All-solid-state battery containing conductive polymer composite 3D spheroidal graphene aluminum doped lithium zirconium oxide solid electrolyte membrane and preparation method of all-solid-state battery

By using conductive polymer composite 3D spherical graphene-like aluminum-doped lithium-zirconium-oxygen solid electrolyte membrane in all-solid-state lithium batteries, the contact between the solid electrolyte layer and the interface is improved, and the solid-solid interface impedance and lithium dendrites are solved. problem, improving battery performance and stability.

CN118782893APending Publication Date: 2024-10-15武汉中正泰能新能源科技有限公司

Patent Information

Application Number
CN202410859762.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In all-solid-state lithium batteries, the solid-solid interface resistance is large and the interface stability is poor, resulting in the generation of lithium dendrites, which limits battery performance.

Method used

A conductive polymer composite 3D spherical graphene-like aluminum-doped lithium-zirconium-oxygen solid electrolyte membrane is used. By setting a solid electrolyte interface infiltration modification layer and an interface management layer at the solid electrolyte layer and interface, the interface contact and stability are improved, and the interface is reduced. Interface impedance.

Benefits of technology

It effectively reduces the solid-solid interface resistance, improves the interface stability, solves the problem of lithium dendrites, and improves the energy density and cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782893A_ABST
    Figure CN118782893A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a conductive polymer composite 3D spheroidal graphene aluminum doped lithium zirconium oxide solid-state electrolyte membrane and preparation of an all-solid-state power battery comprising the solid-state electrolyte membrane. The manufacturing method of the solid-state electrolyte membrane comprises the following steps: S1, coating a base membrane with solid-state electrolyte interface infiltration modification layer slurry, a solid electrolyte interface infiltration modification layer is formed after curing, and a first membrane material is obtained; s2, the solid electrolyte interface infiltration modification layer of the first membrane material is coated with the 3D spheroidal graphene aluminum doped lithium zirconium oxide solid electrolyte slurry, a 3D spheroidal graphene aluminum doped lithium zirconium oxide solid electrolyte layer is formed after curing, and a second membrane material is obtained; and S3, performing hot-pressing compounding on the first membrane material and the second membrane material, and then removing one base membrane to obtain the conductive polymer composite 3D spheroidal graphene aluminum doped lithium zirconium oxide solid electrolyte membrane. According to the all-solid-state battery containing the conductive polymer composite 3D spheroidal graphene aluminum doped lithium zirconium oxide solid-state electrolyte membrane disclosed by the invention, the solid-solid interface impedance is effectively reduced, the interface stability is improved, and the problem of generation of lithium dendrites is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid-state batteries, and in particular to an all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium-oxygen solid electrolyte membrane and a preparation method thereof. Background Art

[0002] As batteries are used more and more widely, the energy density of existing batteries is far from meeting the needs, and it is urgent to improve the energy density of existing batteries. Replacing with new materials is one of the ways to improve battery energy density. The theoretical gram capacity of silicon anode reaches 3500mAh / g, which is nearly ten times the gram capacity of the current mainstream graphite anode. Replacing graphite with silicon anode can greatly improve the energy density of existing batteries. However, the silicon anode will undergo a huge volume change (~300%) during the cycle, causing the silicon particles to pulverize, exposing a fresh surface, contacting with the liquid electrolyte and forming a new SEI film, consuming electrolyte and active lithium, resulting in a short battery cycle life, which hinders the application of silicon anode in batteries.

[0003] Using solid electrolytes to replace liquid electrolytes can solve the above problems. All-solid-state lithium batteries have extremely high safety. Their solid electrolytes are non-flammable, non-corrosive, non-volatile, and non-leaking. They also overcome the lithium dendrite phenomenon, and the probability of spontaneous combustion of cars equipped with all-solid-state lithium batteries will be greatly reduced. At the same time, all-solid-state batteries have achieved a simultaneous increase in energy density, with an energy density of up to 400 to 1400Wh / kg.

[0004] However, the poor interface between the electrode and the solid electrolyte has limited the development of all-solid-state lithium batteries. Unlike traditional batteries using electrolytes, the electrolyte can be well infiltrated between the electrodes, so that lithium ions can migrate freely and quickly. In all-solid-state lithium-ion batteries, the solid electrolyte and the electrode will have a variety of reasons such as interface physical bonding quality (pores, cracks, etc.), lattice mismatch, and differences in thermal expansion coefficients, which will cause the migration speed of lithium ions at the interface between the electrode and the electrolyte to be greatly reduced, forming lithium elements at the interface. Aggregation, limiting the performance of lithium-ion batteries. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide an all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane, which effectively reduces the solid-solid interface impedance, improves the interface stability, and solves the problem of lithium dendrite generation.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] The first aspect of the present invention provides a method for manufacturing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium-oxygen solid electrolyte membrane, comprising the following steps:

[0008] S1. The solid electrolyte interface infiltration modification layer slurry is coated on a base film, and after curing, a solid electrolyte interface infiltration modification layer is formed to obtain a first film material;

[0009] S2. The 3D-type spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte slurry is coated on the solid electrolyte interface wetting modification layer of the first film, and after curing, a 3D-type spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte layer is formed to obtain a second film;

[0010] S3. The first film material and the second film material are hot-pressed and composited, and then one of the base films is peeled off to obtain the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane.

[0011] Furthermore, in step S1, the solid electrolyte interface wetting modification layer slurry contains the following components by mass percentage: 2% to 5% of conductive polymer, 0.5% to 3% of nano-alumina particles, 1% to 5% of nano-silicon dioxide particles, 2% to 8% of conductive agent, and the balance of organic solvent; and / or,

[0012] The thickness of the solid electrolyte interface wetting modification layer is 1 to 3 μm; and / or,

[0013] The base film includes a PET film.

[0014] Further, in step S2, the 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer slurry contains the following components by mass percentage: 2% to 8% conductive polymer, 62% to 70% solid electrolyte, 0.5% to 5% 3D spherical graphene, 0.1% to 3% conductive agent, 1% to 5% nano-silicon dioxide particles, and the remainder organic solvent; and / or,

[0015] The thickness of the 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer is 5 to 15 μm.

[0016] Further, the conductive high molecular polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, and polymethyl methacrylate; and / or,

[0017] The solid electrolyte comprises at least one of LLZO, LALZO and LATP; and / or,

[0018] The particle size of the nano-alumina particles and the nano-silicon dioxide particles is 10 to 100 nm; and / or,

[0019] The conductive agent includes at least one of carbon nanofibers, carbon nanotubes, graphene, conductive carbon black, and conductive graphite; and / or,

[0020] The diameter of the 3D spherical graphene is 2-9 nm, and the tap density is 0.5-0.8 g / cm 3 , with a specific surface area of ​​5000-6000m 2 / g, the resistivity is (9~12)×10 -6 Ω.

