Sulfur-doped halide solid electrolyte, preparation method thereof and application of sulfur-doped halide solid electrolyte in all-solid-state battery

Through the ball milling and cold pressing preparation methods of sulfur-doped halide solid-state electrolytes, the problems of low ionic conductivity and instability of halide electrolytes are solved, and the performance and stability of all-solid-state batteries are improved.

CN118782894APending Publication Date: 2024-10-15TIANJIN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411084793.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing halide solid-state electrolytes have low room temperature ionic conductivity and are unstable with lithium metal anodes, resulting in insufficient all-solid-state battery performance.

Method used

Using sulfur-doped halide solid-state electrolyte, the chemical formula is Li2+aMX6-aSa or Li3+aMX6-aSa, where M includes Zr, Er, Y, In or Sc, and X includes F, Cl, Br, I, through ball milling and cooling The pressure preparation method improves its ionic conductivity and stability.

Benefits of technology

It increases the room temperature ionic conductivity to nearly 1mS/cm, enhances the interface stability of lithium metal anode, and significantly improves the cycle stability and performance of all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782894A_ABST
    Figure CN118782894A_ABST
Patent Text Reader

Abstract

The invention discloses a sulfur-doped halide solid electrolyte, a preparation method thereof and application of the sulfur-doped halide solid electrolyte in an all-solid-state battery, and belongs to the technical field of all-solid-state lithium metal batteries. According to the invention, the heterovalent sulfur element is introduced into the ternary halide electrolyte, and a new crystal structure is induced and generated on the basis of an original phase structure, so that the ionic conductivity of the ternary halide electrolyte is improved; meanwhile, due to the introduction of the sulfur element, the interface stability of the halide electrolyte and the lithium metal negative electrode is improved. The ionic conductivity of the electrolyte at room temperature is close to 1mS / cm, the basic requirements of the electrolyte in practical application are met, and the modified halide electrolyte has good cycle stability when being applied to an all-solid-state lithium metal battery. The halide electrolyte prepared by the method disclosed by the invention is simple to operate and beneficial to expanded production, and has a relatively great application prospect in all-solid-state lithium metal batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of all-solid-state batteries, and in particular relates to a sulfur-doped halide solid electrolyte and a preparation method thereof and an application thereof in an all-solid-state battery. Background Art

[0002] In order to adapt to the development strategy of the new energy industry and the country, lithium-ion batteries are developing in the direction of high specific energy, long life and high safety. Due to the high risk of electrothermal runaway of traditional liquid lithium-ion batteries, accidents caused by the combustion and explosion of lithium batteries occur frequently every year. Therefore, safety issues have become a bottleneck restricting the development of high specific energy liquid lithium batteries. All-solid-state batteries use non-flammable, non-leaking solid electrolytes instead of organic electrolytes to improve the safety of lithium batteries. At the same time, all-solid-state batteries can be matched with lithium metal negative electrodes, which can provide higher energy density while being safe. Solid electrolytes, as one of the key materials for all-solid-state batteries, are mainly divided into polymer electrolytes, inorganic solid electrolytes and composite solid electrolytes. Compared with the other two types, inorganic solid electrolytes are expected to become ideal solid electrolyte materials due to their higher room temperature ionic conductivity, mechanical strength and high-voltage stability.

[0003] At present, the research on inorganic solid electrolytes is mainly focused on sulfide, oxide, halide and other material systems. Among them, halide electrolytes, as an emerging solid electrolyte in recent years, have the following advantages: high room temperature ionic conductivity, wide electrochemical window, stability to high-voltage oxide positive electrode materials, and the raw materials required for their synthesis are cost-effective, the synthesis process is simple, and they are easy to mass produce.

