Composite electrolyte, preparation method thereof and all-solid-state lithium ion battery
By using a composite electrolyte in which a lithium-conducting mixture coats a sulfide electrolyte in an all-solid-state lithium-ion battery, the problem of insufficient charge and discharge efficiency and negative electrode stability in the first cycle of the battery is solved, and the battery performance and adaptability to mass production are improved.
Patent Information
- Application Number
- CN202410719556.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-15
AI Technical Summary
There is room for improvement in the first-cycle charge and discharge efficiency and negative electrode stability of all-solid-state lithium-ion batteries, and the volume change of high-nickel cathode materials during cycling causes material powdering. Increasing test pressure will promote the growth of lithium dendrites and oxide/halogenation The ionic conductivity of the material interlayer is insufficient, which affects battery performance.
A composite electrolyte containing a lithium-conducting mixture coating a sulfide electrolyte is used. By controlling the mass ratio of the plastic crystal to the lithium salt and the mass ratio of the sulfide electrolyte to the lithium-conducting mixture, the lithium ion conductivity and mass transfer efficiency are improved, and the capacity of the positive electrode is reduced. losses, and reduce intolerant reduction side reactions on the negative electrode side.
It improves the first-cycle discharge capacity of the all-solid-state lithium-ion battery and the first efficiency of the positive electrode, enhances the rate performance of the negative electrode, and maintains structural stability at high temperatures, making it suitable for mass production.
Smart Images

Figure CN118782884A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a composite electrolyte and a preparation method thereof, and an all-solid-state lithium-ion battery. Background Art
[0002] Lithium batteries with liquid / gel electrolytes are widely used in commercial electronic devices, but in large-scale applications such as electric vehicles and smart grids, their flammability, volatility, thermal instability, narrow electrochemical window, and difficulty in inhibiting the growth of lithium dendrites limit the safety and energy density of traditional liquid batteries. Therefore, it is imperative to develop new electrolytes for the next generation of batteries.
[0003] All-solid-state batteries use thermally stable solid electrolytes such as sulfides, halides and oxides instead of liquid electrolytes. The conductivity of sulfides is close to that of liquid electrolytes, and they have the advantages of being soft, non-corrosive to equipment and environmentally friendly, which has attracted widespread attention. However, there is still room for improvement in the first-cycle charge and discharge efficiency, and their stability is insufficient when used as negative electrodes. The capacity loss of the positive electrode material mainly results from structural changes after the first discharge, and the number of sites where lithium can be inserted in the material is reduced. The capacity loss of the negative electrode material is mainly due to the formation of the SEI film on the surface of the negative electrode during charging, which irreversibly consumes lithium ions. The first efficiency of the full battery is consistent with the one with the lower first efficiency of the positive or negative electrode.
[0004] In order to alleviate the material pulverization caused by volume change of high-nickel NCM (nickel, cobalt, manganese) positive electrode materials during the cycle, the main solution is to increase the test pressure or add oxide / halide interlayers. However, the increased test pressure also promotes the growth of lithium dendrites to a certain extent and penetrates the electrolyte to cause battery short circuit. At the same time, oxides / halides also have problems such as insufficient ion conductivity, which reduces the positive electrode potential to a certain extent.
[0005] In summary, it is necessary to provide a composite electrolyte and a preparation method thereof and an all-solid-state lithium-ion battery to further improve the first-cycle charge and discharge efficiency of the all-solid-state lithium-ion battery. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a composite electrolyte and a preparation method thereof and an all-solid-state lithium-ion battery to further improve the first-cycle charge and discharge efficiency of the all-solid-state lithium-ion battery.
[0007] A first aspect of the present invention provides a composite electrolyte.
[0008] Specifically, the composite electrolyte includes a lithium conductive mixture and a sulfide electrolyte;
[0009] The lithium conductive mixture is coated with a sulfide electrolyte;
[0010] The lithium-conducting mixture includes plastic crystal and lithium salt;
[0011] The mass ratio of the plastic crystal to the lithium salt is 2 to 12:1.
[0012] Preferably, the mass ratio of the plastic crystal to the lithium salt is 3 to 6.88:1.
[0013] Preferably, the plastic crystal includes P 12 FSI, P 12 TFSI、PP 12 FSI、PP 12 TFSI、PP 11 FSI、PP 22 FSI、PP 23 FSI、PP 11 TFSI、PP 22 TFSI、PP 23 At least one of the TFSI.
[0014] Preferably, the plastic crystal accounts for 5 to 95% of the total mass of the composite electrolyte.