[0021] Furthermore, in the solid electrolyte interface wetting modification layer slurry, the mass percentage of each component is: polyvinylidene fluoride 2% to 4%, nano silicon dioxide particles 2.5% to 3%, nano alumina particles 0.5% to 1%, super-P Li 1.5% to 2.5%, Ketjen black ECP-600JD 0.5% to 1%, VGCF 0.5% to 1%, and the balance acetone; and / or,

[0022] The mass percentage of each component in the 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer slurry is: polyvinylidene fluoride 3% to 5%, LALZO 65% to 70%, 3D spherical graphene 0.5% to 1%, VGCF 0.4 to 0.8%, nano-silicon dioxide particles 1% to 2%, and the balance acetone.

[0023] Furthermore, in step S3, the temperature of the hot pressing compound is 120-180°C.

[0024] The second aspect of the present invention provides a method for manufacturing an all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane, comprising the following steps:

[0025] a. The two solid electrolyte membranes are hot-pressed and composited on both sides of the positive electrode sheet, and then the base film is removed and the positive electrode ear is cut out to obtain a positive electrode sheet containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane;

[0026] b. coating the interface management layer slurry on a base film, and curing to form an interface management layer to obtain a third film material;

[0027] c. hot-pressing the two third films onto both sides of the negative electrode sheet, removing the base film, cutting out the negative electrode tabs, and obtaining a negative electrode sheet containing an interface management layer;

[0028] d. The plurality of positive electrodes containing the conductive polymer composite 3D-like spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane and the plurality of negative electrodes containing the interface management layer are alternately stacked and fixed in a stacked manner to obtain a battery cell;

[0029] e. Coating the outer edge of the battery with anti-short-circuit ceramic oxide;

[0030] f. The cells are sequentially packaged, dried, activated by electrolyte, formed and divided to obtain an all-solid-state battery containing a conductive polymer composite 3D-like spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane;

[0031] Among them, in step a, the solid electrolyte membrane is a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane prepared by the above method.

[0032] Furthermore, in step b, the interface management layer slurry contains the following components by mass percentage: 2% to 8% of conductive polymer, 1% to 4% of nano-silicon dioxide particles, 0.5% to 3% of nano-alumina particles, 0.5% to 2% of conductive agent, and the balance of organic solvent; and / or,

[0033] The interface management layer slurry comprises the following components by mass percentage: 1.5% to 2% polyvinylidene fluoride, 2% to 4% polymethyl methacrylate, 1.5% to 2.5% nano silicon dioxide particles, 0.5% to 1.5% nano aluminum oxide particles, 0.5% to 1% super-P Li, and the balance acetone; and / or,

[0034] The thickness of the interface management layer is 1-2 μm.

[0035] Furthermore, in step e, the method of coating the short-circuit-proof ceramic oxide comprises:

[0036] Immerse the battery cell in an anti-short circuit coating solution for 3 to 10 seconds, then take it out and dry it; or spray the anti-short circuit coating solution on the outer edge of the battery cell, and then dry it;

[0037] Wherein, the anti-short circuit coating solution comprises the following components by mass percentage: 1% to 6% of conductive polymer, 1% to 5% of nano silicon dioxide particles, 1% to 3% of nano aluminum oxide particles, and the balance of organic solvent; and / or,

[0038] The anti-short circuit coating solution comprises the following components by mass percentage: 2% to 5% of polyvinylidene fluoride, 2% to 4% of nano silicon dioxide particles, 1% to 2% of nano aluminum oxide particles, and the balance of acetone.

[0039] The third aspect of the present invention provides an all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane, and the all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane is prepared by the aforementioned method.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1. The present invention provides an all-solid-state battery containing a conductive polymer composite 3D quasi-spherical graphene aluminum-doped lithium zirconium oxide, wherein the solid electrolyte layer includes a conductive polymer, an oxide solid electrolyte, a 3D spherical graphene, nano-ceramic particles and a conductive agent, wherein the conductive polymer can be used as a binder to improve the interface contact, improve the molding performance of the solid electrolyte layer, improve the toughness of the solid electrolyte layer, and fill the gaps generated in the oxide solid electrolyte film during the preparation process; the nano-ceramic particles are small in size and can be filled in the pores between the oxide solid electrolyte particles, thereby avoiding lithium dendrites from penetrating the solid electrolyte layer; in addition, the nano-ceramic particles can also be used as a reinforcing phase to help improve the strength of the solid electrolyte layer; the 3D spherical graphene is quasi-spherical and has a higher specific surface area, so it can increase the contact between the oxide solid electrolyte particles and the conductive agent, build an efficient ion and electron transmission network, and improve the migration ability of charged particles in the solid electrolyte layer.

[0042] 2. The all-solid-state battery containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide provided by the present invention has a solid electrolyte interface wetting modification layer on both sides of the solid electrolyte layer. The solid electrolyte layer serves as a transition layer between the solid electrolyte layer and the positive and negative electrodes, has good toughness, can seal the holes and cracks on the surface of the solid electrolyte layer, improve the interface contact with the positive and negative electrodes, improve the stability of the solid-solid interface, reduce the interface impedance, and solve the problem of lithium dendrite generation.

[0043] 3. The all-solid-state battery containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide provided by the present invention has interface management layers on both sides of the negative electrode sheet. The interface management layer can not only improve the interface contact with the solid electrolyte membrane and enhance the interface stability; but also the interface management layer contains super-P Li, which can replace the pre-lithiation function and replenish lithium to the negative electrode, so that the first coulombic efficiency of the battery is effectively improved.

[0044] 4. The all-solid-state battery containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide provided by the present invention can prepare the positive electrode of the solid electrolyte membrane containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide by hot pressing transfer during the preparation process, and can prepare a very thin solid electrolyte membrane. In addition, during the hot pressing composite process, the conductive polymer in the solid electrolyte interface infiltration modification layer can infiltrate into the cracks and holes on the surface of the solid electrolyte layer, thereby better sealing the cracks and holes. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a schematic diagram of the structure of a positive electrode sheet containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide;

[0046] Figure 2 It is a schematic diagram of the structure of the negative electrode sheet containing the interface management layer;

[0047] Figure 3 Schematic diagram of the stacking structure of a battery cell in one embodiment of the present invention;

[0048] Figure 4 1 is the discharge curve of the all-solid-state battery of Example 1 at different rates;

[0049] Figure 5 This is the first cycle charge and discharge curve of the all-solid-state battery of Example 2;

[0050] Among them: 1. positive electrode; 2. first solid electrolyte interface wetting modification layer; 3. conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer; 4. second solid electrolyte interface wetting modification layer; 5. negative electrode; 6. interface management layer;

[0051] A. A positive electrode sheet containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide; B. A negative electrode sheet containing an interface management layer. DETAILED DESCRIPTION

[0052] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings and the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0053] In view of the problems of large solid-solid interface impedance and poor interface stability in the prior art all-solid-state batteries, the present invention provides an all-solid-state battery, which effectively reduces the solid-solid interface impedance, improves the interface stability, and solves the problem of lithium dendrite generation.

[0054] For details, see Figure 1-3The all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte membrane provided by the present invention comprises a plurality of alternatingly stacked positive electrode sheets A containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide and a negative electrode sheet B containing an interface management layer. Among them, the positive electrode sheet A containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide comprises a positive electrode sheet 1, a first solid electrolyte interface infiltration modification layer 2, a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer 3 and a second solid electrolyte interface infiltration modification layer 4, the first solid electrolyte interface infiltration modification layer 2 is formed on both sides of the positive electrode sheet 1, the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer 3 is formed on the surface of the first solid electrolyte interface infiltration modification layer 2, and the second solid electrolyte interface infiltration modification layer 4 is formed on the surface of the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer 3.

