Solid polymer electrolyte containing flame retardant microcapsule, preparation method of solid polymer electrolyte and battery
By using solid polymer electrolytes containing flame retardant microcapsules in lithium batteries, and using capsule wall grafting double bonds and ionizing radiation curing technology, the negative impact of thermal runaway and flame retardant addition on the performance of lithium batteries has been solved, achieving Efficient thermal stability and electrochemical performance improvement.
Patent Information
- Application Number
- CN202310370113.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-15
AI Technical Summary
Existing lithium batteries have thermal runaway problems under high energy density requirements, leading to safety hazards, and the addition of existing flame retardants will reduce battery performance.
A solid polymer electrolyte containing flame retardant microcapsules is used. By grafting double bond groups on the capsule wall and using ionizing radiation curing technology, the microcapsules are combined with the polymer electrolyte to release the flame retardant to improve the thermal stability of the battery. sex.
It achieves an efficient flame retardant effect under abnormal working conditions of lithium batteries, improves the thermal stability and electrochemical performance of the battery, and avoids the negative impact of flame retardants on battery performance.
Smart Images

Figure CN118782898A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium batteries, and in particular relates to a solid polymer electrolyte containing flame retardant microcapsules, a preparation method thereof and a battery. Background Art
[0002] Lithium batteries are widely used in electronic products, electric vehicles and other fields. At the same time, the requirements for the energy density of lithium batteries in various fields are getting higher and higher. In the existing lithium battery material system, the higher the energy density means the more unstable the battery system, that is, the battery is more prone to safety accidents. Regardless of whether the battery is mechanically damaged, electrically damaged, squeezed and collided, overcharged or short-circuited, accidents generally cause the battery to overheat, catch fire or explode. Therefore, thermal runaway protection of lithium batteries is particularly important. Improving the thermal stability of the battery can greatly improve the overall safety of the battery. The existing lithium battery system itself has some controllable safety characteristics, which are mainly derived from the inherent characteristics of the existing material system. Therefore, some additional means are often used to improve the safety of the battery. The main methods can be divided into external protection measures and internal protection measures.
[0003] External measures include overcurrent protection devices, overtemperature protection devices, overvoltage protection devices, etc. External measures have greatly improved the safety of the product at the application level, but they cannot effectively protect the internal short circuit of the battery, and there is a lag in the response of external safety measures to the internal battery, so there are still many safety hazards. Various thermal protection technologies applied to the inside of the battery include: using diaphragm materials that can be thermally shut down, such as PP, PE, etc., but the thermal shrinkage temperature of such diaphragms is low, and lithium batteries will still short-circuit at high temperatures; or directly mixing flame retardants with positive electrode materials that are easy to generate heat can also play a role in thermal protection, but this method will reduce the capacity of the battery.
[0004] Due to the addition of electrolyte, low flash point electrolytes such as EC, DMC, DEC, etc. are often the main cause of spark overflow. Some researchers believe that flame retardant additives can be directly added to the electrolyte to prevent the battery from igniting. However, most flame retardant additives currently contain phosphorus and fluorine elements. Directly adding flame retardants to the electrolyte will increase the viscosity of the electrolyte due to the addition of the flame retardant, resulting in difficulty in lithium ion transmission. For example, Yao et al. (Comparative study of trimethyl phosphite and trimethyl phosphate as electrolyte additive in lithium ion batteries, Journal of Power Sources, doi.org / 10.1016 / j.jpowsour.2004.11.042.) added 5%-20% trimethyl phosphate (TMP) to 301 electrolyte, which reduced the flammability of the electrolyte, but the electrochemical performance also decreased.
[0005] It can be seen that the solutions to the thermal runaway problem of lithium batteries mainly include: 1. Develop solid electrolytes to avoid the use of liquid electrolytes and solve the problem of electrolyte spark overflow; but at present, polymer solid electrolytes still cannot completely achieve zero solvent, which will lead to the sacrifice of the lithium metal negative electrode, the electrochemical performance of the battery and the decline, and cause the growth of lithium dendrites, which directly affects the safe application of lithium batteries. At the same time, the interface compatibility between traditional solid electrolytes and lithium metal negative electrodes is not ideal; 2. Solve the problem of battery performance degradation caused by the addition of flame retardants. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a solid polymer electrolyte containing flame retardant microcapsules and a preparation method and battery thereof, thereby solving the thermal runaway problem of lithium batteries in the above-mentioned background technology caused by uncontrollable factors during long-term use.
