A-site co-doped alkaline earth metal and lanthanide perovskite oxygen electrode material and preparation method thereof
The perovskite oxygen electrode material co-doped with alkaline earth metals and lanthanide elements in the A-site solves the problem of mismatch in thermal expansion coefficient between the oxygen electrode and the electrolyte in solid oxide batteries, achieving excellent oxygen exchange capacity and high catalytic activity. Ensures battery stability and performance.
Patent Information
- Application Number
- CN202410768757.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The thermal expansion coefficient of the oxygen electrode material and the electrolyte material in the solid oxide battery does not match, causing thermal stress to degrade battery performance during temperature rise and fall tests. Lowering the operating temperature will lead to a decrease in oxygen reduction reaction activity, affecting battery stability and life.
A perovskite oxygen electrode material co-doped with alkaline earth metals and lanthanide elements in the A-site is used. The structural formula is Bi0.8-xLnxCa0.2FeO3-δ. It is prepared by a citric acid combustion method at a low sintering temperature to control the oxygen vacancies and reactions of the material. Activity, improve conductivity and catalytic activity.
Excellent oxygen exchange capacity and high catalytic activity are obtained, with good electrochemical performance and stability, matching the thermal expansion coefficient of the electrolyte, extending battery life and improving stability.
Smart Images

Figure CN118782810A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solid oxide batteries, and in particular to a perovskite oxygen electrode material co-doped with alkaline earth metals and lanthanide elements at the A position and a preparation method thereof. Background Art
[0002] Solid oxide cells (SOC) have attracted attention as a highly efficient energy conversion device. On the one hand, they operate in solid oxide fuel cell mode (SOFCs), using clean energy such as H2 to generate electricity for power generation; on the other hand, they operate in solid oxide electrolysis cell mode (SOECs), converting H2O or CO2 into fuel gases such as H2 or CO for energy storage.
[0003] At present, solid oxide batteries face some problems that hinder their commercial development. For example, the thermal expansion coefficient of oxygen electrode materials does not match that of commonly used electrolyte materials. During the temperature rise and fall test, they will gradually peel off from the electrolyte surface due to the presence of thermal stress, resulting in a decrease in the electrochemical performance and stability of the battery. Although the reaction between battery components can be slowed down by lowering the operating temperature and stabilizing the microstructure of the oxygen electrode and the electrolyte, thereby extending the battery life, as the operating temperature decreases, the oxygen reduction reaction (ORR) activity of the oxygen electrode decreases significantly, and the performance also decreases accordingly. Therefore, it is crucial to develop oxygen electrode materials with excellent performance. Summary of the invention
[0004] The purpose of the present invention is to provide a perovskite oxygen electrode material co-doped with alkaline earth metals and lanthanide elements at the A position and a preparation method thereof. The method has a low sintering temperature and a simple preparation process. The prepared oxygen electrode material can obtain excellent oxygen exchange capacity and high catalytic activity, and also has good electrochemical properties and good stability, and can be used as an oxygen electrode material for solid oxide batteries.
[0005] To achieve the above object, the present invention provides a perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position, wherein the structural formula of the oxygen electrode material is Bi 0.8-x Ln x Ca 0.2 FeO 3-δ , where 0<x≤0.1, δ is the content of oxygen vacancies, and Ln is selected from one of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, and Yb.
[0006] To achieve the above object, the present invention also provides a method for preparing a perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide elements at the A position, comprising the following steps:
[0007] (1) Using metal nitrates of Bi, Ln, Ca, and Fe as the initial raw materials, according to the structural formula Bi 0.8-x Ln x Ca 0.2 FeO 3-δ Weigh each raw material according to the stoichiometric ratio of the corresponding elements, where 0<x≤0.1, δ is the content of oxygen vacancies, and Ln is selected from one of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, and Yb; then weigh an appropriate amount of citric acid;
[0008] (2) Pour various raw metal nitrates into a container, add deionized water, stir at 60-100° C. until the solution becomes clear, then add citric acid and ammonia water in sequence to adjust the pH value of the solution to 6-8, and stir until the water evaporates to form a gel;
[0009] (3) placing the gel obtained in step (2) in a high-temperature drying oven and drying until the gel becomes dry to obtain a precursor;
[0010] (4) Grinding the precursor obtained in step (3), placing it in a high-temperature muffle furnace, and calcining it in an air atmosphere to obtain an oxygen electrode material.
[0011] Preferably, in step (1), the metal nitrates of Bi, Ln, Ca and Fe are Bi(NO3)3·5H2O, Ln(NO3)3·6H2O, Ca(NO3)2·4H2O and Fe(NO3)3·9H2O respectively.
[0012] Preferably, in step (1), citric acid is weighed so that the molar ratio between metal ions and citric acid is 1:1.5.
[0013] Preferably, in step (2), the pH value of the solution is adjusted to 6 and the stirring temperature is 80°C.
[0014] Preferably, in step (3), the temperature of the high temperature drying oven is 150-300° C., and the drying time is 5-12 hours.