[0015] Preferably, the lithium salt includes at least one of LiTFSI, LiFSI, Li(CF3SO2)3C, LiC4F9SO3, LiN(SO2CF2CF3)2, LiB(C2O4)2, LiBF4, LiBF3(C2F5), LiSCN, LiN(CN)2, LiDFOB, LiODFB, LiN(SO2F)2, LiCF3SO3, LiClO4, LiAsF6, and LiSbF6.
[0016] Preferably, the sulfide electrolyte includes Li3PS4, Li4P2S6 or Li 7-a PS 6-a X a wherein X is at least one of Cl, Br, and I, and the value of a is 0.5 to 2.
[0017] Further preferably, the Li 7-a PS 6-a X a Including at least one of Li6PS5Cl, Li6PS5Br, and Li6PS5I.
[0018] Preferably, the mass ratio of the sulfide electrolyte to the lithium-conducting mixture is 1 to 20:1.
[0019] Further preferably, the mass ratio of the sulfide electrolyte to the lithium-conducting mixture is 6 to 10:1.
[0020] The composite electrolyte has the characteristics of high lithium ion conductivity and soft powder particles.
[0021] A second aspect of the present invention provides a method for preparing a composite electrolyte.
[0022] Specifically, the following steps are included:
[0023] The lithium-conducting mixture formed by mixing plastic crystals with lithium salts is used to coat the sulfide electrolyte to obtain the composite electrolyte.
[0024] Preferably, the coating method includes any one of a solvent method, a grinding and mixing method, and a melt mixing method.
[0025] Further preferably, the solvent method comprises the following steps:
[0026] A lithium-conducting mixture formed by mixing plastic crystals and lithium salts is dissolved in a solvent, and a sulfide electrolyte is added for coating. After stirring, the solvent is removed by rotary evaporation, and vacuum drying is performed to obtain a composite electrolyte.
[0027] Preferably, the solvent includes at least one of ethyl acetate, butyl butyrate, isobutyl isobutyrate, cyclohexane, n-heptane and p-xylene.
[0028] Preferably, the state of the lithium-conducting mixture includes any one of liquid, solid and semi-solidified state.
[0029] A third aspect of the present invention provides an all-solid-state lithium-ion battery.
[0030] Specifically, the all-solid-state lithium-ion battery includes the composite electrolyte provided in the first aspect.
[0031] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0032] The present invention prepares a composite electrolyte by coating a lithium-conducting mixture containing plastic crystals with a sulfide electrolyte, and controls the mass ratio of plastic crystals to lithium salts to be 2 to 12:1 and the mass ratio of sulfide electrolyte to lithium-conducting mixture to be 1 to 20:1. The prepared composite electrolyte can improve the contact effect between sulfide and positive electrode active material on the positive electrode side, improve the mass transfer efficiency, and further improve the first effect of the positive electrode and the first cycle discharge capacity; on the negative electrode side, it can reduce the reduction-intolerant side reaction of sulfide and improve the rate performance of graphite negative electrode. In addition, the solid-state battery prepared by the composite electrolyte of the present invention has high structural stability at high temperature; the preparation method of the present invention has a simple process, is compatible with traditional lithium-ion battery process equipment, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Schematic diagram of the preparation method of the composite electrolyte of the present invention. DETAILED DESCRIPTION
[0034] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0035] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0036] Example 1
[0037] Composite electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0038] P 12 TFSI and LiTFSI were mixed in a mass ratio of 3.43:1 and stirred to form a lithium-conducting mixture.
[0039] Take 0.2 g of the lithium-conducting mixture and disperse it in 20 mL of ethyl acetate. After ultrasonic dispersion, add 2 g of Li3PS4. After stirring, remove the ethyl acetate solvent by rotary evaporation. After vacuum drying, obtain the composite electrolyte P. 12 TFSI-3.43@SE.
[0040] Take 0.1 g of the coated composite electrolyte P 12 TFSI-3.43@SE, 0.4 g of NCM85 cathode material, 0.003 g of VGCF and 0.003 g of PTFE were dry-ground to prepare cathode sheets, which were then cut into discs with a diameter of 0.9 cm. 12 TFSI-3.43@SE is used as the intermediate electrolyte layer, and LiIn alloy sheets (Li sheet diameter 0.6 cm, In sheet diameter 0.9 cm) are used as the negative electrode to assemble the solid-state battery for charge and discharge tests. The active material surface density of the electrode sheet is 22.36 mg cm -2 , assembly pressure 4T, test pressure 5Nm, first cycle 0.1C and then 0.1C cycle, room temperature, voltage range 2.2~3.7V (vs.LiIn), cycle 100 cycles. 12 The ionic conductivity of TFSI-3.43@SE is 1.2*10 -3 S cm -1 .