[0004] However, the ionic conductivity of most halide electrolytes is lower than that of liquid electrolytes (10 -2 S / cm) is still low. To further improve the performance of all-solid-state batteries, faster lithium ion transport is needed. Secondly, most halide solid electrolytes are unstable when in direct contact with lithium metal anodes. The central non-lithium metal elements are easily reduced by lithium metal into conductive byproducts, which accelerates the failure of the battery. Therefore, it is often necessary to add an intermediate layer to separate the halide solid electrolyte and the lithium metal anode or lithium alloy anode. Therefore, it is necessary to develop halide solid electrolyte materials with higher ionic conductivity and stable contact with lithium metal anode to improve battery performance.

[0005] In order to solve the above problems existing in the prior art, we propose a sulfur-doped halide solid electrolyte and a preparation method thereof and application in an all-solid-state battery. Summary of the invention

[0006] The present invention provides a sulfur-doped halide solid electrolyte, aiming to solve the problems of low ion conductivity and unstable lithium metal negative electrode of the existing halide solid electrolyte at room temperature.

[0007] To achieve the above object, the present invention provides the following technical solution: a sulfur-doped halide solid electrolyte, the chemical formula of the solid electrolyte is: Li 2+a MX 6-a S a or Li 3+a MX 6-a S a , wherein M includes at least one element selected from Zr, Er, Y, In or Sc, X includes at least one element selected from F, Cl, Br, I, and 0<a≤1.

[0009] Preferably, when 0<a<0.25, the halide includes a first crystalline phase, and the space group is P m1; when 0.25≤a<0.5, the halide includes a first crystal phase and a second crystal phase, and the second crystal phase space group is C2 / m; when 0.5≤a≤1, the halide electrolyte includes only the second crystal phase, and Li 2 The diffraction peak of S.

[0010] Preferably, M is selected as Zr, X is selected as Cl, and 0.25≤a<0.5.

[0011] The present invention also provides a method for preparing the above-mentioned sulfur-doped halide solid electrolyte, comprising the following steps:

[0012] S1. In an inert gas, weigh the precursors LiX and MX according to the stoichiometric ratio. b , wherein b=3 or 4, to obtain a halide mixture powder without adding a sulfur source;

[0013] S2. According to the doping amount a, weigh different masses of sulfur source Li 2 S is added to the mixed powder, and the mixture is manually ground in an agate mortar for 20 to 60 minutes to obtain a uniform mixed powder with fine particles;

[0014] S3, weighing zirconia ball milling beads of different sizes, transferring the ball milling beads and the mixed powder into a zirconia ball milling jar, and then placing them on a planetary ball mill for ball milling;

[0015] S4. After the ball milling is completed, the ball milling tank is opened in the glove box, and the synthesized halide solid electrolyte and the ball milling beads are separated and stored in the glove box for subsequent testing;

[0016] S5. Weigh a certain mass of the above sulfur-doped halide electrolyte powder, pour it into a stainless steel mold for cold pressing, and obtain a sulfur-doped halide solid electrolyte sheet.

[0017] Preferably, the size of the zirconia ball milling beads weighed in step S3 includes one or more of 3 mm, 5 mm, 7 mm and 10 mm, the ball-to-material ratio is (20-60):1, the ball milling speed is 500-800 rpm, the ball milling time is 6-24 h, each operation is 60 min and rest is 5 min.

[0018] Preferably, the colors of the series of mixtures obtained in step S4 change from original white to gradually darker yellow as the doping amount a increases.

[0019] Preferably, the specific process of step S5 is: weighing 150-200 mg of sulfur-doped halide electrolyte and putting it into a stainless steel mold with a diameter of 10 mm, and applying a pressure of 380 MPa for 1 min to obtain a sulfur-doped halide solid electrolyte sheet with a thickness of 1-1.5 mm.

[0020] Preferably, all the above steps are carried out in a glove box, and the water content in the glove box is less than 0.1 ppm, and the oxygen content is less than 0.1 ppm.

[0021] The present invention also provides application of the sulfur-doped halide solid electrolyte in an all-solid-state battery.

