All-solid-state battery and preparation method thereof

By isolating the lithium tape from the silicon film anode in an all-solid-state lithium battery and encapsulating the edge of the battery using polymer electrolyte, the problems of lithium ion consumption and easy damage to the battery edge are solved, and the charging and discharging efficiency and safety of the battery are improved.

CN118782941BActive Publication Date: 2024-11-19JIANGXI YILI NEW ENERGY DEVELOPMENT CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411273794.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

During the first charging and discharging process of all-solid lithium batteries, lithium ions are consumed due to the formation of the negative electrode SEI film, which affects the efficiency and energy density of the battery. The existing lithium supplementation method has the use of lithium powder solvent, resulting in a decrease in conductivity and strong activity of lithium silicon alloys. The powdering of the pole sheet and the battery edges are prone to damage, causing short circuits.

Method used

The lithium tape is separated from the silicon film negative electrode, and the edge of the battery is encapsulated through polymer electrolyte. The high-temperature polymer electrolyte is used to conduct lithium ions, which short-circuits the silicon film negative electrode and the lithium belt to avoid the powderization of the electrode sheet caused by direct contact between the lithium belt. And encapsulate the edges of the battery with non-conductive polymer electrolyte to improve edge strength.

Benefits of technology

The battery's first charging and discharging efficiency and cycle capacity retention rate are improved, and the lithium replenishment effect is avoided due to direct contact with the lithium belt is not bad, and the battery edge is enhanced to prevent short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782941B_ABST
    Figure CN118782941B_ABST
Patent Text Reader

Abstract

The present invention relates to an all-solid-state battery and a preparation method thereof. The all-solid-state battery comprises a laminate and a polymer electrolyte; the laminate comprises a negative electrode, an electrolyte membrane, and a positive electrode arranged in sequence; the negative electrode comprises a negative electrode current collector, a silicon negative electrode plate coated on one side of the negative electrode current collector, and a lithium belt attached to the other side of the negative electrode current collector; the positive electrode comprises a positive electrode current collector and a positive electrode plate coated on either side of the positive electrode current collector; the electrolyte membrane is arranged between the positive electrode plate and the silicon negative electrode plate; and a polymer electrolyte is arranged on all sides of the laminate. The present invention utilizes a polymer electrolyte that does not conduct lithium ions at room temperature, but conducts lithium ions at high temperature, so that lithium and silicon form a short circuit and can self-discharge to replenish lithium, thereby replenishing lithium for the silicon negative electrode, improving the battery's first efficiency and cycle capacity retention rate; at the same time, the battery is encapsulated with a polymer electrolyte on all sides to improve the battery edge strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of all-solid-state batteries and relates to an all-solid-state battery and a preparation method thereof. Background Art

[0002] Compared to liquid-state batteries, all-solid-state lithium batteries offer high energy density and safety. However, during the initial charge and discharge cycle, the formation of the negative electrode SEI film consumes some lithium ions, resulting in low initial coulombic efficiency, which in turn affects the battery's discharge capacity and reduces its energy density.

[0003] When lithium and silicon are placed together, a lithium insertion reaction will spontaneously occur. Therefore, by utilizing this principle, lithium can be used to replenish silicon. All-solid-state battery lithium replenishment is mainly divided into positive electrode lithium replenishment and negative electrode lithium replenishment. Positive electrode lithium replenishment is to add a substance with high specific capacity and relatively large first-cycle irreversible capacity to the positive electrode. For example, in CN116779864A, a sulfide electrolyte and conductive carbon are added to the positive electrode. The conductive carbon promotes the decomposition of the sulfide electrolyte, produces irreversible capacity, and achieves a lithium replenishment effect. However, in this type of method, the specific capacity of the sulfide electrolyte lithium replenisher itself is less than 200mAh / g, and the lithium replenishment effect is slightly poor.

[0004] Negative electrode lithium replenishment generally includes spraying lithium powder on the surface of the silicon negative electrode and laminating lithium strips on the surface of the silicon negative electrode. For example, patent CN114256499A uses lithium powder sprayed on the negative electrode to directly replenish lithium, which belongs to direct lithium replenishment of the negative electrode. However, stable lithium powder is required in this operation, and the use of solvents will also cause the electrolyte conductivity to decrease. Patent CN114725325A adopts a magnetron sputtering method to spray lithium on the surface of the silicon negative electrode. The method is simple, but requires an inert atmosphere, and the magnetron sputtering device is expensive. As for laminating lithium strips on the surface of the silicon negative electrode, in the prior art, after laminating the lithium strips on the surface of the silicon negative electrode, the two need to be rolled in the process of making the pole piece. Since the lithium-silicon alloy produced by the contact reaction between silicon and lithium is highly active, it will cause the pole piece to become powdered, affecting the effect of the negative electrode lithium replenishment, thereby reducing the initial efficiency of the battery.