[0055] In the present invention, the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer includes a conductive polymer, an oxide solid electrolyte, a 3D spherical graphene, nano-silicon dioxide particles and a conductive agent. Among them, the oxide solid electrolyte has excellent chemical stability, can withstand high voltage, and has a high decomposition temperature. However, the Young's modulus of the oxide solid electrolyte particles is relatively high, resulting in poor interface contact with the active material, thereby generating a large interface impedance. Therefore, the present invention also adds a certain amount of conductive polymer to the solid electrolyte layer, wherein the conductive polymer can be used as a binder to improve the interface contact, and can also improve the molding performance of the solid electrolyte layer, improve the toughness of the solid electrolyte layer, and can also fill the gaps generated in the oxide solid electrolyte film during the preparation process.

[0056] In some embodiments of the present invention, the solid electrolyte includes but is not limited to at least one of garnet-type lithium lanthanum zirconium oxide (LLZO), aluminum-doped lithium lanthanum zirconium oxide (LALZO), and lithium aluminum titanium phosphate (LATP). In a preferred embodiment, the oxide solid electrolyte is LALZO, which has the advantages of high room temperature ionic conductivity, stability to metallic lithium, high oxidation potential, and controllable particle size.

[0057] In some embodiments of the present invention, the conductive polymer includes at least one of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polymethyl methacrylate (PMMA). Preferably, the conductive polymer is PVDF.

[0058] Since the particles of the oxide solid electrolyte are relatively large, there are a large number of pores between the particles. The presence of these pores will not only reduce the conductivity of the solid electrolyte layer, but also the lithium dendrites grown on the surface of the negative electrode will penetrate the pores, causing a short circuit in the battery. Therefore, in the present invention, a certain amount of nano-ceramic particles are also added to the solid electrolyte layer. This type of nano-ceramic particles is relatively small in size and can be filled in the pores between the oxide solid electrolyte particles, thereby preventing lithium dendrites from penetrating the solid electrolyte layer; in addition, the nano-ceramic particles can also serve as a reinforcing phase, which helps to improve the strength of the solid electrolyte layer.

[0059] In the present invention, the nano-ceramic particles are nano-silicon dioxide particles, and their D50 particle size is preferably 10 to 100 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc.

[0060] In the present invention, the solid electrolyte layer also includes a conductive agent, which is filled in the pores between the oxide solid electrolyte particles, and a conductive network with a spatial structure can be constructed, thereby improving the conductivity of the oxide solid electrolyte. In some embodiments of the present invention, the above-mentioned conductive agent may be a conductive agent commonly used in the art, including but not limited to at least one of carbon nanofibers, carbon nanotubes, conductive carbon black, and conductive graphite. Preferably, the conductive agent is a fibrous conductive agent, such as carbon nanofibers, carbon nanotubes, etc., which can better connect the oxide solid electrolyte together to form a more complete conductive network. Further preferably, the conductive agent is vapor grown carbon fiber (VGCF).

[0061] In the present invention, the solid electrolyte layer also includes 3D quasi-spherical graphene. Different from ordinary layered graphene, 3D quasi-spherical graphene is quasi-spherical and has a higher specific surface area. Therefore, it can increase the contact between the oxide solid electrolyte particles and the conductive agent, and build an efficient ion and electron transport network, thereby improving the migration ability of charged particles in the solid electrolyte layer. In some embodiments of the present invention, the diameter of the above-mentioned 3D quasi-spherical graphene is 2 to 9 nm, and the tap density is 0.5 to 0.8 g / cm 3 , with a specific surface area of ​​5000-6000m 2 / g, the resistivity is (9~12)×10 -6 Ω.

[0062] In some embodiments of the present invention, the thickness of the solid electrolyte layer is 5 to 15 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 12 μm, 14 μm, 15 μm, etc.

[0063] Due to the material properties of the solid electrolyte layer, cracks and holes will inevitably appear on its surface during the preparation process, resulting in poor interface stability of the solid electrolyte layer, high interface impedance between the positive and negative electrodes, and the generation of lithium dendrites. In the present invention, in order to solve the above problems, a solid electrolyte interface wetting modification layer is composited on both sides of the solid electrolyte layer, such as Figure 1 As shown, the first solid electrolyte interface infiltration modification layer and the second solid electrolyte interface infiltration modification layer are respectively formed, thereby obtaining a solid electrolyte membrane containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide. The raw materials of the solid electrolyte interface infiltration modification layer include conductive polymer, nano-ceramic particles and conductive agent. As a transition layer between the solid electrolyte layer and the positive and negative electrodes, it has good toughness, can close the holes and cracks on the surface of the solid electrolyte layer, improve the interface contact between the positive and negative electrodes, improve the stability of the solid-solid interface, reduce the interface impedance, and solve the problem of lithium dendrite generation.

[0064] In some embodiments of the present invention, the conductive high polymer includes, but is not limited to, one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polymethyl methacrylate (PMMA).

[0065] In some embodiments of the present invention, the nano ceramic particles include one or more of nano Al2O3, nano SiO2, nano TiO2, nano ZrO2, nano CeO2, nano MgO, nano ZnO and nano NiO. The D50 particle size of the nano ceramic particles is preferably 6 to 100 nm, for example, 6 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc. In a preferred embodiment, the nano ceramic particles are nano silicon dioxide particles and nano aluminum oxide particles.

[0066] In some embodiments of the present invention, the conductive agent includes at least one of carbon nanofibers, carbon nanotubes, graphene, conductive carbon black, and conductive graphite. Among them, the carbon nanofibers include vapor grown carbon fibers (VGCF), and the conductive carbon black includes Super-P, acetylene black, Ketjen black, etc.

[0067] In the present invention, the thickness of the solid electrolyte interface wetting modification layer is relatively thin and will not significantly increase the thickness of the solid electrolyte membrane. In some embodiments of the present invention, the thickness of the solid electrolyte interface wetting modification layer is 1 to 3 μm, for example, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, etc.

[0068] See also Figure 1The negative electrode sheet containing the interface management layer includes the negative electrode sheet and the interface management layers formed on both sides of the negative electrode sheet. The interface management layer includes a conductive polymer, nano-ceramic particles and a conductive agent. The presence of the interface management layer can improve the interface contact with the solid electrolyte membrane and enhance the interface stability.

[0069] In some embodiments of the present invention, the conductive polymer includes, but is not limited to, one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polymethyl methacrylate (PMMA). Preferably, the conductive polymer is PMMA and PVDF. PMMA has a good affinity for Li, which is beneficial to the transmission of Li ions; however, PMMA has poor temperature resistance, so by adding a certain amount of PVDF, the temperature resistance of PMMA is improved, which is beneficial to improving the high temperature resistance of the battery.

