Method for producing automotive structure and curable composition

By using compositions such as liquid epoxy resin containing dispersed rubber particles in the manufacturing of automobile structures, the viscosity ratio and oil surface adhesion at 50°C are improved, and the problems of stringing and spray resistance during the adhesive coating process are improved. It solves the problem of low leakage and realizes the appearance optimization and performance improvement of automobile structures.

CN118786177APending Publication Date: 2024-10-15CEMEDINE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023962.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-01
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the manufacturing of existing automobile structures, the adhesive composition is prone to stringing during the coating process, resulting in poor appearance and low spray resistance. It is difficult to effectively suppress and improve stringing and oil surface adhesion.

Method used

A curable composition containing liquid epoxy resin with dispersed rubber particles, latent curing agent, surface-treated fumed silica, blocked urethane resin and polyethylene powder is used. It is sheared at 50°C. The ratio of the viscosity at a shear speed of 0.5/sec to the viscosity at a shear speed of 1000/sec is set to 50 or more to improve stringability and thixotropy and improve oil surface adhesion.

Benefits of technology

It significantly improves the drawability and oil surface adhesion of automobile structures, suppresses poor appearance, improves spray resistance and operability, and is suitable for the manufacture of automobile structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786177A_ABST
    Figure CN118786177A_ABST
Patent Text Reader

Abstract

Provided are: a method for producing an automobile structure, which is capable of suppressing defects in the appearance of an automobile structure; and a curable composition which has improved thixotropy, improved drawability, and excellent oil surface adhesion, and which can be suitably used in the production of an automobile structure. Provided is a method for producing an automobile structure, the method comprising a step for applying a curable composition for producing an automobile structure, the curable composition comprising (A) a liquid epoxy resin in which rubber particles are dispersed, (B) a latent curing agent, (C) surface-treated fumed silica, (D) a blocked urethane resin, and (E) a polyethylene powder, to an adherend, the ratio of the viscosity of the curable composition at a shear rate of 0.5 / sec at 50 DEG C to the viscosity at a shear rate of 1000 / sec is 50 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing an automobile structure capable of suppressing the appearance defects of the automobile structure, and a curable composition having enhanced thixotropy, improved stringiness, and excellent oil surface adhesion. Background Art

[0002] In the past, there is a known structural adhesive composition for manufacturing an automobile structure by joining automobile body panels, body parts, etc. When the structural adhesive composition is applied using an automobile manufacturing assembly line, if the structural adhesive composition contains a rubber component in the past, the adhesive is attached to an undesired place due to stringing during intermittent (stitch) coating, which has a negative impact on the electrodeposition coating of the next step and deteriorates the rust resistance and appearance. In particular, if the stringing is long, the adhesive is exposed from the flange, resulting in a poor appearance of the automobile structure.

[0003] Furthermore, in the spraying process of the automobile manufacturing assembly line, if the structural adhesive composition has a low viscosity when heated, the spraying resistance is low and there is a possibility of being blown away by the spraying. Therefore, the structural adhesive composition is conventionally used in places and locations that are not easily blown away by the spraying.

[0004] As a structural adhesive with improved spray resistance and good discontinuity, Patent Document 1 proposes a structural adhesive composition comprising an epoxy resin in which rubber particles are dispersed in the form of primary particles and an epoxy resin latent curing agent. However, in recent years, it is desired to further suppress poor appearance, improve stringiness, and enhance bonding performance.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 6744405

[0008] Patent document 2: WO2004108825A1 Summary of the invention

[0009] Problems to be solved by the invention

[0010] The present invention has been accomplished in view of the above-mentioned problems of the prior art, and its object is to provide a method for manufacturing an automobile structure that can suppress the poor appearance of the automobile structure, and a curable composition that has improved thixotropy, improved stringiness, and excellent oil surface adhesion and can be suitably used for the manufacture of automobile structures.

[0011] Means for solving problems

[0012] In order to solve the above-mentioned problems, the inventors of the present invention have repeatedly conducted in-depth studies and found that the stringiness is correlated with the thixotropy. By setting the ratio of the viscosity at a shear rate of 0.5 / sec at 50°C to the viscosity at a shear rate of 1000 / sec (viscosity ratio 0.5 / 1000) to 50 or more, the stringiness is significantly improved, and the poor appearance of the automobile structure caused by the adhesive can be suppressed.