[0022] The present invention also provides an all-solid-state battery, the all-solid-state battery comprising a high-voltage oxide positive electrode, an alloy negative electrode, and a solid electrolyte, the solid electrolyte comprising a halide solid electrolyte and a sulfide electrolyte layer, the halide solid electrolyte comprising the sulfur-doped halide solid electrolyte material according to any one of claims 1 to 3, the sulfide electrolyte layer comprising Li 6 PS 5 Cl or Li 10 GP 2 S 12 The alloy negative electrode is selected from one of lithium-indium alloy, lithium-magnesium alloy or lithium-aluminum alloy.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention provides a halide solid electrolyte doped with heterovalent anions, wherein Li 2 MX 6 or Li 3 MX 6As a base, a divalent S element is doped thereon, wherein M includes at least one element selected from Zr, Er, Y, In or Sc, and X includes at least one element selected from F, Cl, Br, and I. Halide solid electrolytes doped with halogen elements of the same family have been reported, but halide solid electrolytes doped with heterovalent elements are rarely reported.

[0025] (2) The present invention obtains a Li 2+a MX 6-a S a or Li 3+a MX 6-a S a A sulfur-doped halide solid electrolyte, where 0<a≤1; by introducing an alivalent S element, a second phase crystal structure is induced on the basis of the original phase structure, thereby improving its ionic conductivity; the ionic conductivity at room temperature is close to 1mS / cm, which meets the basic requirements for the application of all-solid-state electrolytes; at the same time, the introduction of sulfur elements improves the interface stability between the halide electrolyte and the lithium metal negative electrode, and the all-solid-state battery assembled using this electrolyte shows good cycle stability.

[0026] (3) The sulfur-doped halide solid electrolyte provided by the present invention has adjustable composition, uses low-cost raw materials, and has application prospects for large-scale production of the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 XRD diffraction patterns of the halide solid electrolytes prepared in Examples 1 to 7 and Comparative Example 4 of the present invention;

[0028] Figure 2 Electrochemical impedance spectra of the halide solid electrolyte sheets prepared in Examples 1 to 7 of the present invention and Comparative Example 4;

[0029] Figure 3 Li prepared in Comparative Example 1 of the present invention 3.25 InCl 5.75 S 0.25 XRD diffraction pattern of halide solid electrolyte;

[0030] Figure 4 Li prepared in Comparative Example 1 of the present invention 3.25 InCl 5.75 S 0.25 Electrochemical impedance spectroscopy of halide solid electrolytes;

[0031] Figure 5 Li prepared in Comparative Example 2 of the present invention 3.25 E 5.75 S 0.25Electrochemical impedance spectroscopy of halide solid electrolytes;

[0032] Figure 6 Li prepared in Comparative Example 3 of the present invention 2 ZrCl 5.75 I 0.25 Electrochemical impedance spectroscopy of halide solid electrolytes;

[0033] Figure 7 Li prepared in Comparative Example 4 of the present invention 2 ZrCl 6 Electrochemical impedance spectroscopy of halide solid electrolytes;

[0034] Figure 8 The halide solid electrolyte prepared in Example 2 of the present invention is assembled with LiCoO 2 The charge and discharge curve of the all-solid-state battery with positive electrode at room temperature at 0.1C;

[0035] Fig. 9 The charge and discharge curve of the all-solid-state battery assembled with the halide solid electrolyte prepared in Example 2 of the present invention and using NCM811 as the positive electrode at room temperature at 0.1C;

[0036] Fig.10 Li prepared in Comparative Example 4 2 ZrCl 6 Cycling performance diagram of lithium symmetric battery assembled with solid electrolyte sheets at different current densities;

[0037] Fig.11 Li prepared in Example 2 2.25 ZrCl 5.75 S 0.25 Cycling performance diagram of lithium symmetric battery assembled with solid electrolyte sheets at different current densities. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with specific examples and comparative examples, which are provided only to illustrate the present invention, but not to limit the scope of the present invention. The experimental methods in the following examples are conventional methods unless otherwise specified; the materials, reagents, instruments, etc. used are all commercially available unless otherwise specified.