[0070] In some embodiments of the present invention, the nano ceramic particles include one or more of nano Al2O3, nano SiO2, nano TiO2, nano ZrO2, nano CeO2, nano MgO, nano ZnO and nano NiO. The D50 particle size of the nano ceramic particles is preferably 10 to 100 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc. In a preferred embodiment, the nano ceramic particles are nano silicon dioxide particles and nano aluminum oxide particles.

[0071] In some embodiments of the present invention, the conductive agent includes at least one of carbon nanofibers, carbon nanotubes, graphene, conductive carbon black, and conductive graphite. Among them, the carbon nanofibers include vapor grown carbon fibers (VGCF), and the conductive carbon black includes super-P Li, acetylene black, Ketjen black, etc.

[0072] In a preferred embodiment of the present invention, the conductive agent in the above-mentioned negative electrode interface management layer is super-P Li. Due to the formation of the solid electrolyte interface (SEI) film on the surface of the negative electrode during the first charging process of the lithium-ion battery, the active lithium in the positive electrode material will be permanently consumed, resulting in irreversible capacity loss and reducing the first coulombic efficiency of the battery. In this embodiment, since the interface management layer contains super-P Li, it can replace the pre-lithiation function and replenish lithium to the negative electrode, so that the first coulombic efficiency of the battery is effectively improved.

[0073] In some embodiments of the present invention, the thickness of the interface management layer is 1-2 μm, for example, 1 μm, 1.5 μm, 2 μm, etc.

[0074] In a preferred embodiment of the present invention, the outer edges of the positive electrode sheet containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte membrane and the negative electrode sheet containing an interface management layer are provided with an anti-short circuit coating layer to prevent the battery cell from short circuiting. The anti-short circuit coating layer includes a conductive polymer and nano-ceramic particles. Among them, the conductive polymer includes but is not limited to one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polymethyl methacrylate (PMMA).

[0075] In some embodiments of the present invention, the nano ceramic particles include nano silicon dioxide particles and nano aluminum oxide particles. The D50 particle size of the nano ceramic particles is preferably 10 to 100 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc.

[0076] The present invention also provides a method for manufacturing the above-mentioned conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane, comprising the following steps:

[0077] S1. The solid electrolyte interface infiltration modification layer slurry is coated on a base film, and after curing, a solid electrolyte interface infiltration modification layer is formed to obtain a first film material;

[0078] S2. The 3D-type spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte slurry is coated on the solid electrolyte interface wetting modification layer of the first film, and after curing, a 3D-type spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte layer is formed to obtain a second film;

[0079] S3. The first film material and the second film material are hot-pressed and composited, and then one of the base films is peeled off to obtain the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane.

[0080] In the above step S1, the solid electrolyte interface wetting modification layer slurry is obtained by adding conductive polymer, nano-ceramic particles and conductive agent into an organic solvent according to a ratio and stirring evenly; wherein the organic solvent can be selected from commonly used organic solvents that can dissolve polymers, including but not limited to acetone.

[0081] In some embodiments of the present invention, the solid electrolyte interface wetting modification layer slurry contains the following components in mass percentage: 2% to 5% conductive polymer, 0.5% to 3% nano-alumina particles, 1% to 5% nano-silicon dioxide particles, 2% to 8% conductive agent, and the remainder organic solvent. Among them, the mass percentage of conductive high polymer is 2% to 5%, for example, it can be 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% and the like; the mass percentage of nano-alumina particles is 0.5%, % to 3%, for example, it can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3% and the like; the mass percentage of nano-silicon dioxide particles is 1% to 5%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% and the like; the mass percentage of conductive agent is 2% to 8%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8% and the like.

[0082] In a preferred embodiment of the present invention, the composition of the solid electrolyte interface wetting modification layer slurry is: polyvinylidene fluoride 2% to 4%, nano silicon dioxide particles 2.5% to 3%, nano alumina particles 0.5% to 1%, super-PLi 1.5% to 2.5%, Ketjen black ECP-600JD 0.5% to 1%, VGCF 0.5% to 1%, and the balance acetone. A further preferred composition is: PVDF 3%, SiO2 3%, Al2O3 1%, super-P Li 2%, Ketjen black ECP-600JD 0.5%, VGCF 0.5%, and acetone 90%.

[0083] In the above step S1, the base film can be a PET film. In some embodiments, after the solid electrolyte interface wetting modification layer is coated on the base film, the base film is divided into two to obtain two first film materials. In the subsequent step S2, a solid electrolyte layer can be coated on one of the first film materials to obtain a second film material.

[0084] In the above step S2, the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer slurry is obtained by adding conductive polymer, oxide solid electrolyte, 3D spherical graphene, nano-silicon dioxide particles and conductive agent into an organic solvent according to a proportion and stirring evenly; wherein the organic solvent can be selected from commonly used organic solvents that can dissolve polymers, including but not limited to acetone.

[0085] In some embodiments of the present invention, the 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer slurry contains the following components in mass percentage: 2% to 8% conductive polymer, 62% to 70% solid electrolyte, 0.5% to 5% 3D spherical graphene, 0.1% to 3% conductive agent, 1% to 5% nano-silicon dioxide particles, and the remainder organic solvent. Among them, the mass percentage of the conductive high molecular polymer is 2% to 8%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, etc.; the mass percentage of the solid electrolyte is 62% to 70%, for example, it can be 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, etc.; the mass percentage of the 3D spherical graphene is 0.5% to 5%, for example, it can be 0.5%, 1%, 2%, 3%, 4%, 5%, etc.; the mass percentage of the conductive agent is 0.1% to 3%, for example, it can be 0.1%, 0.5%, 1%, 2%, 3%, etc.; the mass percentage of the nano-silicon dioxide particles is 1% to 5%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0086] In a preferred embodiment of the present invention, the composition of the 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer slurry is: polyvinylidene fluoride 3% to 5%, LALZO 65% to 70%, 3D spherical graphene 0.5% to 1%, nano-silicon dioxide particles 1% to 2%, carbon nanofibers 0.4 to 0.8%, and the balance acetone. A further preferred composition is: PVDF 4%, LALZO 68.5%, 3D spherical graphene 1%, nano-SiO2 1%, VGCF 0.5%, and acetone 25%.

[0087] In the above step S3, the first membrane material and the second membrane material are unwound in a roll-to-roll manner, and the solid electrolyte interface wetting modification layer of the first membrane material is ensured to be opposite to the solid electrolyte layer of the second membrane material, and then hot-pressed to composite the first membrane material and the second membrane material together.

[0088] In the above step S3, the temperature of the hot pressing compound is preferably controlled at 120-180°C, for example, it can be controlled at 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, etc.

[0089] In the present invention, the solid electrolyte interface wetting modification layer of the first film material is transferred to the solid electrolyte layer of the second film material by hot pressing and compounding, so that a solid electrolyte membrane with a thickness of less than 20 μm or even less than 15 μm can be prepared. However, it is impossible to prepare a solid electrolyte membrane with such a thin thickness by coating. In addition, during the hot pressing and compounding process, the conductive polymer and nano-ceramic particles in the solid electrolyte interface wetting modification layer can infiltrate into the cracks and holes on the surface of the solid electrolyte layer, thereby better sealing the cracks and holes.