[0013] The method for producing an automobile structure of the present invention is a method for producing an automobile structure, comprising the step of applying a curable composition for producing an automobile structure, which contains (A) a liquid epoxy resin in which rubber particles are dispersed, (B) a latent curing agent, (C) surface-treated fumed silica, (D) a blocked urethane resin, and (E) a polyethylene powder, to an adherend, wherein the ratio of the viscosity of the curable composition at a shear rate of 0.5 / sec to the viscosity at a shear rate of 1000 / sec at 50°C is 50 or more.

[0014] The curable composition of the present invention contains (A) a liquid epoxy resin in which rubber particles are dispersed, (B) a latent curing agent, (C) a surface-treated fumed silica, (D) a blocked urethane resin, and (E) a polyethylene powder, wherein the ratio of the viscosity of the curable composition at a shear rate of 0.5 / sec to the viscosity at a shear rate of 1000 / sec at 50°C is 50 or more. With the above-mentioned configuration, thixotropy is improved, stringiness is improved, and oil surface adhesion can be significantly improved.

[0015] The curable composition of the present invention is suitably used as a curable composition for producing automobile structures.

[0016] Effects of the Invention

[0017] According to the present invention, by using a curable composition having enhanced thixotropy, improved stringiness and excellent oil surface adhesion, a particularly great effect can be exerted, namely, a method for manufacturing an automobile structure with excellent workability that can suppress the poor appearance of the automobile structure caused by stringiness of the curable composition, and a curable composition having enhanced thixotropy, improved stringiness and excellent oil surface adhesion and suitable for the manufacture of automobile structures can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The photographs show the measurement method of the stringiness test, (a) is a photograph showing 30 points of intermittent coating, and (b) is a partial enlarged photograph of (a) showing the measurement position of the stringiness length. DETAILED DESCRIPTION

[0019] Embodiments of the present invention will be described below. However, these embodiments are given for illustrative purposes only, and therefore various modifications are possible without departing from the technical concept of the present invention.

[0020] The curable composition of the present invention contains (A) a liquid epoxy resin in which rubber particles are dispersed, (B) a latent curing agent, (C) surface-treated fumed silica, (D) a blocked urethane resin, and (E) polyethylene powder.

[0021] The ratio of the viscosity of the curable composition at a shear rate of 0.5 / sec at 50°C to the viscosity at a shear rate of 1000 / sec is 50 or more, the thixotropy is improved, and the stringiness can also be improved, and the curable composition has more excellent oil surface adhesion, and is particularly suitable as a structural adhesive composition used in the manufacture of automobile structures.

[0022] The method for producing an automobile structure of the present invention is a method for producing an automobile structure, comprising the step of applying a curable composition for producing an automobile structure, which contains (A) a liquid epoxy resin in which rubber particles are dispersed, (B) a latent curing agent, (C) surface-treated fumed silica, (D) a blocked urethane resin, and (E) a polyethylene powder, to an adherend, wherein the ratio of the viscosity of the curable composition at a shear rate of 0.5 / sec to the viscosity at a shear rate of 1000 / sec at 50°C is 50 or more.

[0023] The manufacturing method of the automobile structure of the present invention is preferably a manufacturing method in an automobile production line. As the process of applying the above-mentioned curable composition to the adherend, it is suitable to be a process of intermittently applying the above-mentioned curable composition to the adherend after heating at 40 to 60°C. By performing heated coating, the ejection property from the nozzle becomes good, so heated coating is preferably performed in the production line. By utilizing the process of heating and applying the above-mentioned curable composition to the adherend at 40 to 60°C, adherends such as body panels, protective covers, doors, and fenders can be appropriately bonded. In particular, in the present invention, the thixotropy during heating is significantly improved, so the wire drawing property is also improved, so the poor appearance of the automobile structure caused by wire drawing that has been produced in the past can be suppressed.

[0024] The manufacturing method of the automobile structure of the present invention preferably adopts a welding joining process (a process using an adhesive and spot welding in combination). In the present invention, by using a curable composition containing the above-mentioned components (A) to (E) and having improved thixotropy at 50°C and excellent oil surface adhesion as an adhesive, the wire drawing property during intermittent coating is improved, and the spray resistance can also be improved. As a result, the poor appearance of the automobile structure can be suppressed, and the parts that could only be spot welded in the past can also be joined based on the welding joining process, so that the application parts of the adhesive on the car body, etc. can be increased, and the rigidity can be improved. As a result, the car becomes lighter, which brings about an improvement in fuel efficiency.

