Electrode with carbon nanotube scaffold
By using 3D composite current collector electrodes in lithium-ion batteries, using conductive carbon nanotube scaffolds and passivation layer structures, the cycle life and stability problems of lithium metal anodes are solved, and the energy density and life of the battery are improved.
Patent Information
- Application Number
- CN202380027402.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-13
- Filing Date
- 2023-01-12
- Publication Date
- 2024-10-15
AI Technical Summary
The cycle life of lithium metal anodes in lithium-ion batteries is affected by the formation of pores, dendrites, and hillocks, leading to short circuits and uneven structures in the battery, thereby reducing battery stability and energy density.
Using a 3D composite current collector electrode, a combination of a conductive 3D vertically aligned carbon nanotube scaffold and a passivation layer forms an anode structure with high safety and cycle stability, reduces the formation of dendrites and hillocks, and improves the electric field Uniformity and material distribution.
It improves the cycle stability and energy density of lithium-ion batteries, extends the life of the battery, and reduces the irreversible loss of anode material and power density loss.
Smart Images

Figure CN118786540A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an electrode, in particular to an electrode comprising a 3D composite current collector, and also to an energy storage device and a manufacturing method comprising the electrode. Background Art
[0002] Rechargeable lithium-ion batteries (LiBs) are considered as the potential technology of choice for the next generation of energy carriers in the global energy transition, for example in the electrification of transportation and renewable energy storage grids. State-of-the-art LiBs aim to improve safety issues related to the liquid nature of the electrolyte while increasing the current energy density of about 270 Wh / kg at the cell level due to the limited capacity of the anode graphite (370 mAh / g). To improve the feasibility of electric vehicles, the goal is to combine batteries with higher energy density (e.g. >400 Wh / kg) and the use of intrinsically safe solutions. One approach is to transition to all-solid-state batteries with lithium metal anodes, which have a potentially high specific capacity of 3860 mAh / g and a redox potential of -3.04 V.
[0003] However, the cycle life of lithium metal anodes is affected by the formation of pores and dendrites during battery charging (e.g., in liquid electrolytes). In addition, lithium metal batteries are affected by one or more of several other issues, including cell shorting due to hillock formation (uneven lithium metal deposition); and undesirable reactions such as the evolution of dead lithium encapsulated by a thin film of solid electrolyte interface (SEI) reaction products, which over time leads to the formation of a porous, inhomogeneous anode structure, which in turn leads to increased diffusion pathways for lithium ions and electrons, resulting in increased polarization. These porous deposits also promote large changes in the internal volume of the anode during plating / stripping cycles, resulting in poor life cycle stability.
[0004] US10741835 discloses an anode structure for a lithium metal battery, the anode structure comprising a current collector, a seed layer preferably used to promote electrochemical plating of metallic lithium deposited on the current collector, a separator, and a main structure between the seed layer and the separator to accommodate the metallic lithium during charging. A first bonding layer and a second bonding layer are required to bond the main structure to the seed layer and the separator, respectively.
[0005] S. Yoon (Journal of Power Sources, 2015 279, 495) describes a thin film anode made of carbon nanotubes (CNT) for flexible lithium-ion batteries. The thin film anode is based on disordered carbon nanotubes, prepared by chemical vapor deposition and direct spinning. The carbon nanotubes carry the anode metal. The study suggests heat treatment in a nitrogen atmosphere to affect the performance. Summary of the invention
[0006] The present disclosure alleviates one or more of the above disadvantages by providing an anode, particularly an electrode including a 3D composite current collector, which is particularly beneficial in use as a metal anode or as a host for a metal anode, while providing a combination of higher safety and cycling stability.
[0007] More specifically, the preferred concept of a 3D structured electrode comprises a conductive 3D vertically aligned carbon nanotube scaffold that is densified and subsequently coated for use as an anode in a metal electrode based battery.
[0008] The 3D composite current collector comprises a conductive substrate current collector having a plurality of laterally distributed conductive upright support elements. The support elements comprise a structure of agglomerated carbon nanotubes, which are substantially parallel oriented in a direction away from the substrate. The structure of agglomerated carbon nanotubes is covered by a passivation layer.