[0041] Example 2
[0042] Composite electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0043] P 12TFSI and LiTFSI were mixed in a mass ratio of 3.43:1 and stirred to form a lithium-conducting mixture.
[0044] 0.2 g of the lithium-conducting mixture was dispersed in 20 mL of ethyl acetate. After ultrasonic dispersion, 1.2 g of Li3PS4 was added. After stirring, the ethyl acetate solvent was removed by rotary evaporation. After vacuum drying, the composite electrolyte P was obtained. 12 TFSI-3.43@SE.
[0045] Take 0.1 g of the coated composite electrolyte P 12 TFSI-3.43@SE, 0.4 g of NCM85 cathode material, 0.003 g of VGCF and 0.003 g of PTFE were dry-ground to prepare cathode sheets, which were then cut into discs with a diameter of 0.9 cm. 12 TFSI-3.43@SE is used as the intermediate electrolyte layer, and LiIn sheet is used as the negative electrode to assemble the solid-state battery for charge and discharge tests.
[0046] Example 3
[0047] Composite electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0048] PP 12 FSI and LiFSI were mixed in a mass ratio of 6.88:1 and stirred to form a lithium-conducting mixture.
[0049] Take 0.2 g of the lithium-conducting mixture and disperse it in 20 mL of ethyl acetate. After ultrasonic dispersion, add 2 g of Li3PS4. After stirring, remove the ethyl acetate solvent by rotary evaporation. After vacuum drying, obtain the composite electrolyte PP. 12 FSI-3.43@SE.
[0050] Take 0.1 g of the coated composite electrolyte PP 12 FSI-6.88@SE, 0.4 g of NCM83 cathode material, 0.005 g of VGCF and 0.005 g of PTFE were dry ground to prepare cathode sheets, which were then cut into discs with a diameter of 0.9 cm. 12 FSI-6.88@SE was used as the intermediate electrolyte layer, and LiIn sheets were used as the negative electrode to assemble the solid-state battery for charge and discharge tests.
[0051] Example 4
[0052] Composite electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0053] PP 12 TFSI and LiTFSI are mixed in a mass ratio of 3:1 and stirred to form a lithium-conducting mixture.
[0054] Take 0.2 g of the lithium-conducting mixture and disperse it in 20 mL of ethyl acetate. After ultrasonic dispersion, add 2 g of Li3PS4. After stirring, remove the ethyl acetate solvent by rotary evaporation. After vacuum drying, obtain the composite electrolyte PP. 12 TFSI-3@SE.
[0055] Take 0.1 g of the coated composite electrolyte PP 12 TFSI-3@SE, 0.4 g of NCM83 cathode material, 0.0025 g of VGCF and 0.005 g of PTFE were dry-ground to prepare cathode sheets, which were then cut into discs with a diameter of 0.9 cm. 12 TFSI-3@SE is used as the middle electrolyte layer, and LiIn sheet is used as the negative electrode to assemble the solid-state battery for charge and discharge tests.
[0056] Example 5
[0057] Composite electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0058] P 12 TFSI and LiTFSI were mixed in a mass ratio of 3.43:1 and stirred to form a lithium-conducting mixture.
[0059] Take 0.2 g of the lithium-conducting mixture and disperse it in 20 mL of ethyl acetate. After ultrasonic dispersion, add 2 g of Li3PS4. After stirring, remove the ethyl acetate solvent by rotary evaporation. After vacuum drying, obtain the composite electrolyte P. 12 TFSI-3.43@SE.
[0060] Take 0.2 g of the coated composite electrolyte P 12 TFSI-3.43@SE, 0.3 g of graphite negative electrode material, 0.005 g of VGCF and 0.005 g of PTFE were dry-ground to prepare positive electrode sheets, which were then cut into discs with a diameter of 0.8 cm. 12 TFSI-3.43@SE is used as the intermediate electrolyte layer, and LiIn sheet is used as the negative electrode to assemble the solid-state battery for charge and discharge tests.
[0061] The surface density of active material of the electrode is 7.49 mg cm -2 , assembly pressure 4T, test pressure 5Nm, 0.05C for two cycles, 0.1C for three cycles, then 0.3C for 100 cycles, room temperature, voltage range -0.6~1.5V (vs.LiIn). The composite electrolyte P was measured with a blocked electrode. 12 The ionic conductivity of TFSI-3.43@SE is 1.2*10 -3 S cm -1 .
[0062] Comparative Example 1
[0063] Electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0064] The difference from Example 1 is that in Comparative Example 1, no plastic crystal and lithium salt are added.