[0025] In addition, since the curable composition has high spray resistance and good discontinuity, it can be intermittently coated when used in an automobile production line, and has excellent operability. The so-called intermittent coating refers to the intermittent coating of the adhesive. By applying intermittent coating in the welding and joining process, the adhesive can be applied to avoid the part where spot welding is performed, which has the effect of suppressing the generation of combustion gases such as smoke and carbon dioxide caused by the burning of the adhesive and reducing the amount of adhesive used. In the manufacturing method of the automobile structure of the present invention, the coating is preferably performed using a robot coater.

[0026] (A ingredient)

[0027] The liquid epoxy resin in which the rubber particles are dispersed as the component (A) has the effect of imparting toughness and improving the spray resistance. In this specification, the term "liquid" means a liquid epoxy resin having a temperature of 23°C and 1.01×10 5 Pa has a fluid state. As the above-mentioned liquid epoxy resin (A), an epoxy resin in which rubber particles are dispersed in the state of primary particles is suitable, and more preferably a rubber particle-dispersed epoxy resin having an epoxy equivalent of 500 to 10,000, in which rubber particles having a number average particle size of 10 to 1,000 nm are dispersed in the state of primary particles. It is preferred that 1 to 100 parts by mass of rubber particles are contained relative to 100 parts by mass of the epoxy resin, and from the viewpoint of fully obtaining the effect of the present invention, 50 to 90 parts by mass is more preferred, and 60 to 80 parts by mass is further preferred.

[0028] Here, the rubber particles are "dispersed in the state of primary particles" means that the cross-linked rubber particles having a number average primary particle size of preferably 10 to 1000 nm are not agglomerated with each other in the epoxy resin but are dispersed independently. This dispersion state can be confirmed, for example, by dissolving the rubber particle-dispersed epoxy resin in a solvent such as methyl ethyl ketone and measuring the particle size using a particle size measuring device based on laser scattering, or by observing the rubber particle-dispersed epoxy resin using an electron microscope.

[0029] As described above, the rubber particles of the above-mentioned component (A) exert the effect of the present invention by being independently dispersed in the epoxy resin, and therefore need to be incompatible in the epoxy resin. For this reason, the rubber particles of the component (A) include a core polymer of a cross-linked rubber particle core layer and a shell polymer of a hard polymer shell layer. The core polymer is present on the inner side of the rubber particles, preferably 55 to 100% by mass, more preferably 60 to 90% by mass, and is a polymer of a monomer for polymerization of the cross-linked rubber particle core layer; the shell polymer is present on the outer side of the rubber particles, preferably 0 to 45% by mass, more preferably 10 to 40% by mass, and is a polymer of a monomer for polymerization of the hard polymer shell layer of a vinyl monomer. The rubber particles of the component (A) preferably have a core-shell structure including a cross-linked rubber particle core layer and a hard polymer shell layer. More preferably, core-shell rubber particles are formed by grafting a hard polymer shell layer onto the cross-linked rubber particle core layer.

[0030] The rubber particles have a number average particle size of 10 to 1000 nm, preferably 10 to 600 nm, more preferably 10 to 500 nm, and even more preferably 10 to 400 nm, from the viewpoint of effective toughness improvement. The number average particle size of the rubber particles can be determined, for example, by dynamic light scattering or electron microscopy.

[0031] The rubber particles of the above-mentioned component (A) are preferably cross-linked rubber particles. Since the above-mentioned cross-linked rubber particles are cross-linked, there are solvent-insoluble components in the rubber particles. Regarding the amount of solvent-insoluble matter in the rubber particles (i.e., the gel fraction related to the cross-linked rubber), after immersing the sample in an excess of methyl ethyl ketone (MEK) at room temperature for 24 hours, centrifugation is performed at 12,000 rpm for 1 hour to remove the solvent together with the soluble components, and the mass of the remaining MEK insoluble matter is measured, thereby expressing it as a ratio of the residual sample mass to the input sample mass in mass percentage. Regarding the amount of solvent-insoluble matter in the above-mentioned cross-linked rubber particles, from the viewpoint of obtaining an excellent performance balance, it is preferably set to 80 to 100 mass%, and particularly preferably 90 to 100 mass%.

[0032] The rubber particles used in the present invention preferably have a core-shell structure comprising a crosslinked rubber particle core layer and a hard polymer shell layer. From the viewpoint of improving toughness, it is more preferably a graft copolymer comprising a hard polymer shell layer obtained by polymerizing one or more vinyl monomers in the presence of a crosslinked rubber particle core layer selected from one or more of butadiene rubber, butadiene-styrene rubber, butadiene butyl acrylate rubber, butyl acrylate rubber and silicone rubber, more preferably butadiene rubber. From the viewpoint of controlling the particle size, it is preferably produced by emulsion polymerization.