[0039] Example 1

[0040] A sulfur-doped halide solid electrolyte, the preparation method is as follows:

[0041] S1. In an inert gas, weigh the precursors LiCl and ZrCl according to the stoichiometric ratio. 4 , obtaining a halide mixture powder without adding a sulfur source;

[0042] S2. Weigh Li with a doping amount of a=0.1 2 S was added to the above mixture with a total mass of 2 g, and ground manually in an agate mortar for 30 min to obtain a uniform mixed powder with fine particles;

[0043] S3, weigh 80 g of 3 mm, 5 mm and 10 mm zirconium oxide ball milling beads, transfer the ball milling beads and the mixed powder into a ball milling jar, and then place them on a planetary ball mill for ball milling;

[0044] S4. After the ball milling is completed, the ball milling tank is opened in the glove box to separate the synthesized halide solid electrolyte and the ball milling beads. The obtained electrolyte chemical formula is Li 2.1 ZrCl 5.9 S 0.1 , and stored in the glove box for subsequent testing;

[0045] S5. Weigh a certain mass of the synthesized halide electrolyte powder, pour it into a 10 mm stainless steel mold, apply a pressure of 380 MPa for cold pressing, hold the pressure for 1 minute, and then take it out to obtain a solid electrolyte sheet with a thickness of 1.2 mm.

[0046] The halide solid electrolyte obtained in Example 1 was subjected to XRD test to analyze its crystal structure. Figure 1 As shown, the XRD diffraction peaks can be well matched with Li 2 ZrCl 6 The standard card corresponds to the space group P3m1, but compared to Li 2 ZrCl 6 The peaks of the carbon nanotubes shift to smaller angles to a certain extent, indicating the successful incorporation of sulfur atoms with larger atomic radius.

[0047] Example 2

[0048] The preparation method of this embodiment is the same as that of embodiment 1, except that the doping amount is a=0.25, and the obtained electrolyte chemical formula is Li 2.25 ZrCl 5.75 S 0.25 .

[0049] The halide solid electrolyte obtained in Example 2 was subjected to XRD test to analyze its crystal structure. Figure 1 As shown, the XRD diffraction peaks can be well matched with Li 2 ZrCl 6The XRD diffraction peaks of Example 1 are slightly different from those of the standard card, but compared with those of Example 1, they are shifted to smaller angles to a certain extent, and the intensities of the diffraction peaks at 2θ=30.3° and 34.7° increase, while the diffraction peak intensity at 2θ=32.3° decreases, indicating that with the increase of sulfur doping content, a different Li 2 ZrCl 6 phase of the crystal structure, the diffraction peak of the second phase can be compared with Li 3 ScCl 6 Corresponding to the standard card, its space group is C2 / m.

[0050] Example 3

[0051] The preparation method of this embodiment is the same as that of embodiment 1, except that the doping amount is a=0.4, and the obtained electrolyte chemical formula is Li 2.4 ZrCl 5.6 S 0.4 .

[0052] The halide solid electrolyte obtained in Example 3 was subjected to XRD test to analyze its crystal structure. Figure 1 As shown, compared with Example 2, the diffraction peak of the second phase is further enhanced, indicating that with the increase of sulfur doping content, more and more second phases are generated and gradually replace the first phase.

[0053] Example 4

[0054] The preparation method of this embodiment is the same as that of embodiment 1, except that the doping amount is a=0.5, and the obtained electrolyte chemical formula is Li 2.5 ZrCl 5.5 S 0.5 .

[0055] The halide solid electrolyte obtained in Example 4 was subjected to XRD test to analyze its crystal structure. Figure 1 As shown, the diffraction peak of the first phase disappears, and only the diffraction peak of the second phase remains, indicating that only the second crystal phase exists in the physical phase at this time.