[0090] The present invention also provides a method for preparing the above-mentioned all-solid-state battery containing the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane, comprising the following steps:

[0091] S4. The two conductive polymer composite 3D class spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membranes were hot-pressed composite on both sides of the positive electrode sheet, and then the base film was removed and the positive electrode ears were cut to obtain a positive electrode sheet containing a conductive polymer composite 3D class spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane;

[0092] S5. The interface management layer slurry is coated on a base film, and after curing, an interface management layer is formed to obtain a third film material;

[0093] S6. The two third films are respectively hot-pressed and laminated on both sides of the negative electrode sheet, and then the base film is peeled off and the negative electrode tab is cut out to obtain a negative electrode sheet containing an interface management layer;

[0094] S7. The plurality of positive electrodes containing the conductive polymer composite 3D-like spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane and the plurality of negative electrodes containing the interface management layer are alternately stacked and fixed in a stacked manner to obtain a battery cell;

[0095] S8. Coating the outer edge of the battery cell with an anti-short-circuit ceramic oxide;

[0096] S9. The battery cells are packaged, dried, electrolyte activated, formed and capacity divided in sequence to obtain the all-solid-state battery containing the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane.

[0097] In the above step S4, the solid electrolyte membrane can be divided into two parts, and then unwound in a roll-to-roll manner, so that the solid electrolyte interface infiltration modification layer faces the positive electrode sheet, and hot pressing is performed to composite the solid electrolyte membrane on both sides of the positive electrode sheet. The positive electrode sheet is composed of a positive electrode current collector and a positive electrode active material layer. The positive electrode current collector material may include any one or a combination of at least two of aluminum, copper, nickel, and zinc, preferably aluminum; the positive electrode active material in the positive electrode active material layer may include LiCoO2, LiMnO2, LiNiO2, LiVO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiMn2O4, LiTi5O 12 、Li(Ni 0.5 Mn 1.5 )O4, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, LiNbO3, any one of sodium iron phosphate or a combination of at least two thereof.

[0098] In the above steps S4 and S5, the temperature of the hot pressing compound is preferably controlled at 120-180°C, for example, it can be controlled at 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, etc.

[0099] In the above step S5, the interface management layer slurry is obtained by adding conductive polymer, nano-ceramic particles and conductive agent into an organic solvent according to a ratio and stirring evenly. The organic solvent can be a commonly used organic solvent that can dissolve polymers, including but not limited to acetone.

[0100] In some embodiments of the present invention, the interface management layer slurry contains the following components in mass percentage: 2% to 8% conductive polymer, 1% to 4% nano-silicon dioxide particles, 0.5% to 3% nano-aluminum oxide particles, 0.5% to 2% conductive agent, and the remainder organic solvent; wherein the mass percentage of the conductive polymer is 2% to 8%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, etc.; the mass percentage of the nano-silicon dioxide particles is 1% to 4%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, etc.; the mass percentage of the nano-aluminum oxide particles is 0.5% to 3%, for example, it can be 0.5%, 1%, 2%, 3%, etc.; the mass percentage of the conductive agent is 0.5% to 2%, for example, it can be 0.5%, 1%, 1.5%, 2%, etc.

[0101] In a preferred embodiment of the present invention, the interface management layer slurry contains the following components by mass percentage: 1.5% to 2% polyvinylidene fluoride, 2% to 4% polymethyl methacrylate, 1.5% to 2.5% nano-silicon dioxide particles, 0.5% to 1.5% nano-alumina particles, 0.5% to 1% super-P Li, and the balance acetone. A further preferred composition is: 2% polyvinylidene fluoride, 3% polymethyl methacrylate, 2% nano-silicon dioxide particles, 1% nano-alumina particles, 1% super-P Li, and 91% acetone.

[0102] In the above step S5, the base film includes but is not limited to a PET film. In some embodiments, after the interface management layer is coated on the base film, the base film is divided into two to obtain two third film materials.

[0103] In the above step S6, two sheets of the third film material are unwound in a roll-to-roll manner, with the interface management layer facing the negative electrode sheet, and hot-pressed composite is performed, so that the third film material is composited on both sides of the negative electrode sheet. The negative electrode sheet can be composed of a negative electrode current collector and a negative electrode active material layer. The negative electrode current collector material can include any one of aluminum, copper, nickel, and zinc, or a combination of at least two, preferably copper; the negative electrode active material in the negative electrode active material layer can include carbon material, lithium metal or lithium alloy, and the lithium alloy can be one of aluminum-lithium alloy, lithium-tin alloy, lithium-lead alloy, and lithium-silicon alloy.

[0104] In the above step S8, the specific steps of coating the short-circuit-proof ceramic oxide are as follows:

[0105] The battery cell is immersed in the anti-short circuit coating solution for 3 to 10 seconds, then taken out and dried; or the anti-short circuit coating solution is sprayed on the outer edge of the battery cell, and then dried.

[0106] In the above method, the anti-short circuit coating solution is obtained by adding conductive high molecular polymer, nano-silicon dioxide particles, nano-alumina particles and conductive agent into an organic solvent according to a proportion and stirring evenly; wherein the organic solvent can be selected from commonly used organic solvents that can dissolve high molecular polymers, including but not limited to acetone.

[0107] In some embodiments of the present invention, the anti-short circuit coating solution includes the following components by mass percentage: 1% to 6% of conductive polymer, 2% to 4% of nano-silicon dioxide particles, 1% to 3% of nano-aluminum oxide particles, and the remainder of organic solvent. Among them, the mass percentage of the conductive polymer is 1% to 6%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, etc.; the mass percentage of the nano-silicon dioxide particles is 2% to 4%, for example, it can be 2%, 2.5%, 3%, 3.5%, 4%, etc.; the mass percentage of the nano-aluminum oxide particles is 1% to 3%, for example, it can be 1%, 2%, 3%, etc.

[0108] In a preferred embodiment of the present invention, the anti-short circuit coating solution includes the following components by mass percentage: 2% to 5% polyvinylidene fluoride, 2% to 4% nano-silicon dioxide particles, 1% to 2% nano-alumina particles, and the balance acetone. A further preferred composition is: 3% polyvinylidene fluoride, 2% nano-silicon dioxide particles, 1% nano-alumina particles, and 94% acetone.

[0109] The present invention will be further described below in conjunction with specific embodiments.

[0110] In the following examples, the LALZO used has a D50 particle size of 100-200 nm and a specific surface area of ​​>10 m 2 / g, ionic conductivity ≥0.6mS / cm.

[0111] Example 1

[0112] The present embodiment provides a solid electrolyte all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide, and its design scheme is shown in Table 1, wherein the active material of the positive electrode is LiFePO4 with a content of 93%, the active material of the negative electrode is Li with a content of 80%, and the battery capacity is 3500Ah.

[0113] Table 1 Design of the battery in Example 1

[0114]

[0115] The preparation method of the solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte of this embodiment is as follows:

[0116] 1. Preparation of solid electrolyte membrane containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide

[0117] S1. Preparation of solid electrolyte interface wetting modification layer slurry and solid electrolyte layer slurry containing conductive polymer composite 3D spherical graphene aluminum doped lithium zirconium oxygen

[0118] PVDF, nano-SiO2, nano-Al2O3, super-p Li, Ketjen Black ECP-600JD, and VGCF are added to acetone, heated and stirred evenly to obtain a solid electrolyte interface wetting modification layer slurry; in the slurry, the mass percentage of each component is: PVDF 3%, nano-SiO2 3%, nano-Al2O3 1%, super-p Li 2%, Ketjen Black ECP-600JD 0.5%, VGCF0.5%, and acetone 91%.