[0005] Furthermore, solid-state battery electrodes are prone to edge pulverization during the charge and discharge process. Once the electrolyte membrane edge is damaged, it is very easy to cause a short circuit. Therefore, based on operability, efficiency and cost-effectiveness, it is particularly important to develop a new lithium replenishment method. Summary of the Invention

[0006] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and provide an all-solid-state battery and its preparation method. The present invention innovatively separates the lithium strip from the silicon membrane negative electrode and encapsulates the battery edge with a polymer electrolyte. First, the polymer electrolyte has temperature dependence, and the room temperature conductivity is less than 10 -6 S / cm, basically does not conduct lithium ions, and can reach 10 above 60℃ -4S / cm, which can conduct lithium ions. Therefore, when the assembled battery is activated (charge and discharge in an environment above 60°C to replenish lithium), the silicon film negative electrode will form a short circuit with the lithium strip, achieving the negative electrode lithium replenishment effect; secondly, the lithium strip is not in direct contact with the silicon negative electrode, and the problem of poor lithium replenishment effect due to powdering of the electrode will not occur in the process of making the electrode; finally, the polymer electrolyte is non-conductive. Using the polymer electrolyte to encapsulate the battery edge can prevent the short circuit caused by damage to the battery edge, thereby improving the edge strength and safety of the battery.

[0007] The purpose of the present invention can be achieved by the following solutions:

[0008] In the first aspect, the present invention provides an all-solid-state battery, which includes a laminate and a polymer electrolyte; the laminate includes a negative electrode, an electrolyte membrane, and a positive electrode arranged in sequence; the negative electrode includes a negative electrode collector, a silicon negative electrode plate coated on one side of the negative electrode collector, and a lithium ribbon attached to the other side of the negative electrode collector; the positive electrode includes a positive electrode collector and a positive electrode plate coated on either side of the positive electrode collector; the electrolyte membrane is arranged between the positive electrode plate and the silicon negative electrode plate; and a polymer electrolyte is arranged on all four sides of the laminate.

[0009] As an embodiment of the present invention, the negative electrode current collector includes copper foil; the positive electrode current collector includes aluminum foil.

[0010] As an embodiment of the present invention, the components of the silicon negative electrode plate include silicon-based active materials, a binder, and a conductive agent.

[0011] Furthermore, the silicon-based active material includes one or more of micron silicon, nano silicon, and silicon monoxide.

[0012] Furthermore, the binder includes one or more of PVDF, SBR, NBR, and BR; the conductive agent includes one or more of super-P, VGCF, and CNT.

[0013] As an embodiment of the present invention, the mass ratio of the silicon-based active material, the binder and the conductive agent is 100-xy:x:y, wherein 0<x≤10, 0≤y≤1. In some preferred embodiments, the silicon negative electrode plate may not contain a conductive agent.

[0014] As an embodiment of the present invention, the thickness of the lithium strip is 10-80 μm, and the surface loading is 0.5-4.3 mg / cm 2 If the thickness of the lithium strip is too thick and the surface loading is too large, short circuit and lithium waste may occur easily.

[0015] As an embodiment of the present invention, the electrolyte membrane includes one of an oxide electrolyte, a sulfide electrolyte, and a halide electrolyte.

[0016] Furthermore, the electrolyte membrane includes Li7La3Zr2O 12 , Li 1.4 Al 0.4 Ti 1.6 (PO4)3, Li6PS5Cl, Li 10 GeP2S 12 , Li3InCl6, Li3HoCl6, one or more.

[0017] As an embodiment of the present invention, the components of the positive electrode plate include a positive electrode-based active material, an electrolyte, a conductive agent, and a binder.

[0018] Furthermore, the positive electrode active material includes one or more of a ternary positive electrode, a lithium cobalt oxide positive electrode, a lithium iron phosphate positive electrode, a lithium-rich manganese-based positive electrode, and a lithium nickel manganese oxide positive electrode. The ternary positive electrode includes NCM811.

[0019] Furthermore, the conductive agent includes one or more of super-P, VGCF, and CNT; the binder includes one or more of PVDF, PTFE, SBR, NBR, and BR; and the electrolyte includes one or more of oxide electrolyte, sulfide electrolyte, and halide electrolyte.

