein the contact angle of the catalyst layer after the treatment is between 10° and 80°.
2. The method for preparing a hydrophilic catalyst layer for a fuel cell according to claim 1, characterized in that: In step S1, the solid content of the catalyst slurry is 1-30%, the I / C is 0.8-1.1 by mass ratio, and the water-to-alcohol ratio is 3-6:1; The power of the ultrasonic generator is 10-10000W, and the ultrasonic treatment time is 10-300min.
3. The method for preparing a hydrophilic catalyst layer for a fuel cell according to claim 1, characterized in that: In step S2, the catalyst slurry is coated on a PTFE substrate or a PEM or a GDL material; The coating method includes one of wire rod coating, ultrasonic spray coating and slot coating.
4. The method for preparing a hydrophilic catalyst layer for a fuel cell according to claim 1, characterized in that: In step S3, the power of the plasma emission device is 1-1000W, and the plasma treatment time is 1-600min; The process gas introduced during plasma treatment includes one or more of oxygen, nitrogen, argon, air, argon-hydrogen mixed gas and CF4.
5. The method for preparing a hydrophilic catalyst layer for a fuel cell according to claim 1, characterized in that: The catalyst is a platinum-based catalyst or a non-platinum-based catalyst, wherein the platinum-based catalyst includes Pt / C, PtCo / C, PtNi / C and PtCoMn / C, and the non-platinum-based catalyst includes FeN / C and Pd / C.
6. A hydrophilic catalyst layer for a fuel cell, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 5.