[0007] One of the technical solutions adopted by the present invention to solve its technical problems is: providing a solid polymer electrolyte containing flame retardant microcapsules, including lithium salt, flame retardant microcapsules, and double bond-containing polymers; the flame retardant microcapsules include a capsule core and a capsule wall; the capsule core is a flame retardant, and the capsule wall is a low-melting point polymer that will undergo phase change and decomposition at a temperature under abnormal battery operating conditions, that is, the capsule wall responds to rupture at a temperature under abnormal battery operating conditions, thereby releasing the flame retardant inside; and double bond groups are formed on the surface of the capsule wall, and the flame retardant microcapsules and the double bond-containing polymer are double-bonded and solidified by ionizing radiation.
[0008] The temperature of the battery under abnormal operating conditions is generally 45°C-250°C, among which lithium iron phosphate is generally around 200°C and ternary materials are around 160°C.
[0009] After the surface is endowed with double bonds, the high-efficiency flame-retardant microcapsules can be well bonded with the polymer, and the synergistic effect between different components can be utilized to prevent the flame retardant from deteriorating the electrochemical performance of the lithium battery, thereby improving the electrochemical performance of the electrode material and the safety performance under abnormal operating conditions.
[0010] In a preferred embodiment of the present invention, the content of the flame retardant microcapsules is 1-50wt% of the double bond-containing polymer.
[0011] In a preferred embodiment of the present invention, the capsule wall is at least one layer, and a silane coupling agent containing double bonds is grafted on the surface of the capsule wall.
[0012] In a preferred embodiment of the present invention, the capsule wall is made of urea-formaldehyde resin, phenolic resin, melamine resin, epoxy resin, polymethyl methacrylate, polymethyl pyrrolidone, sodium alginate, hydroxymethyl cellulose, methyl cellulose, polylactic acid, polylactide, polyethylene glycol, polyethylene, polypropylene, polycaprolactone, polyhydroxybutyric acid, polystyrene, polybutadiene, polyether or polyurea. The capsule wall formed by the low melting point polymer is in direct contact with the environment, providing structure and protecting the core material.
[0013] In a preferred embodiment of the present invention, the flame retardant includes a phosphorus-containing flame retardant, a halogen flame retardant, and a metal hydroxide flame retardant.
[0014] In a preferred embodiment of the present invention, the double bond-containing polymer includes one or more of polyethylene glycol dimethacrylate, methoxy polyethylene glycol acrylate, ethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol dimethacrylate, triethylene glycol diacrylate, tetraethylene glycol dimethacrylate, tetraethylene glycol diacrylate, 1,3-propylene glycol dimethacrylate, 1,2-propylene glycol dimethacrylate, 1,3-propylene glycol diacrylate, 1,2-propylene glycol diacrylate, 1,4-butylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol diacrylate, 1,3-butylene glycol diacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate and pentaerythritol tetraacrylate.
[0015] The second technical solution adopted by the present invention to solve the technical problem is: a method for preparing a solid polymer electrolyte containing flame retardant microcapsules is provided, comprising the following steps:
[0016] 1) Preparation of microcapsules:
[0017] Prepolymerizing the precursor of the capsule wall to obtain solution A; dispersing the flame retardant in the same solvent as solution A and emulsifying to obtain solution B; slowly pouring solution A into solution B and stirring thoroughly, adding a curing agent after stirring evenly to crosslink and solidify to form microcapsules containing a double bond polymer as the capsule wall and a flame retardant as the capsule core;
[0018] 2) Microcapsule surface modification:
[0019] The microcapsules prepared in step 1) are mixed and grafted with a silane coupling agent having a double bond, and after grafting, the microcapsules are washed and dried to obtain flame retardant microcapsules having double bond groups on the surface;
[0020] 3) Ionizing radiation in-situ curing:
[0021] The flame retardant microcapsules prepared in step 2) are mixed with a double-bond polymer and a lithium salt, and then in-situ cured by ionizing radiation using Co-60 as a gamma-ray radiation source to prepare a solid polymer electrolyte containing the flame retardant microcapsules.
[0022] In a preferred embodiment of the present invention, in step 2), the silane coupling agent accounts for 5wt% of the microcapsules, and the mixed grafting time is 4h.
[0023] In a preferred embodiment of the present invention, in step 3), the radiation dose is 50 KGy.