[0020] In some preferred embodiments, the electrolyte comprises Li6PS5Cl.

[0021] As an embodiment of the present invention, the mass ratio of the positive electrode-based active material, electrolyte, binder, and conductive agent is 100-xyz:x:y:z; wherein, 0<x≤50, 0<y≤10, and 0<z≤10.

[0022] As an embodiment of the present invention, the polymer electrolyte includes a polymer and a lithium salt.

[0023] Furthermore, the mass ratio of the polymer to the lithium salt is 100-x:x; wherein 10<x<60.

[0024] Furthermore, the polymer includes one or more of PEO, PVDF, PVDF-HFP, and PMMA.

[0025] Furthermore, the lithium salt includes one or more of LiPF6, LiTFSI, LiFSI, and LiDFOB.

[0026] In a second aspect, the present invention provides a method for preparing an all-solid-state battery, the method comprising the following steps:

[0027] S1, coating a silicon negative electrode sheet on one side of the negative electrode current collector, and coating a positive electrode sheet on either side of the positive electrode current collector;

[0028] S2, attaching a lithium ribbon to the other side of the negative electrode current collector;

[0029] S3, placing the side of the negative electrode current collector coated with the silicon negative electrode sheet on either side of the electrolyte membrane, and the positive electrode sheet on the other side of the electrolyte membrane to form a laminate;

[0030] S4. Apply the polymer electrolyte solution to the four sides of the laminate, and then dry it to obtain the all-solid-state battery.

[0031] As an embodiment of the present invention, in step S4, the method for preparing the polymer electrolyte solution includes: dissolving a polymer and a lithium salt in a solvent to obtain a polymer electrolyte solution.

[0032] Furthermore, the solvent includes at least one of acetonitrile and DMF; the solid content of the polymer electrolyte solution is 4%-20%. Too low or too high a solid content will reduce film forming properties.

[0033] As an embodiment of the present invention, in step S4, the drying temperature is 60-100° C. and the drying time is 1-10 h.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. This invention separates the lithium ribbon from the silicon membrane anode, encapsulating the battery edge with a polymer electrolyte. Utilizing the high-temperature conduction of lithium ions from the polymer electrolyte, this short-circuit creates a negative-electrode lithium replenishment effect, thereby improving the battery's initial charge and discharge efficiency and cycle capacity retention. This avoids the prior art practice of directly contacting the lithium ribbon with the silicon anode for lithium replenishment, which results in poor lithium replenishment due to electrode powdering. Furthermore, the design of separating the lithium ribbon from the silicon membrane anode facilitates battery integration and facilitates dispersed lithium replenishment, conserving lithium ribbon.

[0036] 2. The existing solid-state battery electrodes are prone to edge powdering during the charge and discharge process. Once the edge of the electrolyte membrane is damaged, it is very easy to cause a short circuit. The present invention encapsulates the battery side with a non-conductive polymer electrolyte to improve the battery edge strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Other features, objects and advantages of the present invention will become more apparent upon reading the detailed description of non-limiting embodiments with reference to the following drawings:

[0038] Figure 1 This is a structural diagram of the all-solid-state battery prepared in Example 1;

[0039] Figure 2This is a structural diagram of the all-solid-state battery prepared in Example 2;

[0040] Figure 3 This is a structural diagram of the all-solid-state battery prepared in Comparative Example 1;

[0041] Figure 4 This is a structural diagram of the all-solid-state battery prepared in Comparative Example 3;

[0042] Figure 5 The charge and discharge test results of the all-solid-state battery prepared in Example 1 are as follows;

[0043] Figure 6 The charge and discharge test results of the all-solid-state battery prepared in Comparative Example 1 are shown;

[0044] Figure 7 The charge and discharge test results of the all-solid-state battery prepared in Comparative Example 2 are shown;

[0045] Among them, 1: polymer electrolyte 2: silicon negative electrode plate 3: lithium belt 4: negative electrode current collector 5: electrolyte membrane 6: positive electrode plate 7: positive electrode current collector. DETAILED DESCRIPTION

[0046] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments. The following examples are implemented under the premise of the technical solution of the present invention, provide detailed implementation methods and specific operating procedures, and will help those skilled in the art to further understand the present invention. It should be pointed out that the scope of protection of the present invention is not limited to the following embodiments, and a number of adjustments and improvements made under the premise of the concept of the present invention all fall within the scope of protection of the present invention.