[0033] The crosslinked rubber particle core layer may be copolymerized with less than 50% of a component containing the following vinyl monomers to such an extent that the physical properties thereof are not impaired.

[0034] Examples of the vinyl monomer include aromatic vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, and divinylbenzene; cyanide vinyl monomers such as acrylonitrile and methacrylonitrile; methacrylic acid and methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, glycidyl methacrylate, hydroxyethyl methacrylate, ethylene glycol dimethacrylate, and 1,3-butanediol dimethacrylate; and acrylic acid and acrylate esters such as methyl acrylate, butyl acrylate, glycidyl acrylate, hydroxybutyl acrylate, and phenoxyethyl acrylate. The above vinyl monomers may be used alone or as a mixture thereof.

[0035] The rubber particles of the component (A) preferably contain one or more groups selected from epoxy groups and functional groups capable of reacting with epoxy groups, from the viewpoint of allowing the rubber particles to exist stably for a long period of time in the composition of the present invention, and more preferably contain the above-mentioned groups in the hard polymer shell layer.

[0036] The crosslinked rubber particle core layer preferably has a glass transition temperature of 0° C. or lower from the viewpoint of improving toughness.

[0037] The epoxy resin used in the component (A) may have an epoxy equivalent of 80 to 10,000, and preferably has an epoxy equivalent of 80 to 200.

[0038] Examples of the epoxy resins include glycidyl ether-substituted products of compounds having known basic skeletons such as bisphenol compounds, hydrogenated bisphenol compounds, phenol or o-cresol novolac, aromatic amines, polycyclic aliphatic or aromatic compounds, and compounds having an epoxycyclohexane skeleton. Representative epoxy resins include diglycidyl ether of bisphenol A and its condensate, i.e., so-called bisphenol A type epoxy resins.

[0039] As the epoxy resin in which the rubber particles of the component (A) are dispersed in the state of primary particles, for example, an epoxy resin composition described in Patent Document 2 can be used.

[0040] (Component B)

[0041] As the latent curing agent of the above-mentioned component (B), known epoxy resin latent curing agents can be applied. For example, a latent curing agent for epoxy resin activated by heating can be selected from the group consisting of guanamines, guanidines, aminoguanidines, ureas, imidazoles, modified polyamines and their derivatives, dicyandiamide, boron trifluoride amine complex, organic acid hydrazides, melamine, etc. Among them, dicyandiamide, which is widely used, is preferred. It should be noted that the addition amount of the latent curing agent of the above-mentioned component (B) is determined according to the epoxy equivalent of the substrate.

[0042] (Component C)

[0043] The surface treated fumed silica of the component (C) has the effect of imparting thixotropy and improving spray resistance. As the surface treated fumed silica of the component (C), fumed silica surface treated with a known surface treatment agent can be used, for example, surface treated hydrophobic fumed silica surface treated with a hydrophobizing agent such as polydimethylsiloxane or dimethyldichlorosilane can be appropriately used. The specific surface area of ​​the fumed silica of the component (C) is preferably 10 m 2 / g~500m 2 / g, more preferably 50m 2 / g~300m 2 / g.

[0044] The blending ratio of the surface-treated fumed silica of the component (C) is not particularly limited, but is preferably 5 to 30 parts by mass based on 100 parts by mass of the epoxy resin of the component (A).

[0045] (Component D)

[0046] The blocked carbamate resin of the above-mentioned component (D) has the effect of imparting toughness and improving adhesion. As the blocked carbamate resin of the above-mentioned component (D), a known blocked carbamate resin obtained by blocking a carbamate prepolymer obtained by reacting a polyhydroxy compound with a polyisocyanate compound with a blocking agent can be used. As the blocked carbamate resin of the above-mentioned component (D), specifically, a blocked carbamate obtained by blocking a polyurethane having an isocyanate (NCO) content of 0.1 to 10% by mass with an active methylene compound, an oxime compound, a phenol compound, a lactam compound, and a secondary amine compound can be suitably used.

[0047] The blending ratio of the blocked urethane resin of the component (D) is not particularly limited, but is preferably 25 to 55 parts by mass based on 100 parts by mass of the epoxy resin of the component (A).