[0024] The ionizing radiation grafting method uses the high energy of the radiation to open the double bonds of the polymer and the double bonds on the surface of the flame-retardant microcapsule to form free radicals, and then performs in-situ recombination and curing to evenly disperse the microcapsules in the polymer electrolyte, increase the protection area, and improve the thermal stability of the lithium battery. Among them, the high-energy ionizing radiation in-situ cures the polymer solid electrolyte to obtain a solid polymer electrolyte with high safety performance, and utilizes the synergistic effect between different components to improve the electrochemical and thermal stability of the electrode material. At the same time, the high energy of ionizing radiation can achieve in-situ curing of the solid electrolyte without heating and without introducing initiators, cross-linking agents, catalysts and other solvents.
[0025] The third technical solution adopted by the present invention to solve the technical problem is: providing a solid electrolyte lithium ion battery, including the above-mentioned solid polymer electrolyte containing flame retardant microcapsules.
[0026] Compared with the background technology, this technical solution has the following advantages:
[0027] 1. The present invention utilizes microcapsule coating technology to protect the internal core material, and the release of the internal material can protect the lithium battery under abnormal working conditions. After the microcapsules with high-efficiency flame retardant effect are grafted on the surface, the microcapsules are combined with polymer electrolytes by in-situ curing with ionizing radiation, which reduces the interface impedance, improves the interface compatibility, and can achieve zero solvent addition;
[0028] 2. The preparation method of the present invention adopts a step-by-step synthesis method to achieve the combination of flame retardant additives and lithium batteries. First, a low-melting point polymer is synthesized as a capsule wall, and then the flame retardant as the capsule core is emulsified at high speed to obtain micelles with smaller particle size. The micelles are wrapped by adding the capsule wall of the low-melting point polymer, and then solid-liquid separation is performed to obtain microcapsules with high-efficiency flame retardant effect. Subsequently, a coupling agent with a double bond is used to treat the cured microcapsules, so that the microcapsules with high-efficiency flame retardant effect have the physical and chemical properties of the double bond. Finally, a certain mass ratio of double-bonded polymer and lithium salt are blended, and irradiation graft polymerization and in-situ curing are carried out in one pot.
[0029] 3. The present invention adopts a polymer solid electrolyte with good processability and a lithium metal negative electrode to assemble a battery, which solves the problem of interface stability and increases the safety performance of the solid electrolyte; utilizes microcapsule surface modification and adopts a solvent-free addition method to form a uniform phase with the polymer electrolyte. The flame retardant microcapsules provide protection under normal operating conditions and release the flame retardant under abnormal operating conditions, thereby achieving the purpose of not deteriorating the electrochemical performance but also protecting the battery from abnormal operating conditions, thereby achieving the purpose of reasonably adding flame retardants. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The flame retardant microcapsules and their element distribution diagram in Example 1;
[0031] Figure 2 This is a schematic diagram of the principle of the flame retardant microcapsules in Example 1 releasing the flame retardant under abnormal working conditions;
[0032] Figure 3 is the infrared spectrum of the flame retardant microcapsules in Example 1;
[0033] Figure 4 This is the combustion experiment of Example 1. DETAILED DESCRIPTION
[0034] Example 1
[0035] A solid polymer electrolyte containing flame retardant microcapsules, the preparation method comprising the following steps:
[0036] (1) Preparation of flame retardant microcapsules:
[0037] Add triphenyl phosphate (flame retardant) and sodium dodecylbenzene sulfonate (surfactant) to an aqueous solution. The mass of the surfactant is 1-2wt% of the total mass of the aqueous solution, and the mass of triphenyl phosphate is 30-80wt% of the mass of the urea-formaldehyde resin prepolymer. Raise the temperature to 80°C, which is above the melting temperature of triphenyl phosphate (70°C), and stir at 1500r / min for 2 hours to fully emulsify the flame retardant and prepare an emulsion. The low-melting point polymer is polymerized in two steps: first, a urea-formaldehyde resin prepolymer is prepared, and then the obtained low-melting point polymer prepolymer is slowly added to the above-mentioned emulsion, and then resorcinol (cross-linking agent) is added to the emulsion, and the pH is adjusted to about 3 for cross-linking polymerization. The microcapsules that become precipitates from the liquid phase after polymerization are washed and transferred to a 60°C vacuum oven for drying;
[0038] (2) The microcapsules are dispersed in an ethanol solution, 5% vinyltrimethoxysilane is added, and after condensation and reflux at 80° C. for 12 h, solid-liquid separation and drying are performed to obtain flame-retardant microcapsules with double bonds on the surface.