[0047] Example 1

[0048] 1) Using micron silicon and PVDF as binders, with a weight ratio of 95:5 and NMP as solvent, a single-sided coating of film-forming silicon negative electrode sheet 2 is applied on the surface of copper foil (i.e., negative electrode current collector 4). The micron silicon surface loading is 5 mg / cm 2 , the area is 3cm*4cm.

[0049] 2) Prepare the positive electrode sheet 6 by dry process with NCM811, Li6PS5Cl, VGCF, and PTFE, with a weight ratio of 80:18:1:1, attached to one side of the aluminum foil (i.e., the positive electrode collector 7), and the NCM811 surface loading is 20 mg / cm 2 , area is 3cm*4cm, apply one sheet.

[0050] 3) Lithium strip 3 has a thickness of 50 μm and a surface loading of approximately 2.5 mg / cm 2 , with an area of ​​3cm*4cm. Stick it on the other side of the negative electrode in step 1.

[0051] 4) Li6PS5Cl is selected as the electrolyte membrane 5, according to Figure 1 Lamination is performed in this manner. Figure 1 This is a cross-sectional view of the battery.

[0052] 5) 1 g of PEO and 300 mg of LiTFSI were dissolved in 15 mg of acetonitrile.

[0053] 6) Spray the solution from step 5) onto the four sides of the battery, and then dry it in a vacuum oven at room temperature to obtain polymer electrolyte 1.

[0054] 7) Place the battery at 60 degrees Celsius for 5 hours, then charge and discharge it at a rate of 0.1C for one cycle. The charge and discharge test results are as follows: Figure 5 As shown in Table 1, the specific battery first efficiency and 100-cycle residual capacity retention rate data are shown in Table 1.

[0055] Example 2

[0056] 1) Using micron silicon and PVDF as binders, with a weight ratio of 95:5 and NMP as solvent, a film-forming silicon negative electrode sheet 2 is coated on the surface of the copper foil (i.e., the negative electrode current collector 4). The micron silicon surface loading is 5 mg / cm 2 , area is 3cm*4cm, two sheets are coated on one side.

[0057] 2) The positive electrode sheet 6 was prepared by dry process using NCM811, Li6PS5Cl, VGCF, and PTFE with a weight ratio of 80:18:1:1. It was attached to both sides of the aluminum foil (i.e., the positive electrode current collector 7). The NCM811 surface loading was 20 mg / cm 2 , area is 3cm*4cm, double-sided coating one sheet.

[0058] 3) Lithium strip 3 has a thickness of 50 μm and a mass of approximately 2.5 mg / cm 2 , with an area of ​​3cm*4cm, and stick it on the other side of a single-sided coated negative electrode in step 1.

[0059] 4) Li6PS5Cl is selected as the electrolyte membrane 5, according to Figure 2 Lamination is performed in this manner.

[0060] 5) 1 g of PEO and 300 mg of LiTFSI were dissolved in 15 mg of acetonitrile.

[0061] 6) Spray the solution from step 5 onto the four sides of the battery, and then dry it in a vacuum oven at room temperature to form polymer electrolyte 1.

[0062] 7) The battery was placed at 60 degrees Celsius for 5 hours, and then charged and discharged for one cycle at 0.1 C. The specific battery initial efficiency and 100-cycle residual capacity retention data are shown in Table 1.

[0063] Comparative Example 1

[0064] The preparation method of this comparative example is basically the same as that of Example 1, except that the lithium strip and polymer electrolyte are not provided. Specifically:

[0065] 1) Using micron silicon and PVDF as binders, with a weight ratio of 95:5 and NMP as solvent, a single-sided coating of film-forming silicon negative electrode sheet 2 is applied on the surface of copper foil (i.e., negative electrode current collector 4). The micron silicon surface loading is 5 mg / cm 2 , the area is 3cm*4cm.

[0066] 2) Prepare the positive electrode sheet 6 by dry process with NCM811, Li6PS5Cl, VGCF, and PTFE, with a weight ratio of 80:18:1:1, and attach it to both sides of the aluminum foil (i.e., the positive electrode current collector 7). The NCM811 surface loading is 20 mg / cm 2 , area is 3cm*4cm, apply one sheet.

[0067] 3) Li6PS5Cl is selected as the electrolyte membrane 5, according to Figure 3 Lamination is performed in this manner.

[0068] 4) Test as in Example 1, the charge and discharge test results are as follows Figure 6 Specific battery first efficiency and 100-cycle residual capacity retention rate data are shown in Table 1.