[0056] Example 5

[0057] The preparation method of this embodiment is the same as that of embodiment 1, except that the doping amount is a=0.65, and the obtained electrolyte chemical formula is Li 2.65 ZrCl 5.35 S 0.65 .

[0058] Example 6

[0059] The preparation method of this embodiment is the same as that of embodiment 1, except that the doping amount is a=0.8, and the obtained electrolyte chemical formula is Li 2.8 ZrCl5.2 S 0.8 .

[0060] Example 7

[0061] The preparation method of this embodiment is the same as that of embodiment 1, except that the doping amount is a=1, and the obtained electrolyte chemical formula is Li 3 ZrCl 5 S.

[0062] The halide solid electrolytes obtained in Examples 5-7 were subjected to XRD testing to analyze their crystal structures. Figure 1 As shown, when the doping amount a is greater than 0.5, only the second phase remains in the halide solid electrolyte.

[0063] In order to verify whether sulfur doping can also induce phase change in ternary halide solid electrolytes centered on other metal elements, we designed Comparative Examples 1 and 2:

[0064] Comparative Example 1

[0065] The preparation method of this embodiment is the same as that of embodiment 2, and the sulfur doping amount is a=0.25. The only difference is that LiCl and InCl are used as precursors. 3 The electrolyte chemical formula is Li 3.25 InCl 5.75 S 0.25 .

[0066] The halide solid electrolyte obtained in Comparative Example 1 was subjected to XRD test to analyze its crystal structure. Figure 3 As shown in the figure, after doping with alivalent sulfur, its XRD diffraction peaks can be well matched with the original Li 3 InCl 6 The results show that the diffraction peaks of the ternary halide solid electrolyte are not significantly different from those of the standard electrolyte, and no new diffraction peaks appear, indicating that no new phase is generated. This further proves that alivalent sulfur doping will not change the phase of the ternary halide solid electrolyte with trivalent indium as the central atom.

[0067] Comparative Example 2

[0068] The preparation method of this embodiment is the same as that of embodiment 2, and the sulfur doping amount is a=0.25. The only difference is that LiCl and ErCl are used as precursors, and the obtained electrolyte chemical formula is Li 3.25 E 5.75 S 0.25 .

[0069] In order to explore whether doping with halogen elements of the same group can also induce phase change in ternary halide solid electrolytes, we designed Comparative Example 3.

[0070] Comparative Example 3

[0071] The preparation method of this embodiment is the same as that of embodiment 2, except that LiI with a doping amount of a=0.25 is weighed in S2 and added to the above mixture to obtain an electrolyte with a chemical formula of Li 2 ZrCl 5.75 I 0.25 .

[0072] The halide solid electrolyte obtained in Comparative Example 3 was subjected to XRD test to analyze its crystal structure. Figure 6 As shown, under the same doping amount a = 0.25, its XRD diffraction peak is similar to Li 2 ZrCl 6 The results show that the diffraction peaks of the second phase correspond to the standard card, and no diffraction peaks of the second phase appear, indicating that halogen elements with the same valence will not change the crystal structure of the solid electrolyte after doping.

[0073] Comparative Example 4

[0074] This comparative example prepares an undoped original halide solid electrolyte, and the specific steps are as follows:

[0075] S1. In an inert gas, weigh the precursors LiCl and ZrCl according to the stoichiometric ratio. 4 , the total mass is 2g.

[0076] S2, manually grinding in an agate mortar for 30 min to obtain a uniform mixed powder with fine particles;

[0077] S3. Weigh 80 g of 3 mm, 5 mm and 10 mm zirconium oxide ball milling beads, transfer the ball milling beads and the mixture into a ball milling jar, and then place them on a planetary ball mill for ball milling.

[0078] S4. After the ball milling is completed, the ball milling tank is opened in the glove box to separate the synthesized halide solid electrolyte and the ball milling beads. The obtained electrolyte chemical formula is Li 2 ZrCl 6 , and kept in the glove box for subsequent testing.