[0009] The passivation layer shields the carbon nanotubes from direct contact with the electrode material and / or the electrolyte material. The passivation layer comprises a first composition that allows electrons to be transported to / from the structure of the agglomerated carbon nanotubes.
[0010] The first composition may include a metal or metal alloy selected from aluminum, nickel, copper, silver, gold, palladium, platinum or a combination of two or more thereof, preferably aluminum. Alternatively or additionally, the first composition includes an electrical insulator having a thickness and resistivity configured to form a tunnel junction with the structure (6) of agglomerated carbon nanotubes.
[0011] The passivation layer defines an outer wall that encapsulates the structure of the agglomerated carbon nanotubes, shielding it from the base at the conductive substrate current collector along its sidewalls, up to and including the top surface of the structure's distal end, at the top away from the substrate. An elongated gap structure is defined in the complementary space between the opposing sidewalls.
[0012] As will be explained in more detail herein, the electrodes disclosed herein can be advantageously used in a variety of applications or configurations, including but not limited to anodes comprising the above-mentioned electrodes, cathodes comprising the above-mentioned electrodes, and energy storage devices comprising the above-mentioned electrodes, such as one or more anodes and cathodes included therein or as one or more anodes and cathodes therein. Typically, these applications / configurations involve supplying one or more subsequent functional material layers along the outer surface of the current collector to form a multi-layer stack, such as a lithium metal battery multi-layer. Therefore, the upright support element can be understood as supporting one or more subsequent functional material layers, such as battery active layers, while providing the function of distributed power collection / distribution to / from subsequent layers. In addition, as will be explained in more detail below, the upright support element can be understood as improving the uniformity of the electric field, improving the uniformity of the distribution of anode and / or cathode materials, reducing the formation of dendrites, reducing the irreversible loss of anode materials during battery manufacturing and / or battery cycling, and / or reducing the power density loss at the end of the battery life.
[0013] Other aspects of the present disclosure relate to an energy storage device, such as a lithium metal battery, comprising the electrode disclosed herein.
[0014] A further aspect relates to a method of manufacturing an electrode and / or battery as disclosed herein. The method includes providing a 3D composite substrate current collector having a conductive substrate current collector and a plurality of laterally distributed agglomerated carbon nanotube structures, which are substantially parallel oriented in a direction away from the substrate, and forming a plurality of laterally distributed conductive support elements with upright sidewalls by covering the agglomerated carbon nanotube structures with a passivation layer of a first composition, the passivation layer being used to shield the carbon nanotubes from direct contact with an electrode or electrolyte material (e.g., an anode metal composition or an electrolyte composition) while allowing electrons to be transported to / from the agglomerated carbon nanotube structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] These and other features, aspects, and advantages of the apparatus, systems, and methods of the present disclosure will become better understood through the following description, appended claims, and accompanying drawings, in which:
[0016] Figure 1A depicts a cross-sectional side view of an electrode disclosed herein;
[0017] Figure 1B depicts a partial cross-sectional side view of an embodiment of an electrode disclosed herein;
[0018] Figure 2A and Figure 2B depicts a partial cross-sectional side view of an embodiment of a 3D anode comprising an electrode disclosed herein;
[0019] Figure 3A depicts a cross-sectional top view of an electrode disclosed herein;
[0020] Figure 3B , Figure 4A and Figure 4B Various embodiments of a 3D anode including an electrically insulating cap are depicted;
[0021] Figure 5A Other aspects of the electrodes disclosed herein are shown;
[0022] Figure 5B depicts a cross-sectional side view of an electrode disclosed herein;
[0023] Fig. 6A schematically illustrates an exploded side view of a battery including an electrode disclosed herein;
[0024] Figure 6B and Figure 6C Other aspects of the electrodes disclosed herein are shown;
[0025] Fig. 7A schematically illustrates a method of making the electrodes disclosed herein; and
[0026] Figure 7B Schematic top views of aspects related to the fabrication of the electrodes disclosed herein are provided. DETAILED DESCRIPTION
[0027] The terms used to describe specific embodiments are not intended to limit the present disclosure. As used herein, the singular forms "a", "an", "the" are also intended to include the plural forms, unless the context clearly indicates otherwise. The term "and / or" includes any and all combinations of one or more of the relevant listed items. It should be understood that the terms "comprise" and / or "comprising" stipulate the presence of the features, but do not exclude the presence or increase of one or more other features. It should be further understood that when a particular step of a method is referred to as being after another step, unless otherwise stated, it may be directly after the other step, or one or more intermediate steps may be performed before performing the particular step. Similarly, it should be understood that when describing a connection between structures or components, unless otherwise stated, the connection may be established directly or through an intermediate structure or component.