[0119] PVDF, 3D spherical graphene, LALZO, nano-SiO2, and VGCF are added to acetone, heated and stirred evenly to obtain a solid electrolyte layer slurry; in the slurry, the mass percentage of each component is: PVDF 4%, LALZO 68.5%, 3D spherical graphene 1%, nano-SiO2 1%, VGCF 0.5%, and acetone 25%.

[0120] S2. The solid electrolyte interface wetting modification layer slurry is coated on a PET film with a length of 200 m by a coating machine, and an interface wetting modification layer with a thickness of 1.5 μm is obtained after curing; and then the PET film is cut from the middle into two first film materials with a length of 100 m.

[0121] S3. Take a piece of the first film material, and use a coating machine to coat the solid electrolyte layer slurry containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide on the solid electrolyte interface wetting modification layer, and after curing, obtain a solid electrolyte layer with a thickness of 8 μm, which is called the second film material.

[0122] S4. Unwind another first film material and a second film material in a roll-to-roll manner, so that the solid electrolyte interface wetting modification layer of the first film material is opposite to the solid electrolyte layer of the second film material. Then the first film material and the second film material are hot-pressed and laminated by a hot-pressing laminating machine, and the temperature of the hot-pressing and laminating is 150°C. Then, one of the PET films is peeled off to obtain a solid electrolyte membrane containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide.

[0123] 2. Preparation of positive electrode sheet containing conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane

[0124] S5. According to the mass ratio of 93:4:3, the positive electrode active material LiFePO4, conductive carbon black and adhesive material PVDF are added to the N-methylpyrrolidone solution and mixed to obtain a positive electrode active layer slurry with a solid content of 52% and a viscosity of 8600mPa·s; then the positive electrode active layer slurry is coated on the outer surface of the aluminum foil by a coating machine and dried to obtain a LiFePO4 positive electrode sheet.

[0125] S6. Unwind two solid electrolyte membranes containing conductive polymer composite 3D spherical graphene aluminum doped lithium zirconium oxide in a roll-to-roll manner, and then transfer them to both sides of the positive electrode sheet by hot pressing and compounding, and the temperature of hot pressing and compounding is 150° C. Then cut out the positive electrode tabs, peel off the PET film, and then cut into specifications of 800mm×1600mm, so as to manufacture a positive electrode sheet containing conductive polymer composite 3D spherical graphene aluminum doped lithium zirconium oxide solid electrolyte membrane for standby use.

[0126] 3. Preparation of negative electrode sheet containing interface management layer

[0127] S7. The metallic lithium is rolled into a lithium film with a thickness of 10 μm by a press, and then the lithium film is composited on both sides of a copper foil or a copper mesh to form a negative electrode film.

[0128] S8. Add PVDF, PMMA, nano-SiO2, nano-Al2O3, and super-p Li into acetone, heat and stir evenly to obtain a negative electrode interface management layer slurry; in the slurry, the mass percentage of each component is: PVDF 2%, PMMA 3%, nano-SiO2 2%, nano-Al2O3 1%, super-p Li 1%, and acetone 91%.

[0129] S9. The interface management layer slurry is coated on a PET film with a length of 100 m by a coating machine, and after curing, an interface management layer with a thickness of 1.5 μm is obtained; and then the PET film is cut from the middle into two third films with a length of 100 m.

[0130] S10. Unwind two sheets of the third film material in a roll-to-roll manner, and then transfer them to both sides of the lithium negative electrode film by hot pressing and laminating, and the temperature of hot pressing and laminating is 150° C. Then cut out the negative electrode tabs, peel off the PET film, and then cut into a specification of 800mm×1600mm, so as to manufacture a negative electrode sheet containing an interface management layer for standby use.

[0131] 4. Battery assembly stacking

[0132] S11. Alternately stack the positive electrode sheet containing the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte membrane and the negative electrode sheet containing the interface management layer, and then shape and fix them into an integral battery cell.

[0133] 5. Anti-short circuit ceramic oxide coating

[0134] S12. Add PVDF, nano-SiO2, and nano-Al2O3 to acetone, heat and stir evenly to obtain an anti-short circuit coating solution; in the solution, the mass percentage of each component is: PVDF 3%, nano-SiO2 2%, nano-Al2O3 1%, and acetone 94%.

[0135] S13. Place the prepared battery cell in an anti-short circuit coating solution, soak for 10 seconds, seal the outer edge of the battery cell, and then dry it.

[0136] 6. Battery cell assembly and packaging

[0137] S14. After the short-circuit-proof ceramic oxide is coated with an aluminum-plastic film, drying, electrolyte activation, formation, polymerization, and capacity separation are performed in sequence to obtain a finished all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide. The nominal capacity of the all-solid-state battery is 3500Ah.

[0138] Battery performance test

[0139] 1. Gram capacity

[0140] The all-solid-state battery of Example 1 was charged and discharged at a rate of 1C, and the first-week discharge capacity, positive electrode gram capacity and first efficiency of the all-solid-state battery were tested. The results are shown in Table 2.

[0141] Table 2

[0142] 1C discharge capacity (mAh) 1C positive electrode gram capacity (mAh / g) First efficiency (%) 3560 145 95

[0143] As shown in the results of Table 2, the LiFePO4 all-solid-state battery of the present invention has a positive electrode capacity of 145 mAh / g and has a relatively high energy density.

[0144] 2. Rate performance

[0145] The all-solid-state battery prepared in Example 1 was tested for rate discharge performance. The results are shown in Table 3 and Figure 4 shown.

[0146] Table 3 Rate discharge test results of the all-solid-state battery of Example 1

[0147] magnification 1C 2C 3C 5C Capacity(Ah) 3560 3498 3475 3463 Capacity retention rate / 98.3% 97.6% 97.2%

[0148] See Table 3 and Figure 4 At discharge rates of 1C, 2C, 3C and 5C, the all-solid-state battery maintained a relatively high capacity retention rate, that is, the all-solid-state battery of this embodiment had a small capacity difference when discharged at different rates and had good rate discharge performance.

[0149] 3. Normal temperature cycle performance

[0150] The all-solid-state battery prepared in Example 1 was discharged at a rate of 1C at room temperature for 1500 cycles and the capacity of the lithium battery at each cycle was detected. The voltage value and capacity value were recorded and a relationship curve between the capacity and the number of cycles was plotted. The results are shown in Table 4.

[0151] Table 4 All-solid-state room temperature cycle performance test results of Example 1

[0152] Weekly 100 300 500 1000 1500 Capacity retention rate 101.2% 98.3% 96.8% 95.5% 93.6%

[0153] It can be seen from Table 4 that the all-solid-state battery still maintains a high capacity retention rate after 1500 cycles, indicating that the all-solid-state battery of the present invention has good room temperature cycle performance.