[0079] S5. Weigh a certain mass of the synthesized halide electrolyte powder, pour it into a 10 mm stainless steel mold, apply a pressure of 380 MPa for cold pressing, hold the pressure for 1 minute, and then take it out to obtain a solid electrolyte sheet with a thickness of 1.2 mm.

[0080] The room temperature ionic conductivity of the halide solid electrolyte in each embodiment and comparative example was tested by the blocking electrode test method, the test frequency was 0.1Hz~1MHz, and the calculation formula was σ=d / (SR), where d is the thickness of the electrolyte, S is the area of ​​the electrolyte side contacting the blocking electrode, and R is the resistance obtained by the AC impedance test. For the room temperature ionic conductivity of each embodiment and comparative example, please refer to Figure 2 , Figure 4-Figure 7 , and Table 1.

[0081] Table 1 Room temperature ionic conductivity of each embodiment and comparative example

[0082] Example Solid electrolyte chemical formula Room temperature ionic conductivity (S / cm) Example 1 <![CDATA[Li 2.1 ZrCl 5.9 S 0.1 ]]> <![CDATA[6.37×10 -4 ]]> Example 2 <![CDATA[Li 2.25 ZrCl 5.75 S 0.25 ]]> <![CDATA[9.55×10 -4 ]]> Example 3 <![CDATA[Li 2.4 ZrCl 5.6 S 0.4 ]]> <![CDATA[5.97×10 -4 ]]> Example 4 <![CDATA[Li 2.5 ZrCl 5.5 S 0.5 ]]> <![CDATA[5.15×10 -4 ]]> Example 5 <![CDATA[Li 2.65 ZrCl 5.35 S 0.65 ]]> <![CDATA[4.95×10 -4 ]]> Example 6 <![CDATA[Li 2.8 ZrCl 5.2 S 0.8 ]]> <![CDATA[4.04×10 -4 <!-- 5 -->]]> Example 7 <![CDATA[Li 3 ZrCl 5 S]]> <![CDATA[3.08×10 -4 ]]> Comparative Example 1 <![CDATA[Li 3.25 InCl 5.75 S 0.25 ]]> <![CDATA[4.51×10 -4 ]]> Comparative Example 2 <![CDATA[Li 3.25 ErCl 5.75 S 0.25 ]]> <![CDATA[5.18×10 -4 ]]> Comparative Example 3 <![CDATA[Li 2 ZrCl 5.75 I 0.25 ]]> <![CDATA[5.33×10 -4 ]]> Comparative Example 4 <![CDATA[Li 2 ZrCl 6 ]]> <![CDATA[3.36×10 -4 ]]>

[0083] from Figure 1 As can be seen from Table 1, when the doping amount is small (Example 1), the electrolyte contains only the first phase and has a relatively high crystallinity, so its ionic conductivity is not significantly improved compared to the undoped electrolyte. As the doping amount increases, the second phase gradually appears (Examples 2-3), and the crystallinity decreases, at which time the ionic conductivity is significantly improved. When the doping amount is further increased (Examples 4-7), the content of the second phase gradually increases, the crystallinity increases, and finally only the second phase remains, and there is Li 2 The impurity phase of S appears, which leads to a decrease in ionic conductivity. In Comparative Example 1-2, the tetravalent Zr is replaced with trivalent In and Er, which does not change its physical phase, so the effect on its ionic conductivity is not significant. In Comparative Example 3, the divalent sulfur element is replaced with iodine element of the same family as chlorine, which does not change its physical phase, so the improvement of ionic conductivity is not obvious.