[0065] Take 0.1g electrolyte SE, 0.4g NCM85 positive electrode material, 0.003g VGCF and 0.003g PTFE and dry grind them to make positive electrode sheets, and cut them into discs with a diameter of 0.9cm. Use electrolyte SE as the middle electrolyte layer and LiIn sheet as the negative electrode to assemble solid-state batteries and conduct charge and discharge tests.
[0066] Comparative Example 2
[0067] Composite electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0068] The difference from Example 2 is that in Example 2, the mass ratio of plastic crystal to lithium salt is increased.
[0069] P 12 TFSI and LiTFSI were mixed at a mass ratio of 13.72:1 and stirred to form a lithium-conducting mixture.
[0070] 0.2 g of the lithium-conducting mixture was dispersed in 20 mL of ethyl acetate. After ultrasonic dispersion, 1.2 g of Li3PS4 was added. After stirring, the ethyl acetate solvent was removed by rotary evaporation. After vacuum drying, the composite electrolyte P was obtained. 12 TFSI-13.72@SE.
[0071] Take 0.1 g of the coated composite electrolyte P 12 TFSI-13.72@SE, 0.4 g of NCM85 cathode material, 0.003 g of VGCF and 0.003 g of PTFE were dry-ground to prepare cathode sheets, which were then cut into discs with a diameter of 0.9 cm. 12 TFSI-13.72@SE was used as the intermediate electrolyte layer, and LiIn sheets were used as the negative electrode to assemble the solid-state battery for charge and discharge tests.
[0072] Comparative Example 3
[0073] Composite electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0074] The difference between Comparative Example 3 and Example 3 is that in Comparative Example 3, the mass ratio of plastic crystal to lithium salt is reduced.
[0075] PP 12 FSI and LiFSI were mixed in a mass ratio of 1.64:1 and stirred to form a lithium-conducting mixture.
[0076] Take 0.2 g of the lithium-conducting mixture and disperse it in 20 mL of ethyl acetate. After ultrasonic dispersion, add 2 g of Li3PS4. After stirring, remove the ethyl acetate solvent by rotary evaporation. After vacuum drying, obtain the composite electrolyte PP. 12 FSI-1.64@SE.
[0077] Take 0.1 g of the coated composite electrolyte PP 12 FSI-1.64@SE, 0.4 g of NCM83 cathode material, 0.005 g of VGCF and 0.005 g of PTFE were dry ground to prepare cathode sheets, which were then cut into discs with a diameter of 0.9 cm. 12 FSI-1.64@SE was used as the intermediate electrolyte layer, and LiIn sheets were used as the negative electrode to assemble the solid-state battery for charge and discharge tests.
[0078] Comparative Example 4
[0079] Composite electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0080] The difference between Comparative Example 4 and Example 4 is that the plastic crystal is replaced by succinonitrile (SN).
[0081] SN and LiTFSI were mixed in a mass ratio of 3:1 and stirred to form a lithium-conducting mixture.
[0082] 0.2 g of the lithium-conducting mixture was dispersed in 20 mL of ethyl acetate. After ultrasonic dispersion, 2 g of Li3PS4 was added. After stirring, the ethyl acetate solvent was removed by rotary evaporation. After vacuum drying, the composite electrolyte SN-3@SE was obtained.
[0083] Take 0.1g of coated composite electrolyte SN-3@SE, 0.4g of NCM83 positive electrode material, 0.0025g of VGCF and 0.005g of PTFE to dry grind the positive electrode sheet and cut it into a disc with a diameter of 0.9cm. Use composite electrolyte SN-3@SE as the intermediate electrolyte layer and LiIn sheet as the negative electrode to assemble a solid-state battery for charge and discharge tests.
[0084] Comparative Example 5
[0085] Electrolyte and preparation method thereof and all-solid-state lithium-ion battery.
[0086] The difference from Example 5 is that in Comparative Example 5, no plastic crystal and lithium salt are added.
[0087] Take 0.1g electrolyte SE, 0.3g graphite negative electrode material, 0.005g VGCF and 0.005g PTFE and dry grind them to make positive electrode sheets, and cut them into discs with a diameter of 0.8cm. Use electrolyte SE as the middle electrolyte layer and LiIn sheet as the negative electrode to assemble solid-state batteries and conduct charge and discharge tests.
[0088] Detection method:
[0089] 1. First coulombic efficiency: The all-solid-state lithium-ion battery is charged and discharged for the first time at room temperature at a rate of 0.1C. The first coulombic efficiency = first discharge capacity / first charge capacity × 100%;
[0090] 2. The discharge capacity of the nth cycle is less than 80% of the first cycle: 0.1C cycle, the discharge specific capacity is read from the battery cycle data.