[0039] (3) Weigh 5 mL of double-bond-containing polymer PEGDA, add 15% of double-bond-containing microcapsules and an appropriate amount of lithium salt (O: Li = 18) and disperse them evenly. Then, use Co-60 as a point source of γ-ray radiation and a radiation dose of 50 KGy for radiation curing for 1 hour.
[0040] The solid polymer electrolyte containing flame retardant microcapsules prepared in this embodiment includes lithium salt, flame retardant microcapsules, and double-bond polymers; the flame retardant microcapsules include a capsule core and a capsule wall; the capsule core is triphenyl phosphate, and the capsule wall is made of urea-formaldehyde resin that will respond and break under abnormal battery operating temperature, and the surface of the capsule wall is grafted with a silane coupling agent containing double bonds, and the double bonds of the silane coupling agent and the double bonds of the polymer PEGDA on the surface of the flame retardant microcapsules are opened by the high energy of gamma rays to form free radicals, and then in-situ recombination and curing are performed, so that the flame retardant microcapsules are uniformly dispersed in the polymer electrolyte, and the capsule wall is directly in contact with the environment to provide structure and protect the capsule core, while preventing the flame retardant from deteriorating the electrochemical performance of the lithium battery, and improving the electrochemical performance of the electrode material and the safety performance under abnormal operating conditions.
[0041] The pole piece punching machine punches the prepared solid electrolyte into a disc with a diameter of 18mm, and finally assembles the positive electrode, negative electrode and solid electrolyte into a 2016 button battery.
[0042] Example 2
[0043] (1) Preparation of flame-retardant microcapsules: Add triphenyl phosphate and sodium dodecylbenzene sulfonate to an aqueous solution, wherein the mass of the surfactant is 1-2wt% of the total mass of the aqueous solution, and the mass of the flame retardant is 30-80wt% of the mass of the prepolymer. Raise the temperature to 80°C and stir at 1500r / min for 2 hours to fully emulsify the flame retardant and prepare an emulsion. The low-melting point polymer is polymerized in a two-step method, and the obtained low-melting point polymer prepolymer is slowly added to the above-mentioned emulsion, and then a cross-linking agent is added to the emulsion, and the pH is adjusted to about 3 for cross-linking polymerization. The cured microcapsules are washed and transferred to a 60°C vacuum oven for drying;
[0044] (2) The microcapsules are dispersed in an ethanol solution, 5% vinyl silane coupling agent vinyl trimethoxysilane is added, and after condensation and reflux at 80°C for 12 hours, solid-liquid separation and drying are performed to obtain flame-retardant microcapsules with double bonds on the surface.
[0045] (3) Weigh 5 mL of double-bond polymer PEGDA, add 15% of double-bond microcapsules and an appropriate amount of lithium salt (O: Li = 18) to it and disperse evenly, then use a radiation dose of 30 KGy for radiation curing for 1 hour. The pole piece punching machine punches the prepared solid electrolyte into a disc with a diameter of 18 mm, and finally assembles the positive electrode, negative electrode, and solid electrolyte into a 2016 button battery.
[0046] Example 3
[0047] (1) Preparation of flame-retardant microcapsules: Add triphenyl phosphate and sodium dodecylbenzene sulfonate to an aqueous solution, wherein the mass of the surfactant is 1-2wt% of the total mass of the aqueous solution, and the mass of the flame retardant is 30-80wt% of the mass of the prepolymer. Raise the temperature to 80°C and stir at 1500r / min for 2 hours to fully emulsify the flame retardant and prepare an emulsion. The low-melting point polymer is polymerized in a two-step method, and the obtained low-melting point polymer prepolymer is slowly added to the above-mentioned emulsion, and then a cross-linking agent is added to the emulsion, and the pH is adjusted to about 3 for cross-linking polymerization. The cured microcapsules are washed and transferred to a 60°C vacuum oven for drying;
[0048] (2) The microcapsules are dispersed in an ethanol solution, 5% of vinyl trimethoxysilane containing double bonds is added, and after condensation and reflux at 80° C. for 12 h, solid-liquid separation and drying are performed to obtain flame-retardant microcapsules with double bonds on the surface.