[0084] This is because the introduction of the heterovalent S element induces a second phase crystal structure on the basis of the original phase structure, and the material reacts more strongly to external effects when the two phases coexist than when the single phase is present. High-energy ball milling is an external stimulus, and the process of high-energy ball milling easily destroys the lattice of the material and makes the material amorphous. From XRD, it can be seen that when the two phases coexist, the XRD diffraction peak intensity is lower and the peak width is wider, indicating that there are more amorphous phases, indicating that the two-phase region reacts more strongly to external stimuli, and the diffraction peaks in the area away from the two-phase region are very high and very strong, indicating that there are fewer amorphous phases. The sulfur-doped solid electrolyte synthesized by the present invention relies on the amorphous phase to conduct lithium ions, so the more amorphous phases there are, the higher its ionic conductivity.

[0085] The present invention also provides an application of the above-mentioned sulfur-doped halide solid electrolyte material, and the sulfur-doped halide solid electrolyte prepared in the above-mentioned embodiment 2 is applied to an all-solid-state lithium metal battery, and the specific method is as follows:

[0086] (1) Preparation of composite positive electrode:

[0087] Weigh 70 mg LiCoO2 Or single crystal NCM811 positive electrode material, 30 mg of the halide electrolyte powder prepared in Example 2 above, the two materials were put into an agate mortar and manually ground for 60 minutes to obtain a composite positive electrode material with a positive electrode material to electrolyte mass ratio of 7:3.

[0088] (2) Preparation of full battery:

[0089] First, weigh 35 mg of sulfide electrolyte Li 6 PS 5 Cl was placed in a PEEK mold and maintained at a pressure of 1 ton for 1 min. Then, 70 mg of the halide solid electrolyte prepared in Example 2 was weighed and placed on one side of the sulfide electrolyte and maintained at a pressure of 1.2 tons for 1 min. Then, 15 mg of the composite solid electrolyte powder prepared above was weighed and placed on one side of the halide solid electrolyte and maintained at a pressure of 1.5 tons for 1.5 min. Then, an indium sheet with a diameter of 10 mm and a thickness of 0.1 mm and a lithium sheet with a diameter of 7 mm and a thickness of 0.1 mm were cut and placed on the other side of the sulfide electrolyte in turn. A pressure of 0.5 tons was applied, the mold was tightened, and the battery performance was tested with a blue light.

[0090] Figure 8 and Fig. 9 LiCoO 2 The first cycle charge and discharge curve of the full battery assembled with NCM811 as the positive electrode at room temperature at a rate of 0.1C, with a voltage range of 1.9-3.6V and 2.2-3.8Vvs.Li + / LiIn, the results show that it has excellent battery performance.

[0091] (3) Preparation of symmetrical battery:

[0092] 100 mg of the sulfur-doped halide solid electrolyte prepared in Example 2 was weighed and poured into a PEEK mold, and the pressure was maintained at 2 tons for 2 minutes. Then, a lithium sheet with a diameter of 10 mm was placed on each side of the electrolyte sheet, and a pressure of 0.5 tons was applied and the mold was tightened. A symmetrical battery performance test was performed using a blue light.

[0093] Fig.10 and Fig.11 Li / Li assembled using sulfur-doped halide solid electrolyte 2.25 ZrCl 5.75 S 0.25 / Li symmetric battery and comparative Li / Li 2 ZrCl 6 / Li symmetric battery, the applied current density starts from 0.1mA / cm2 and gradually increases. It can be seen that with the increase of current density, Li / Li 2 ZrCl6 The polarization voltage of the Li / Li symmetric battery increases rapidly until it reaches the protection voltage of 5V, and the test is terminated. 2.25 ZrCl 5.75 S 0.25 The polarization voltage of the / Li symmetric battery increases slowly until the battery short circuits, indicating that the sulfur-doped electrolyte has significantly improved the stability of the lithium metal anode. During the symmetric battery cycle, the sulfur in the sulfur-doped electrolyte reacts with lithium in situ to form a stable Li 2 The S-conducting lithium interface layer prevents the electrolyte from further reacting with lithium metal.