[0028] As used herein, the terms anode and anode composition may be understood to relate to elements and materials that, in the normal discharge procedure of the battery, act as negative electrode materials, respectively, releasing electrons in an electrochemical oxidation reaction with the anode / anode material, which acts as an acceptor / reducing material. The terms cathode and cathode composition relate to the corresponding counterparts (positive electrode / electron acceptor). In the charging procedure, the roles of the oxidant / reducing agent are clearly reversed.
[0029] Hereinafter, the present disclosure is described more fully with reference to the accompanying drawings, in which embodiments of the present disclosure are shown. In the accompanying drawings, the absolute and relative sizes of systems, components, layers, and regions may be exaggerated for clarity. The embodiments may be described with reference to schematic and / or cross-sectional diagrams of possible idealized embodiments and intermediate structures of the present disclosure. In the specification and drawings, like numbers always represent like elements. Related terms and their derivatives should be interpreted as referring to the directions shown in the drawings being described or discussed at the time. These related terms are for ease of description and do not require the system to be constructed or operated in a specific direction unless otherwise specified.
[0030] Figure 1A A cross-sectional side view of an electrode 1 disclosed herein is depicted. The electrode includes a 3D composite current collector 2. The current collector includes a conductive substrate current collector 3 having a plurality of laterally distributed conductive upright support elements 4. The support elements 4 include a structure 6 of agglomerated carbon nanotubes 7, which is substantially parallel oriented in a direction away from the substrate 3. The structure 6 of agglomerated carbon nanotubes is covered by a passivation layer 10, which is used to shield the carbon nanotubes 7 from direct contact with the electrode material (e.g., anode metal) and / or electrolyte, wherein the passivation layer 10 includes a first composition 10c that allows electrons to be transported to / from the structure of the agglomerated carbon nanotubes. The passivation layer 10 defines an outer wall, including side walls 5 of the upright support elements. Between adjacent support elements 4, elongated gap structures 5i provide space for subsequent functional layers.
[0031] Advantageously, the conductive substrate may be provided as a flexible metal foil, such as a copper foil, or as Figure 1B , Figure 5A , Fig. 6A and Figure 6B As shown, it is provided as a metal-coated flexible carrier 3c, such as a metal-coated plastic film. The flexible metal foil and / or metal-coated carrier advantageously allows the electrode to be rolled, follow the geometry of the external 3D-shaped carrier, and / or reduce the manufacturing time by supporting a roll-to-roll manufacturing process.
[0032] It should be understood that the shape and size of the support element 4 can depend on the application. Typically, the height s7 of the structure 6 of the agglomerated carbon nanotubes is at least 2 μm. The higher the structure, the more obvious the effect of 3D current collection, for example, the amount and volume of electrode material that can be electrically connected to the current collector. The upper limit can be defined only by process limitations. For example, limitations on providing carbon nanotube structures exceeding a certain upper limit (e.g., >100 microns (μm)), and / or limitations on providing conformal coatings on the structural substrate. It has been found that structures with a height in the range of 5 μm to 50 μm achieve a practical balance between device performance (such as total capacity) and manufacturing complexity.