[0049] (3) Weigh 5 mL of double-bond polymer PEGDA, add 15% of double-bond microcapsules and an appropriate amount of lithium salt (O: Li = 18) to it and disperse evenly, then use a radiation dose of 100 KGy for radiation curing. The pole piece punching machine punches the prepared solid electrolyte into a disc with a diameter of 18 mm, and finally assembles the positive electrode, negative electrode, and solid electrolyte into a 2016 button battery.
[0050] Example 4
[0051] (1) Preparation of flame-retardant microcapsules: Add triphenyl phosphate and sodium dodecylbenzene sulfonate to an aqueous solution, wherein the mass of the surfactant is 1-2wt% of the total mass of the aqueous solution, and the mass of the flame retardant is 30-80wt% of the mass of the prepolymer. Raise the temperature to 80°C and stir at 1500r / min for 2 hours to fully emulsify the flame retardant and prepare an emulsion. The low-melting point polymer is polymerized in a two-step method, and the obtained low-melting point polymer prepolymer is slowly added to the above emulsion, and then a cross-linking agent is added to the emulsion to adjust the pH to about 3. Wash the cured microcapsules and transfer them to a 60°C vacuum oven for drying;
[0052] (2) The microcapsules are dispersed in an ethanol solution, 5% of vinyl trimethoxysilane containing double bonds is added, and after condensation and reflux at 80° C. for 12 h, solid-liquid separation and drying are performed to obtain flame-retardant microcapsules with double bonds on the surface.
[0053] (3) Weigh 5 mL of double-bond polymer PEGDA, add 5% of double-bond microcapsules and lithium salt (O: Li = 18) to it and disperse evenly, then use 50 KGy of radiation dose for radiation curing. The pole piece punching machine punches the prepared solid electrolyte into a disc with a diameter of 18 mm, and finally assembles the positive electrode, negative electrode, and solid electrolyte into a 2016 button battery.
[0054] Example 5
[0055] (1) Preparation of flame-retardant microcapsules: Triphenyl phosphate and sodium dodecylbenzene sulfonate are added to an aqueous solution, wherein the mass of the surfactant is 1-2wt% of the total mass of the aqueous solution, and the mass of the flame retardant is 30-80wt% of the mass of the prepolymer. The temperature is raised to 80°C and stirred at 1500r / min for 2 hours to fully emulsify the flame retardant and prepare an emulsion. The low-melting point polymer is polymerized in two steps, and the obtained low-melting point polymer prepolymer is slowly added to the above emulsion, and then resorcinol is added to the emulsion to adjust the pH to about 3. The cured microcapsules are washed and transferred to a 60°C vacuum oven for drying;
[0056] (2) The microcapsules are dispersed in an ethanol solution, 5% of a silane coupling agent containing double bonds is added, and after condensation and reflux at 80° C. for 12 h, solid-liquid separation and drying are performed to obtain flame-retardant microcapsules with double bonds on the surface.
[0057] (3) Weigh 5 mL of double-bond polymer PEGDA, add 10% of double-bond microcapsules to it and disperse them evenly with lithium salt (O: Li = 18), and then use 50 KGy of radiation dose for radiation curing. The pole piece punching machine punches the prepared solid electrolyte into a disc with a diameter of 18 mm, and finally assembles the positive electrode, negative electrode, and solid electrolyte into a 2016 button battery.
[0058] Example 6
[0059] (1) Preparation of flame-retardant microcapsules: Add flame retardant and surfactant to an aqueous solution, wherein the mass of surfactant is 1-2wt% of the total mass of the aqueous solution, and the mass of flame retardant is 30-80wt% of the mass of prepolymer. The heating temperature needs to be above the melting point of the flame retardant, 80°C is more common) and stir at 1500r / min for 2 hours to fully emulsify the flame retardant and prepare an emulsion. The low-melting point polymer is polymerized in a two-step method, and the obtained low-melting point polymer prepolymer is slowly added to the above-mentioned emulsion, and then a cross-linking agent is added to the emulsion, and the pH is adjusted to about 3 for cross-linking polymerization. The cured microcapsules are washed and transferred to a 60°C vacuum oven for drying;
[0060] (2) The microcapsules are dispersed in an ethanol solution, 5% of a silane coupling agent containing double bonds is added, and after condensation and reflux at 80° C. for 12 h, solid-liquid separation and drying are performed to obtain flame-retardant microcapsules with double bonds on the surface.