[0069] Comparative Example 2

[0070] The preparation method of this comparative example is basically the same as that of Example 1, except that the thickness of the lithium strip in step 3) is replaced with 200 μm and the surface loading is replaced with about 10 mg / cm 2 Specifically:

[0071] 1) Using micron silicon and PVDF as binders, with a weight ratio of 95:5 and NMP as solvent, a film-forming silicon negative electrode is coated on one side of the copper foil surface. The micron silicon surface loading is 5 mg / cm 2 , the area is 3cm*4cm.

[0072] 2) The positive electrode was prepared by dry process using NCM811, Li6PS5Cl, VGCF, and PTFE with a weight ratio of 80:18:1:1. The positive electrode was attached to one side of the aluminum foil and the NCM811 surface loading was 20 mg / cm 2 , area is 3cm*4cm, apply one sheet.

[0073] Step 3) The thickness of the lithium strip is 200 μm, about 10 mg / cm 2 , the area is 3cm*4cm.

[0074] 4) Li6PS5Cl is selected as the electrolyte membrane, according to Figure 1Lamination is performed in this manner.

[0075] 5) 1 g of PEO and 300 mg of LiTFSI were dissolved in 15 mg of acetonitrile.

[0076] 6) Spray the solution from step 5) on all sides of the battery, and then dry it in a vacuum oven at room temperature to obtain a polymer electrolyte.

[0077] 7) Place the battery at 60 degrees Celsius for 5 hours, then charge and discharge it at a rate of 0.1C for one cycle. The battery test results are as follows: Figure 7 , the battery is short-circuited.

[0078] Comparative Example 3

[0079] The preparation method of this comparative example is basically the same as that of Example 1, except that the lithium strip is directly attached to the lower surface of the silicon negative electrode without adding a polymer electrolyte.

[0080] 1) Using micron silicon and PVDF as binders, with a weight ratio of 95:5 and NMP as solvent, a single-sided coating of film-forming silicon negative electrode sheet 2 is applied on the surface of copper foil (i.e., negative electrode current collector 4). The micron silicon surface loading is 5 mg / cm 2 , the area is 3cm*4cm.

[0081] 2) Prepare the positive electrode sheet 6 by dry process with NCM811, Li6PS5Cl, VGCF, and PTFE, with a weight ratio of 80:18:1:1, attached to one side of the aluminum foil (i.e., the positive electrode collector 7), and the NCM811 surface loading is 20 mg / cm 2 , area is 3cm*4cm, apply one sheet.

[0082] 3) Lithium strip 3 has a thickness of 50 μm and a surface loading of approximately 2.5 mg / cm 2 , with an area of ​​3cm*4cm. Stick it on the lower surface of the silicon negative electrode sheet 2 in step 1.

[0083] 4) Li6PS5Cl is selected as the electrolyte membrane 5, according to Figure 4 The cells were stacked in this manner. Then, the battery was charged and discharged at a rate of 0.1C for one cycle. The battery's initial efficiency and the remaining capacity retention after 100 cycles are shown in Table 1.

[0084] Comparative Example 4

[0085] The preparation method of this comparative example is basically the same as that of Example 1, except that 1g of PEO and 300mg of LiTFSI in step 5) are replaced with 1g of polyimide, a non-ion-channeling polymer. Specifically:

[0086] 1) Using micron silicon and PVDF as binders, with a weight ratio of 95:5 and NMP as solvent, a film-forming silicon negative electrode is coated on one side of the copper foil surface. The micron silicon surface loading is 5 mg / cm 2 , the area is 3cm*4cm.

[0087] 2) The positive electrode was prepared by dry process using NCM811, Li6PS5Cl, VGCF, and PTFE with a weight ratio of 80:18:1:1. The positive electrode was attached to one side of the aluminum foil and the NCM811 surface loading was 20 mg / cm 2 , area is 3cm*4cm, apply one sheet.

[0088] 3) The thickness of the lithium strip is 50 μm, and the surface loading is about 2.5 mg / cm 2 , with an area of ​​3cm*4cm. Stick it on the other side of the negative electrode in step 1.

[0089] 4) Li6PS5Cl is selected as the electrolyte membrane, according to Figure 1 Lamination is performed in this manner.

[0090] 5) Non-ion channel polymer: 1 g of polyimide is dissolved in 15 mg of acetonitrile.

[0091] 6) Spray the solution from step 5) on all sides of the battery, and then dry it in a vacuum oven at room temperature to obtain a polymer electrolyte.