[0091] Test results:
[0092] Table 1 Test results of Examples 1 to 4 and Comparative Examples 1 to 4
[0093]
[0094] The all-solid-state lithium-ion battery prepared in Example 1 of the present invention has higher performance than that of Comparative Example 1 in terms of first charge specific capacity, first discharge specific capacity, first coulomb efficiency, and discharge capacity of the nth cycle lower than 80% of the first cycle discharge, indicating that the performance of the all-solid-state lithium-ion battery will be reduced if no plastic crystal is added in Comparative Example 1. Compared with Example 2, the mass ratio of plastic crystal to lithium salt in Comparative Example 2 is increased, which reduces the lithium conductivity, thereby reducing the charge / discharge specific capacity of the positive electrode sheet; compared with Example 3, the mass ratio of plastic crystal to lithium salt in Comparative Example 3 is too small, the viscosity is increased, the lithium conductivity is reduced, and the charge / discharge specific capacity of the positive electrode sheet is reduced; compared with Example 4, in Comparative Example 4, the plastic crystal is replaced with succinonitrile (SN), and there is a side reaction between SN and the sulfide electrolyte, which reduces the charge and discharge performance of the positive electrode sheet.
[0095] Table 2 Test results of Example 5 and Comparative Example 5
[0096]
[0097] Compared with comparative example 5, example 5 of the present invention additionally adds plastic crystals. On the negative electrode side, the composite electrolyte prepared by the present invention can reduce the reduction-intolerant side reaction of sulfides and improve the rate performance of the graphite negative electrode.
[0098] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution obtained by any modification, equivalent replacement, improvement, etc. made by a person skilled in the art based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art shall be within the scope of protection determined by the claims.
Claims
1. A composite electrolyte, characterized in that The composite electrolyte includes a lithium conductive mixture and a sulfide electrolyte; The lithium conductive mixture is coated with a sulfide electrolyte; The lithium-conducting mixture includes plastic crystal and lithium salt; The mass ratio of the plastic crystal to the lithium salt is 2 to 12:
1.
2. The composite electrolyte according to claim 1, characterized in that The plastic crystal includes P 12 FSI, P 12 TFSI、PP 12 FSI、PP 12 TFSI、PP 11 FSI、PP 22 FSI、PP 23 FSI、PP 11 TFSI、PP 22 TFSI、PP 23 At least one of the TFSI.
3. The composite electrolyte according to claim 1, characterized in that The plastic crystal accounts for 5 to 95% of the total mass of the composite electrolyte.
4. The composite electrolyte according to claim 1, characterized in that The lithium salt includes at least one of LiTFSI, LiFSI, Li(CF3SO2)3C, LiC4F9SO3, LiN(SO2CF2CF3)2, LiB(C2O4)2, LiBF4, LiBF3(C2F5), LiSCN, LiN(CN)2, LiDFOB, LiODFB, LiN(SO2F)2, LiCF3SO3, LiClO4, LiAsF6, and LiSbF6.
5. The composite electrolyte according to claim 1, characterized in that The sulfide electrolyte includes Li3PS4, Li4P2S6 or Li 7-a PS 6-a X a wherein X is at least one of Cl, Br, and I, and the value of a is 0.5 to 2.
6. The composite electrolyte according to claim 1, characterized in that The mass ratio of the sulfide electrolyte to the lithium-conducting mixture is 1 to 20:
1.
7. The method for preparing the composite electrolyte according to any one of claims 1 to 6, characterized in that: The following steps are involved: The lithium-conducting mixture formed by mixing plastic crystals with lithium salts is used to coat the sulfide electrolyte to obtain the composite electrolyte.
8. The preparation method according to claim 7, characterized in that: The coating method includes any one of a solvent method, a grinding and mixing method, and a melt mixing method.
9. The preparation method according to claim 7, characterized in that: The state of the lithium conductive mixture includes any one of liquid, solid and semi-solidified state.
10. An all-solid-state lithium-ion battery, characterized in that: The all-solid-state lithium-ion battery comprises the composite electrolyte according to any one of claims 1 to 6.
Citation Information
Patent Citations
Solid electrolyte, energy storage device, and method for producing solid electrolyte
CN113508446A
Organic ion plastic crystal doped composite electrolyte membrane and preparation method and application thereof
CN115224357A
Sulfide solid electrolyte elastic membrane, preparation method thereof and lithium ion battery
CN117996165A
Solid-state electrolyte layer for all-solid-state lithium-ion secondary battery and all-solid-state lithium-ion secondary battery including the same
JP2020198270A
Secondary battery
JP2022082060A