[0061] (3) Weigh 5 mL of double-bond polymer PEGDA, add 20% of double-bond microcapsules and an appropriate amount of lithium salt (O: Li = 18) to it and disperse evenly, then use a radiation dose of 50 KGy for radiation curing. The pole piece punching machine punches the prepared solid electrolyte into a disc with a diameter of 18 mm, and finally assembles the positive electrode, negative electrode, and solid electrolyte into a 2016 button battery.
[0062] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A solid polymer electrolyte containing flame retardant microcapsules, comprising a lithium salt, characterized in that: It also includes flame retardant microcapsules and double bond-containing polymers; the flame retardant microcapsules include a capsule core and a capsule wall; the capsule core is a flame retardant, the capsule wall is a low-melting point polymer that will undergo phase change and decomposition under abnormal operating temperature of the battery, and double bond groups are formed on the surface of the capsule wall, and the flame retardant microcapsules and the double bond-containing polymer are double-bonded and cured by ionizing radiation.
2. A solid polymer electrolyte containing flame retardant microcapsules according to claim 1, characterized in that: The content of the flame retardant microcapsules is 1-50wt% of the double bond-containing polymer.
3. The solid polymer electrolyte containing flame retardant microcapsules according to claim 1, characterized in that: The capsule wall is at least one layer, and a silane coupling agent containing double bonds is grafted on the surface of the capsule wall.
4. The solid polymer electrolyte containing flame retardant microcapsules according to claim 1, characterized in that: The capsule wall is made of urea-formaldehyde resin, phenol-formaldehyde resin, melamine resin, epoxy resin, polymethyl methacrylate, polymethyl pyrrolidone, sodium alginate, hydroxymethyl cellulose, methyl cellulose, polylactic acid, polylactide, polyethylene glycol, polyethylene, polypropylene, polycaprolactone, polyhydroxybutyric acid, polystyrene, polybutadiene, polyether or polyurea.
5. The solid polymer electrolyte containing flame retardant microcapsules according to claim 1, characterized in that: The flame retardant includes phosphorus-containing flame retardant, halogen flame retardant and metal hydroxide flame retardant.
6. The solid polymer electrolyte containing flame retardant microcapsules according to claim 1, characterized in that: The double bond-containing polymer includes one or more of polyethylene glycol dimethacrylate, methoxy polyethylene glycol acrylate, ethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol dimethacrylate, triethylene glycol diacrylate, tetraethylene glycol dimethacrylate, tetraethylene glycol diacrylate, 1,3-propylene glycol dimethacrylate, 1,2-propylene glycol dimethacrylate, 1,3-propylene glycol diacrylate, 1,2-propylene glycol diacrylate, 1,4-butylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol diacrylate, 1,3-butylene glycol diacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate and pentaerythritol tetraacrylate.
7. A method for preparing a solid polymer electrolyte containing flame retardant microcapsules according to any one of claims 1 to 6, characterized in that: The steps include: 1) Preparation of microcapsules: Prepolymerizing the precursor of the capsule wall to obtain solution A; dispersing the flame retardant in the same solvent as solution A and emulsifying to obtain solution B; slowly pouring solution A into solution B and stirring thoroughly, adding a curing agent after stirring evenly to crosslink and solidify to form microcapsules containing a double bond polymer as the capsule wall and a flame retardant as the capsule core; 2) Microcapsule surface modification: The microcapsules prepared in step 1) are mixed and grafted with a silane coupling agent having a double bond, and after grafting, the microcapsules are washed and dried to obtain flame retardant microcapsules having double bond groups on the surface; 3) Ionizing radiation in-situ curing: The flame retardant microcapsules prepared in step 2) are mixed with a double-bond polymer and a lithium salt, and then in-situ cured by ionizing radiation using Co-60 as a gamma-ray radiation source to prepare a solid polymer electrolyte containing the flame retardant microcapsules.
8. The preparation method according to claim 7, characterized in that: In step 2), the silane coupling agent accounts for 5wt% of the microcapsules, and the mixed grafting time is 4h.
9. The preparation method according to claim 7, characterized in that: In the step 3), the radiation dose is 50 KGy.
10. A solid electrolyte lithium ion battery, characterized in that: The invention comprises a solid polymer electrolyte containing flame retardant microcapsules as described in any one of claims 1 to 6.
Citation Information
Cited By
B1-grade cable insulating material for home decoration and preparation method thereof
CN121086393A