[0048] (Ingredient E)

[0049] The polyethylene powder as the component (E) has the effect of improving adhesiveness. In particular, by using the blocked urethane resin as the component (D) and the polyethylene powder as the component (E) together, the adhesiveness to oily surfaces can be significantly improved.

[0050] As the polyethylene powder of the component (E), known polyethylene resin powder can be used. The particle size of the polyethylene powder of the component (E) is not particularly limited, but preferably a fine powder having a median particle size of 100 μm or less as measured by a laser method, more preferably a fine powder having a median particle size of 50 μm or less.

[0051] The blending ratio of the polyethylene powder of the component (E) is not particularly limited, but is preferably 10 to 45 parts by mass based on 100 parts by mass of the epoxy resin of the component (A).

[0052] (Optional Ingredients)

[0053] In the above-mentioned curable composition, on the basis of the above-mentioned components, as long as the effect of the present invention is not impaired, epoxy resin, modified epoxy resin, urethane resin, curing accelerator, filler, diluent, reactive diluent, viscosity modifier, hygroscopic agent, silane coupling agent (such as epoxy silane) and the like may also be added. In addition, on the basis of the above-mentioned components, body pigments (filling materials) such as calcium carbonate, barium sulfate, talc, wollastonite, organic pigments (such as monoazo pigments), inorganic pigments (such as carbon black, titanium oxide, iron oxide) and other coloring pigments may also be added. In addition, thixotropic materials such as Ketjen black, silicon dioxide, microparticles of calcium carbonate, sepiolite may also be added. As an adhesive modifier to further improve the adhesiveness such as peel strength, acrylic resin may also be added.

[0054] The curable composition preferably contains substantially no liquid rubber component.

[0055] The curable composition is a composition that improves stringiness and suppresses appearance defects of automobile structures by setting the ratio of the viscosity at a shear rate of 0.5 / sec to the viscosity at a shear rate of 1000 / sec at 50°C (viscosity ratio 0.5 / 1000) to 50 or more, and a viscosity ratio (0.5 / 1000) of 65 or more is more suitable for suppressing appearance defects.

[0056] The viscosity at 50° C. is preferably 700 to 5000 (Pa·s), more preferably 1000 to 3000 (Pa·s) at a shear rate of 0.5 / sec, and is preferably 1 to 30 (Pa·s) at a shear rate of 1000 / sec.

[0057] The curable composition can be used particularly as a one-component type.

[0058] The above-mentioned curable composition can be used for various purposes such as adhesives, coatings, coatings, sealing materials, bonding materials, potting materials, putty materials and primers. The above-mentioned curable composition is particularly preferably used as an adhesive for automobiles, etc. due to its improved thixotropy, improved wire drawing properties and excellent oil surface adhesion. In addition, it can also be used for various buildings, civil engineering, electrical / electronic fields, etc. When the above-mentioned curable composition is used as an automotive adhesive, it can be suitably used for structural bonding of parts such as the body of an automobile, automobile parts, etc. to manufacture an automobile structure, and can particularly be suitably used for bonding in a process (welding and joining process) using spot welding and an adhesive. That is, the above-mentioned curable composition can also be suitably used for bonding the body of an automobile.

[0059] Example

[0060] The present invention will be further specifically described below with reference to Examples. However, these Examples are given for illustrative purposes only and should not be construed in a limiting sense.

[0061] (Examples 1 to 3 and Comparative Examples 1 to 6)

[0062] A curable composition was prepared according to the following procedure using the components in parts by mass shown in Table 1. The materials in Table 1 were mixed in a 5L universal mixer (manufactured by DALTON CORPORATION), stirred for 30 minutes, and then degassed under reduced pressure for 10 minutes to prepare a curable composition.

[0063] [Table 1]

[0064]

[0065] The materials in Table 1 are as follows.

[0066] *1) "Kane Ace MX-154" (manufactured by KANEKA Corporation) Liquid epoxy resin in which core-shell rubber is dispersed (rubber particle content: 40% by mass)

[0067] *2) "Epiclon 850" bisphenol A epoxy resin manufactured by DIC Corporation

[0068] *3) "RA-840" CTBN-modified epoxy resin manufactured by Huntsman

[0069] *4) "DYHARD 100SH" dicyandiamide manufactured by AlzChem

[0070] *5) "DYHARD UR200" DCMU manufactured by AlzChem

[0071] *6) "ADEKA RESIN QR-9466" Blocked urethane resin manufactured by ADEKA

[0072] *7) “TS-720” surface treated fumed silica manufactured by CABOT

[0073] *8) "Aerosil R972" untreated silica manufactured by Japan Aerosil Co., Ltd.