[0092] 7) The battery was placed at 60 degrees Celsius for 5 hours, and then charged and discharged for one cycle at a rate of 0.1C. The battery's initial efficiency and 100-cycle residual capacity retention are shown in Table 1.

[0093] Table 1 Results of the first efficiency and 100-cycle residual capacity retention of the batteries of Examples 1-2 and Comparative Examples 1-4

[0094]

[0095] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various variations or modifications within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. An all-solid-state battery, It is characterized in that The all-solid-state battery comprises a laminate and a polymer electrolyte; the laminate comprises a negative electrode, an electrolyte membrane and a positive electrode arranged in sequence; the negative electrode comprises a negative electrode collector, a silicon negative electrode sheet coated on one side of the negative electrode collector, and a lithium strip attached to the other side of the negative electrode collector; the positive electrode comprises a positive electrode collector and a positive electrode sheet coated on either side of the positive electrode collector; the electrolyte membrane is arranged between the positive electrode sheet and the silicon negative electrode sheet; the laminate is provided with a polymer electrolyte on all sides; The thickness of the lithium strip is 10-80 μm, and the surface loading is 0.5-4.3 mg / cm 2 ; The polymer electrolyte includes a polymer and a lithium salt; the polymer includes one or more of PEO, PVDF, PVDF-HFP, and PMMA; the lithium salt includes LiPF 6 , LiTFSI, LiFSI, LiDFOB; the mass ratio of the polymer to the lithium salt is 100-x:x; wherein 10<x<60.

2. The all-solid-state battery according to claim 1, It is characterized in that The negative electrode current collector includes copper foil; the positive electrode current collector includes aluminum foil.

3. The all-solid-state battery according to claim 1, It is characterized in that The components of the silicon negative electrode plate include silicon-based active materials, binders, and conductive agents; the silicon-based active materials include one or more of micron silicon, nano silicon, and silicon dioxide; the binder includes one or more of PVDF, SBR, NBR, and BR; the conductive agent includes one or more of super-P, VGCF, and CNT.

4. The all-solid-state battery according to claim 3, It is characterized in that The mass ratio of the silicon-based active material, the binder and the conductive agent is 100-xy:x:y; wherein 0<x≤10, 0≤y≤1.

5. The all-solid-state battery according to claim 1, It is characterized in that The electrolyte membrane includes Li 7 La 3 Zr 2 O 12 , Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 , Li 6 PS 5 Cl, Li 10 G 2 S 12 , Li 3 InCl 6 , Li 3 HoCl 6 One or more of the .

6. The all-solid-state battery according to claim 1, It is characterized in that The components of the positive electrode plate include positive electrode-based active materials, electrolytes, conductive agents, and binders; The positive electrode-based active material includes one or more of a ternary positive electrode, a lithium cobalt oxide positive electrode, a lithium iron phosphate positive electrode, a lithium-rich manganese-based positive electrode, and a lithium nickel manganese oxide positive electrode; The electrolyte includes one or more of an oxide electrolyte, a sulfide electrolyte, and a halide electrolyte; The mass ratio of the positive electrode-based active material, the electrolyte, the binder, and the conductive agent is 100-xyz:x:y:z; wherein 0<x≤50, 0<y≤10, and 0<z≤10.

7. A method for preparing an all-solid-state battery as claimed in any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: S1, coating a silicon negative electrode sheet on one side of the negative electrode current collector, and coating a positive electrode sheet on either side of the positive electrode current collector; S2, attaching a lithium strip to the other side of the negative electrode current collector; S3, placing the side of the negative electrode current collector coated with the silicon negative electrode plate on either side of the electrolyte membrane, and placing the positive electrode plate on the other side of the electrolyte membrane to form a laminate; S4. Apply the polymer electrolyte solution to the four sides of the laminate, and then dry it to obtain the all-solid-state battery.

8. The preparation method according to claim 7, It is characterized in that In step S4, the drying temperature is 60-100° C. and the drying time is 1-10 hours.

Citation Information

Patent Citations

  • Preparation method of all-solid-state battery with lithium-supplementing sulfide solid electrolyte membrane

    CN114256499A

  • Lithium supplementing method for silicon-based negative pole piece of all-solid-state lithium ion battery

    CN114725325A

  • Method for supplementing lithium in all-solid-state battery by using inorganic solid electrolyte

    CN116779864A

  • Lithium ion laminated core and application thereof

    CN112259803A

  • Lithium supplement negative pole piece, preparation method thereof and lithium ion battery