[0154] 4. High temperature performance

[0155] The all-solid-state battery prepared in Example 1 was stored at room temperature for 28 days after standard charging. The initial capacity was obtained by standard discharge test at a rate of 0.2C. The recovery capacity was obtained by standard charge and discharge test after standing for 30 minutes. The capacity after storage was obtained by standard charge and discharge test after storage at 60°C for 7 days. The test results are shown in Table 5.

[0156] Table 5 Performance comparison of the all-solid-state battery of Example 1 before and after storage at 60°C for 7 days

[0157]

[0158] It can be seen from Table 5 that the all-solid-state battery of the present invention has good high-temperature performance.

[0159] The all-solid-state battery prepared in Example 1 was cycled for 1500 cycles at 60°C and a rate of 1C, and its capacity retention rate was detected and recorded. The results are shown in Table 6.

[0160] Table 6 High temperature cycle performance test results of the all-solid-state battery of Example 1

[0161] Weekly 100 300 500 1000 1500 Capacity retention rate 98.2% 96.0% 93.8% 90.2% 88.7%

[0162] It can be seen from Table 6 that the all-solid-state battery prepared in Example 1 has a lower cycle performance at 60°C than at room temperature, but still has good cycle performance at 60°C, that is, the all-solid-state battery can be used in a high temperature environment for a long time.

[0163] 5. Low temperature performance

[0164] The all-solid-state battery of Example 1 was placed in an environment of 25°C and -20°C, respectively, and discharged at a rate of 0.2C after 2 hours to detect the capacity of the full battery, and the voltage and capacity retention rate data were recorded, wherein the battery capacity at 25°C, i.e., 3547Ah, was used as the standard capacity value of the capacity retention rate. The full battery capacity at different temperatures is shown in Table 7.

[0165] Table 7 Comparison of 0.2C discharge performance of all-solid-state batteries of Example 1 at room temperature and low temperature

[0166] Temperature(℃) 25 -20 Capacity(Ah) 3547 2276 Capacity retention rate / 64.1%

[0167] It can be seen from Table 7 that the capacity of the all-solid-state battery in this embodiment at low temperature is significantly reduced compared to normal temperature. It can be used in low temperature environment for a short period of time, but the performance is significantly reduced.

[0168] Example 2

[0169] Example 2 provides an all-solid-state battery, the design of which is shown in Table 8, wherein the active material of the positive electrode is NaFePO4 with a content of 95.5%, the active material of the negative electrode is Li with a content of 80%, and the battery capacity is 2500Ah.

[0170] Table 8 Design of the battery in Example 2

[0171]

[0172] The battery preparation process of this embodiment is the same as that of embodiment 1, except that the preparation process of the positive electrode sheet is:

[0173] According to the mass ratio of 95.5:2.5:2, the positive electrode active material sodium iron phosphate, conductive carbon black and adhesive material PVDF were added to the N-methylpyrrolidone solution and mixed to obtain the positive electrode active layer slurry with a solid content of 55% and a viscosity of 4500mPa·s. The positive electrode active layer slurry was then coated on the outer surface of the aluminum foil with a coating machine and dried to obtain the NaFePO4 positive electrode sheet.

[0174] Battery performance test

[0175] 1. Gram capacity

[0176] The all-solid-state battery in Example 2 was charged and discharged at a rate of 0.2C, and the battery's first-week discharge capacity, positive electrode gram capacity, and first efficiency were tested. The results are shown in Table 9.

[0177] Table 9

[0178] 0.2C discharge capacity (mAh) Positive electrode capacity (mAh / g) First efficiency (%) 2545 105 92

[0179] As shown in the results of Table 9, the positive electrode capacity of the NaFePO4 solid-state full battery of this embodiment reaches 105 mAh / g, which has a relatively high energy density.

[0180] Figure 5 The first cycle charge and discharge curve of the NaFePO4 solid-state full battery is shown.

[0181] 2. Rate performance

[0182] The all-solid-state battery prepared in Example 2 was tested for rate discharge performance, and the results are shown in Table 10.

[0183] Table 10 Rate discharge test results of the all-solid-state battery of Example 2

[0184] magnification 0.5C 1C 2C Capacity(Ah) 2542 2508 2495 Capacity retention rate / 98.7% 98.2%

[0185] Please refer to Table 10. At discharge rates of 0.5C, 1C, and 2C, the all-solid-state batteries maintained a relatively high capacity retention rate, that is, the all-solid-state battery of this embodiment has a small capacity difference when discharged at different rates and has good rate discharge performance.

[0186] 3. Normal temperature cycle performance

[0187] The all-solid-state battery prepared in Example 2 was discharged at a rate of 0.5C at room temperature for 1000 cycles and the capacity of the battery at each cycle was detected. The voltage value and capacity value were recorded and a relationship curve between the capacity and the number of cycles was plotted. The results are shown in Table 11.

[0188] Table 11 All-solid-state room temperature cycle performance test results of Example 2

[0189] Weekly 100 300 500 1000 Capacity retention rate 99.4% 95.1% 92.8% 87.5%

[0190] It can be seen from Table 11 that the all-solid-state battery still maintains a high capacity retention rate after 1000 cycles, indicating that the all-solid-state battery of the present invention has good room temperature cycle performance.

[0191] 4. High temperature performance

[0192] The all-solid-state battery prepared in Example 2 was stored at room temperature for 28 days after standard charging. The initial capacity was obtained by standard discharge test at a rate of 0.5C. The recovery capacity was obtained by standard charge and discharge test after standing for 30 minutes. The post-storage capacity was obtained by standard charge and discharge test after storage at 55°C for 7 days. The test results are shown in Table 12.

[0193] Table 12 Performance comparison of the all-solid-state battery of Example 2 before and after storage at 55°C for 7 days

[0194]

[0195] It can be seen from Table 12 that the all-solid-state battery of the present invention has good high-temperature performance.

[0196] The all-solid-state battery prepared in Example 2 was cycled for 1000 cycles at 55°C and a rate of 0.5C, and its capacity retention rate was detected and recorded. The results are shown in Table 13.

[0197] Table 13 High temperature cycle performance test results of the all-solid-state battery of Example 2

[0198] Weekly 100 300 500 1000 Capacity retention rate 98.4% 94.7% 90.1% 85.3%

[0199] It can be seen from Table 13 that the all-solid-state battery prepared in Example 1 has a lower cycle performance at 55°C than at room temperature, but still has good cycle performance at 55°C, that is, the all-solid-state battery can be used in a high temperature environment for a long time.

[0200] 5. Low temperature performance

[0201] The all-solid-state battery of Example 2 was placed in an environment of 25°C and -20°C, respectively, and discharged at a rate of 0.5C after 2 hours to detect the capacity of the full battery, and the voltage and capacity retention rate data were recorded, wherein the battery capacity at 25°C, i.e., 2536Ah, was used as the standard capacity value of the capacity retention rate. The full battery capacity at different temperatures is shown in Table 14.