[0074] *9) “Whiton SB” calcium carbonate manufactured by Shiraishi Calcium Co., Ltd.

[0075] *10) "Hakuenhua CCR-B" surface treated calcium carbonate manufactured by Shiraishi Industries Co., Ltd.

[0076] *11) “QC-X” calcium oxide manufactured by Inoue Lime Industry Co., Ltd.

[0077] *12) "FLOTHENE UF-20S" polyethylene powder manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0078] Each of the curable compositions of Examples 1 to 3 and Comparative Examples 1 to 4 produced as described above was used in the performance tests shown below. The results are shown in Table 2 below.

[0079] (1) Viscosity

[0080] The viscosity of the curable composition obtained above at 50° C. at shear rates of 5 / sec and 1000 / sec was determined using RST-CPS manufactured by Brookfield equipped with a heating device and a sensor system. Samples having a ratio of the viscosity at a shear rate of 0.5 / sec to the viscosity at a shear rate of 1000 / sec of 50 or more were evaluated as ○, and samples having a ratio of less than 50 were evaluated as ×.

[0081] (2) Wire drawing properties

[0082] The curable composition obtained above was intermittently coated using a robot coater under the following conditions, and the stringiness was measured. A photograph showing the measurement method of the stringiness test is shown in Figure 1 middle.

[0083] As the robot coater, SYS6000 manufactured by Atlas Copco was used.

[0084] The nozzle was set at a distance of 6 mm from the coating object, the coating speed was set at 500 mm / sec, the coating temperature was set at 50°C, and intermittent coating was performed on the 90° longitudinal surface. Figure 1 As shown in (a), repeat 3 times with 10 dots. Figure 1As shown in (b), the portion hanging down from the end point of each coating point was evaluated as the string length. Samples with an average string length of 9 mm or less at 30 coating points were rated as ○, and samples with a string length of more than 9 mm were rated as ×.

[0085] (3) Oil surface adhesion test

[0086] Using the curable composition obtained above as an adhesive, an oil surface adhesion test was performed by the peel strength evaluation shown below.

[0087] Prepare two cold-rolled steel plates with a length of 200 mm, a width of 25 mm, and a thickness of 0.6 mm, and perform a 90° bending process at a distance of 50 mm from the end. Apply the processing oil (rust-proof oil or stamping oil) of the object to the above cold-rolled steel plate, stand it vertically and dry it at 40°C for 1 week. Apply the adhesive to the above cold-rolled steel plate with a coating thickness of 0.2 mm, overlap the above two cold-rolled steel plates so that the overlapping part is 150 mm, and remove the exposed adhesive. In this way, a peel test piece is made. The above peel test piece is put into a dryer at 160°C, and the adhesive part is heated by keeping it at 160°C for 20 minutes. After sintering, cool it naturally for 24 hours, and then use a universal tensile testing machine to test it at a tensile speed of 200 mm / min. The sample with a failure state of CF (cohesive failure) 100% is set as ○, and the sample that is not CF 100% is set as ×.

[0088] [Table 2]

[0089]

[0090] In Examples 1 to 3, the oil surface adhesion was excellent, the viscosity ratio was 50 or more, the thixotropy was improved, and the average stringiness was within 9 mm, and the stringiness was improved. On the other hand, in Comparative Examples 1 to 6, the results of either or both of the thixotropy, stringiness, and oil surface adhesion were poor.

Claims

1. A curable composition comprising: (A) a liquid epoxy resin in which rubber particles are dispersed, (B) Latent curing agent, (C) surface treated fumed silica, (D) a blocked urethane resin, and (E) polyethylene powder, The ratio of the viscosity of the curable composition at a shear rate of 0.5 / sec to the viscosity at a shear rate of 1000 / sec under a condition of 50° C. is 50 or more.

2. The curable composition according to claim 1, in, The curable composition is a curable composition for manufacturing an automobile structure.

3. A method for manufacturing an automobile structure, the method comprising applying a curable composition for manufacturing an automobile structure to an adherend, The curable composition for manufacturing an automobile structure comprises: (A) a liquid epoxy resin in which rubber particles are dispersed, (B) Latent curing agent, (C) surface treated fumed silica, (D) a blocked urethane resin, and (E) polyethylene powder, The ratio of the viscosity of the curable composition at a shear rate of 0.5 / sec to the viscosity at a shear rate of 1000 / sec under a condition of 50° C. is 50 or more.