[0015] Preferably, in step (4), the calcination temperature is 800-1000° C. and the calcination time is 5-10 hours.
[0016] The present invention can improve the oxygen vacancy concentration and reaction activity of the perovskite oxygen electrode material by co-doping alkaline earth metal and lanthanide elements at the A position of the base material BiFeO3; doping with alkaline earth metal Ca element can improve the conductivity of the perovskite material and improve the oxygen exchange performance; in addition, doping with lanthanide elements is conducive to enhancing the catalytic activity of the oxygen electrode material. The present invention adopts the citrate combustion method for preparation, with low sintering temperature and simple preparation process, and uses co-doping to regulate the key properties of the material (thermal expansion coefficient, polarization impedance, etc.). The prepared oxygen electrode material has excellent oxygen exchange capacity and high catalytic activity, and also has good electrochemical performance and good stability, and can be used as an oxygen electrode material for solid oxide batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the XRD pattern of the oxygen electrode material prepared in Example 1;
[0018] Figure 2 is the XRD pattern of the oxygen electrode material prepared in Example 2;
[0019] Figure 3 is a SEM image of the oxygen electrode material prepared in Example 2;
[0020] Figure 4 is a schematic diagram of the relationship between the thermal expansion coefficient and temperature of a dense sample strip prepared from the oxygen electrode material prepared in Example 2;
[0021] Figure 5 It is a schematic diagram of the impedance curve of the oxygen electrode material prepared in Example 2. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0023] Embodiment 1
[0024] A perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position, wherein the structural formula of the oxygen electrode material is Bi 0.7 La 0.1 Ca 0.2 FeO 3-δ , where δ is the content of oxygen vacancies.
[0025] The method for preparing the above oxygen electrode material comprises the following steps:
[0026] (1) According to the structural formula Bi 0.7 La 0.1 Ca 0.2 FeO 3-δ33.9549 g of Bi(NO3)3·5H2O, 4.3301 g of La(NO3)3·6H2O, 4.723 g of Ca(NO3)2·4H2O, and 40.3997 g of Fe(NO3)3·9H2O were weighed in the stoichiometric ratio of the corresponding elements of 0.7:0.1:0.2:1, where δ is the content of oxygen vacancies; then 63.042 g of citric acid was weighed in the molar ratio of metal ions to citric acid of 1:1.5;
[0027] (2) Pour various raw metal nitrates into a beaker, add 200 mL of deionized water, place the mixed solution on a magnetic stirrer, stir at 80° C. until the solution becomes clear, then add citric acid and ammonia water in sequence to adjust the pH value of the solution to 6, and keep the solution stirred at 80° C. until the water evaporates and a gel is formed;
[0028] (3) placing the gel obtained in step (2) in a high temperature drying oven and drying at 200° C. for 10 h until the gel becomes dry to obtain a precursor;
[0029] (4) The precursor obtained in step (3) was ground and placed in a high-temperature muffle furnace, and calcined at 900° C. for 5 h in an air atmosphere to obtain Bi 0.7 La 0.1 Ca 0.2 FeO 3-δ Oxygen electrode material, the XRD spectrum of the prepared oxygen electrode powder is as follows Figure 1 As shown. Figure 1 It can be seen that the prepared material does not have any impurities, confirming that the prepared material is a pure phase perovskite oxygen electrode material.
[0030] Embodiment 2
[0031] A perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position, wherein the structural formula of the oxygen electrode material is Bi 0.7 Pr 0.1 Ca 0.2 FeO 3-δ , where δ is the content of oxygen vacancies.
[0032] The method for preparing the above oxygen electrode material comprises the following steps:
[0033] (1) According to the structural formula Bi 0.7 La 0.1 Ca 0.2 FeO 3-δ33.9549 g of Bi(NO3)3·5H2O, 4.3501 g of Pr(NO3)3·6H2O, 4.723 g of Ca(NO3)2·4H2O, and 40.3997 g of Fe(NO3)3·9H2O were weighed in the stoichiometric ratio of the corresponding elements of 0.7:0.1:0.2:1, where δ is the content of oxygen vacancies; then 63.042 g of citric acid was weighed in the molar ratio of metal ions to citric acid of 1:1.5;
[0034] (2) Pour various raw metal nitrates into a beaker, add 200 mL of deionized water, place the mixed solution on a magnetic stirrer, stir at 80° C. until the solution becomes clear, then add citric acid and ammonia water in sequence to adjust the pH value of the solution to 7, and keep the solution stirred at 80° C. until the water evaporates and a gel is formed;
[0035] (3) placing the gel obtained in step (2) in a high temperature drying oven and drying at 250° C. for 12 h until the gel becomes dry to obtain a precursor;
[0036] (4) The precursor obtained in step (3) was ground and placed in a high-temperature muffle furnace, and calcined at 900° C. for 5 h in an air atmosphere to obtain Bi 0.7 Pr 0.1 Ca 0.2 FeO 3-δ Oxygen electrode material, XRD spectrum and SEM image of the prepared oxygen electrode powder are shown as follows Figure 2 and Figure 3 As shown. Figure 2 It can be seen that the prepared material does not have any impurities, confirming that the prepared material is a pure phase perovskite oxygen electrode material. Figure 3 It can be seen that the oxygen electrode material grains are closely arranged and the grain size is uniform.