[0202] Table 14 Comparison of 0.2C discharge performance of all-solid-state batteries of Example 2 at room temperature and low temperature

[0203] Temperature(℃) 25 -20 Capacity(Ah) 2536 2098 Capacity retention rate / 82.7%

[0204] It can be seen from Table 14 that the capacity of the all-solid-state battery in this embodiment at low temperature is significantly reduced compared to normal temperature. It can be used in low temperature environment for a short period of time, but the performance is significantly reduced.

[0205] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for manufacturing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte membrane, characterized in that: The following steps are involved: S1. The solid electrolyte interface infiltration modification layer slurry is coated on a base film, and after curing, a solid electrolyte interface infiltration modification layer is formed to obtain a first film material; S2. The 3D-type spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte slurry is coated on the solid electrolyte interface wetting modification layer of the first film, and after curing, a 3D-type spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte layer is formed to obtain a second film; S3. The first film material and the second film material are hot-pressed and composited, and then one of the base films is peeled off to obtain the conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane.

2. The method for manufacturing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium-oxygen solid electrolyte membrane according to claim 1, characterized in that: In step S1, the solid electrolyte interface wetting modification layer slurry contains the following components by mass percentage: 2% to 5% conductive polymer, 0.5% to 3% nano-alumina particles, 1% to 5% nano-silicon dioxide particles, 2% to 8% conductive agent, and the balance organic solvent; and / or, The thickness of the solid electrolyte interface wetting modification layer is 1 to 3 μm; and / or, The base film includes a PET film.

3. The method for manufacturing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium-oxygen solid electrolyte membrane according to claim 1, characterized in that: In step S2, the 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer slurry contains the following components by mass percentage: 2% to 8% conductive polymer, 62% to 70% solid electrolyte, 0.5% to 5% 3D spherical graphene, 0.1% to 3% conductive agent, 1% to 5% nano-silicon dioxide particles, and the remainder organic solvent; and / or, The thickness of the 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer is 5 to 15 μm.

4. The method for manufacturing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium-oxygen solid electrolyte membrane according to claim 2 or 3, characterized in that: The conductive high molecular polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, and polymethyl methacrylate; and / or, The solid electrolyte comprises at least one of LLZO, LALZO and LATP; and / or, The particle size of the nano-alumina particles and the nano-silicon dioxide particles is 10 to 100 nm; and / or, The conductive agent includes at least one of carbon nanofibers, carbon nanotubes, graphene, conductive carbon black, and conductive graphite; and / or, The diameter of the 3D spherical graphene is 2-9 nm, and the tap density is 0.5-0.8 g / cm 3 , with a specific surface area of ​​5000-6000m 2 / g, the resistivity is (9~12)×10 -6 Ω.

5. The method for manufacturing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium-oxygen solid electrolyte membrane according to claim 2 or 3, characterized in that: The mass percentage of each component in the solid electrolyte interface wetting modification layer slurry is: polyvinylidene fluoride 2% to 4%, nano silicon dioxide particles 2.5% to 3%, nano alumina particles 0.5% to 1%, super-P Li 1.5% to 2.5%, Ketjen black ECP-600JD 0.5% to 1%, VGCF 0.5% to 1%, and the balance acetone; and / or, In the 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte layer slurry, the mass percentage of each component is: polyvinylidene fluoride 3% to 5%, LALZO 65% to 70%, 3D spherical graphene 0.5% to 1%, VGCF 0.4 to 0.8%, nano-silicon dioxide particles 1% to 2%, and the balance acetone.

6. The method for manufacturing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium-oxygen solid electrolyte membrane according to claim 2 or 3, characterized in that: In step S3, the temperature of the hot pressing compound is 120-180°C.

7. A method for manufacturing an all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte membrane, characterized in that: The following steps are involved: a. The two solid electrolyte membranes are hot-pressed and composited on both sides of the positive electrode sheet, and then the base film is removed and the positive electrode ear is cut out to obtain a positive electrode sheet containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane; b. coating the interface management layer slurry on a base film, and curing to form an interface management layer to obtain a third film material; c. hot-pressing two sheets of the third film material onto both sides of the negative electrode sheet, then removing the base film, cutting out the negative electrode tabs, and obtaining a negative electrode sheet containing an interface management layer; d. The plurality of positive electrodes containing the conductive polymer composite 3D-like spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane and the plurality of negative electrodes containing the interface management layer are alternately stacked and fixed in a stacked manner to obtain a battery cell; e. Coating the outer edge of the battery with anti-short-circuit ceramic oxide; f. The cells are sequentially packaged, dried, activated by electrolyte, formed and divided to obtain an all-solid-state battery containing a conductive polymer composite 3D-like spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane; Wherein, in step a, the solid electrolyte membrane is a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte membrane prepared by the method described in any one of claims 1 to 6.

8. The method for preparing an all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane according to claim 7, characterized in that: In step b, the interface management layer slurry contains the following components by mass percentage: 2% to 8% conductive polymer, 1% to 4% nano silicon dioxide particles, 0.5% to 3% nano aluminum oxide particles, 0.5% to 2% conductive agent, and the balance organic solvent; and / or, The interface management layer slurry comprises the following components by mass percentage: 1.5% to 2% polyvinylidene fluoride, 2% to 4% polymethyl methacrylate, 1.5% to 2.5% nano silicon dioxide particles, 0.5% to 1.5% nano aluminum oxide particles, 0.5% to 1% super-PLi, and the balance acetone; and / or, The thickness of the interface management layer is 1-2 μm.

9. The method for preparing an all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane according to claim 7, characterized in that: In step e, the method of coating the short-circuit-proof ceramic oxide comprises: Immerse the battery cell in an anti-short circuit coating solution for 3 to 10 seconds, then take it out and dry it; or spray the anti-short circuit coating solution on the outer edge of the battery cell, and then dry it; Wherein, the anti-short circuit coating solution comprises the following components by mass percentage: 1% to 6% of conductive polymer, 1% to 5% of nano silicon dioxide particles, 1% to 3% of nano aluminum oxide particles, and the balance of organic solvent; and / or, The anti-short circuit coating solution comprises the following components by mass percentage: 2% to 5% of polyvinylidene fluoride, 2% to 4% of nano silicon dioxide particles, 1% to 2% of nano aluminum oxide particles, and the balance of acetone.

10. An all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxide solid electrolyte membrane, characterized in that: The all-solid-state battery containing a conductive polymer composite 3D spherical graphene aluminum-doped lithium zirconium oxygen solid electrolyte membrane is prepared by the method described in any one of claims 7 to 9.

Citation Information

Patent Citations

  • Preparation method of electrode based on double-conductive passivation layer

    CN116053597A

  • All-solid-state battery and preparation method thereof

    CN116525955A

  • Garnet type oxide solid electrolyte, preparation method and application thereof

    CN116683021A

  • Solid electrolyte slurry, composite current collector and secondary battery

    CN117747928A

Cited By

  • Sulfide composite electrolyte and preparation method and application thereof

    CN119650822A

  • A sulfide composite electrolyte and its preparation method and application

    CN119650822B

  • Lithium-loving elastic electrolyte, preparation method thereof and solid-state lithium metal battery

    CN120127213A

  • Novel all-solid-state thin film lithium battery and preparation method thereof

    CN120511340A

  • All-solid-state battery, preparation method thereof and electric device

    CN121748499A