[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A sulfur-doped halide solid electrolyte, characterized in that: The chemical formula of the solid electrolyte is: Li 2+a MX 6- a S a or Li 3+a MX 6-a S a , wherein M includes at least one element selected from Zr, Er, Y, In or Sc, X includes at least one element selected from F, Cl, Br, I, and 0<a≤1.

2. The sulfur-doped halide solid electrolyte according to claim 1, characterized in that: When 0— When <a<0.25, the halide includes a first crystal phase, and the space group is P3m1; when 0.25≤a<0.5, the halide includes a first crystal phase and a second crystal phase, and the space group of the second crystal phase is C2 / m; when 0.5≤a≤1, the halide electrolyte only includes the second crystal phase, and the diffraction peak of Li2S appears.

3. The sulfur-doped halide solid electrolyte according to claim 1, characterized in that: The M is selected as Zr, X is selected as Cl, and 0.25≤a<0.

5.

4. The method for preparing a sulfur-doped halide solid electrolyte according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. In an inert gas, weigh the precursors LiX and MX according to the stoichiometric ratio. b , wherein b=3 or 4, to obtain a halide mixture powder without adding a sulfur source; S2. According to the doping amount a, weigh different masses of sulfur source Li2S and add them to the mixed powder, and grind the mixture manually in an agate mortar for 20 to 60 minutes to obtain a uniform mixed powder with fine particles; S3, weighing zirconia ball milling beads of different sizes, transferring the ball milling beads and the mixed powder into a zirconia ball milling jar, and then placing them on a planetary ball mill for ball milling; S4. After the ball milling is completed, the ball milling tank is opened in the glove box, and the synthesized halide solid electrolyte and the ball milling beads are separated and stored in the glove box for subsequent testing; S5. Weigh a certain mass of the above sulfur-doped halide electrolyte powder, pour it into a stainless steel mold for cold pressing, and obtain a sulfur-doped halide solid electrolyte sheet.

5. The method for preparing the sulfur-doped halide solid electrolyte according to claim 4, characterized in that: The size of the zirconia ball milling beads weighed in step S3 includes one or more of 3 mm, 5 mm, 7 mm and 10 mm, the ball-to-material ratio is (20-60):1, the ball milling speed is 500-800 rpm, the ball milling time is 6-24 h, each operation is 60 min and rest is 5 min.

6. The method for preparing the sulfur-doped halide solid electrolyte according to claim 4, characterized in that: The colors of the series of mixtures obtained in step S4 change from original white to gradually darker yellow as the doping amount a increases.

7. The method for preparing the sulfur-doped halide solid electrolyte according to claim 4, characterized in that: The specific process of step S5 is: weighing 150-200 mg of sulfur-doped halide electrolyte and putting it into a stainless steel mold with a diameter of 10 mm, and applying a pressure of 380 MPa for 1 min to obtain a sulfur-doped halide solid electrolyte sheet with a thickness of 1-1.5 mm.

8. The method for preparing the sulfur-doped halide solid electrolyte according to claim 4, characterized in that: All the above steps were carried out in a glove box with a water content of <0.1 ppm and an oxygen content of <0.1 ppm.

9. Use of the sulfur-doped halide solid electrolyte according to any one of claims 4 to 8 in an all-solid-state battery.

10. An all-solid-state battery, characterized in that: The all-solid-state battery comprises a high-voltage oxide positive electrode, an alloy negative electrode, and a solid electrolyte, wherein the solid electrolyte comprises a halide solid electrolyte and a sulfide electrolyte layer, wherein the halide solid electrolyte comprises the sulfur-doped halide solid electrolyte material described in any one of claims 1 to 3, and the sulfide electrolyte layer comprises Li6PS5Cl or Li 10 GP2S 12 The alloy negative electrode is selected from one of lithium-indium alloy, lithium-magnesium alloy or lithium-aluminum alloy.

Citation Information

Cited By

  • Oxyhalide solid-state electrolyte and preparation method therefor, solid-state battery cell, battery device, and electric device