[0037] Weigh 2g of Bi prepared in Example 2 0.7 Pr 0.1 Ca 0.2 FeO 3-δ The oxygen electrode material was placed in a stripping mold and maintained at a pressure of 300 MPa for 5 minutes to form a rectangular sample strip, which was then placed in a muffle furnace and calcined at 950°C for 5 hours to obtain a dense sample strip (with a specification of approximately 0.44 cm × 0.5 cm × 1.9 cm). The prepared dense sample strip was placed in a thermal expansion instrument to test the thermal expansion coefficient at a test temperature of 30-900°C. The test results are shown in FIG. Figure 4 As shown. Figure 4 It can be seen that the thermal expansion coefficient is 16.7638×10 -6 K -1 , which is lower than the thermal expansion coefficient of commonly used Co-based materials by 20×10-6 K -1 The low thermal expansion coefficient of the oxygen electrode material prepared in this embodiment matches the thermal expansion coefficient of common electrolyte materials. The oxygen electrode material with a low thermal expansion coefficient can ensure that the battery will not fall off from the electrolyte during the test, thereby ensuring the stability of the battery during the test.
[0038] In order to characterize the catalytic performance of oxygen electrode material samples, a symmetrical cell method was used to measure the Bi 0.7 Pr 0.1 Ca 0.2 FeO 3-δ The polarization impedance (ASR) of Bi 0.7 Pr 0.1 Ca 0.2 FeO 3-δ The sample was placed in air atmosphere and tested for ASR at 700-800°C, and the impedance curve fitted by EIS was obtained, as shown in Figure 5 As shown. Figure 5 It can be seen that Bi 0.7 Pr 0.1 Ca 0.2 FeO 3-δ The ASR of the oxygen electrode sample shows a gradually decreasing trend with increasing temperature. Oxygen electrode materials with low polarization impedance are an effective way to improve the electrochemical performance and long-term stability of the battery. This shows that the oxygen electrode material prepared in this example has good electrochemical performance and good stability.
Claims
1. A perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at the A position, characterized in that: The structural formula of the oxygen electrode material is Bi 0.8-x Ln x Ca 0.2 FeO 3-δ , where 0<x≤0.1, δ is the content of oxygen vacancies, and Ln is selected from one of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, and Yb.
2. The method for preparing a perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position according to claim 1, characterized in that: The following steps are involved: (1) Using metal nitrates of Bi, Ln, Ca, and Fe as the initial raw materials, according to the structural formula Bi 0.8-x Ln x Ca 0.2 FeO 3-δ Weigh each raw material according to the stoichiometric ratio of the corresponding elements, where 0<x≤0.1, δ is the content of oxygen vacancies, and Ln is selected from one of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, and Yb; then weigh an appropriate amount of citric acid; (2) Pour various raw metal nitrates into a container, add deionized water, stir at 60-100° C. until the solution becomes clear, then add citric acid and ammonia water in sequence to adjust the pH value of the solution to 6-8, and stir until the water evaporates to form a gel; (3) placing the gel obtained in step (2) in a high-temperature drying oven and drying until the gel becomes dry to obtain a precursor; (4) Grinding the precursor obtained in step (3), placing it in a high-temperature muffle furnace, and calcining it in an air atmosphere to obtain an oxygen electrode material.
3. The method for preparing a perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position according to claim 2, characterized in that: In step (1), the metal nitrates of Bi, Ln, Ca and Fe are Bi(NO3)3·5H2O, Ln(NO3)3·6H2O, Ca(NO3)2·4H2O and Fe(NO3)3·9H2O respectively.
4. The method for preparing a perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position according to claim 2 or 3, characterized in that: In step (1), citric acid is weighed according to a molar ratio of metal ions to citric acid of 1:1.
5.
5. The method for preparing a perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position according to claim 2 or 3, characterized in that: In step (2), the pH value of the solution is adjusted to 6 and the stirring temperature is 80°C.
6. The method for preparing a perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position according to claim 2 or 3, characterized in that: In step (3), the temperature of the high temperature drying oven is 150-300° C., and the drying time is 5-12 hours.
7. The method for preparing a perovskite oxygen electrode material co-doped with alkaline earth metal and lanthanide element at A position according to claim 2 or 3, characterized in that: In step (4), the calcination temperature is 800-1000° C. and the calcination time is 5-10 hours.
Citation Information
Patent Citations
Rare-earth element-doped BaFeO3-delta-based ABO3 type perovskite fuel cell cathode material and application thereof
CN102208662A
Fuel cell / electrolytic tank oxygen electrode material, preparation method and application thereof
CN115810763A
Solid oxide cell
JP2009152014A
Cited By
Bismuth ferrite-based energy storage ceramic with high entropy design as well as preparation method and application of bismuth ferrite-based energy storage ceramic
CN119613099A