[0033] A buffer layer is usually provided between the conductive substrate current collector and the carbon nanotubes, and the carbon nanotubes grow from the buffer layer. As is known in the art, the buffer layer usually includes an oxide layer, which can be a conductive oxide, on which catalyst seed particles that catalyze the growth of the carbon nanotubes are provided. Depending on the growth conditions, catalyst residues can be left at the bottom interface of the carbon nanotubes (base-type carbon nanotube growth) and / or catalyst residues can be present at the ends of the carbon nanotubes (tip-type growth).
[0034] The lateral spacing w1 between the opposite side walls 5 of the adjacent agglomerated structures 6 of the carbon nanotubes 7 determines the size of the gap structure 5i, and thus determines the volume available for deposition of subsequent electroactive material layers (e.g., electrode or electrolyte materials). The closer the positions of the adjacent support elements are, the more uniform the current collection from the subsequent covering layer is. The farther the adjacent support elements are spaced, the smaller their lateral size is, the larger the volume available for the subsequent functional electroactive material layer is, and the smaller their relative contribution to the carbon nanotubes is.
[0035] It was found that a practical range of lateral dimensions of the structures, such as the cross-sectional spacing w2 between the opposing sidewalls 5 of the agglomerated structures 6, is in the range of 0.1 μm to 20 μm. The thinner the structure, the smaller the contribution of the carbon nanotube structure to the total weight and volume relative to the electroactive material disposed on top and between the structures. It was found that a value of about 100 nm constitutes a practical lower limit for a practical balance between increased reduction and manufacturing complexity.
[0036] The shape of the support element may include one or more isolated structures, such as pillars or columns, wall structures, having elongated dimensions in the lateral direction along the substrate; patterned (e.g., sawtooth) wall sections, wall structures, and interconnected wall structures. While pillar structures may provide the largest surface area per unit volume of carbon, support elements with a smaller surface area / volume ratio, such as structures having dimensions extending laterally in the direction along the substrate, such as wall sections, patterned wall sections (e.g., sawtooth) or even interconnected wall sections, may advantageously provide a higher resilience to forces in the lateral direction (e.g., bending). Figure 7B (Right) A top view of an exemplary structure of agglomerated carbon nanotubes arranged in a hexagonal pattern is provided.
[0037] The passivation layer 10 includes or is substantially composed of a first composition 10c that allows electrons to be transported to / from the structure of the agglomerated carbon nanotubes. The passivation layer of the first composition 10c extends along the outer surface of the structure of the agglomerated carbon nanotubes from the base at the conductive substrate current collector to and including the terminal and tip of the structure. Obviously, the passivation layer can also extend along the conductive substrate current collector 3 between adjacent structures 6 of agglomerated carbon nanotubes.
[0038] Advantageously, the passivation layer 10 can form a substantially closed coating and shell while allowing electron transport capabilities to / from the structure of agglomerated carbon nanotubes. Providing a substantially closed shell mitigates foreign matter (e.g., electroactive materials) from contacting individual carbon nanotubes 7 and entering the internal volume 7i within the structure (i.e., between adjacent carbon nanotubes 7).
[0039] Thus, the application of the shielding coating 10 was found to: mitigate the degradation of the current collecting capacity of the carbon nanotube structure due to interactions between the carbon nanotubes (e.g., irreversible chemical reactions) or even prevent degradation of the current collecting capacity, particularly at defect sites, due to direct contact with electroactive materials (particularly high reactance anode metal compositions). Additionally, it was found that the shielding coating 10 minimized the loss of functional electroactive materials (e.g., anode metals) due to interactions with the carbon nanotubes. Further, it was found that the shielding coating 10 mitigated volume changes within the agglomerated structure 6 by hindering or substantially preventing the penetration of electrode metal / metal ions into the interior 7i of the structure 6 of the agglomerated carbon nanotubes 7, thereby improving the structural integrity of the support 4 and extending the cycle life of the electrochemically active device including the electrode 1.
[0040] Advantageously, a passivation layer 10 can be provided so that the penetration of the passivation material through the outermost portion surrounding the inner core within the structure of the agglomerated carbon nanotubes can be minimized, so that the coating material forms a shell, whereby the voids defined as the spaces between adjacent agglomerated carbon nanotubes at the central portion of the structure can remain substantially free of coating material 10c. Obviously, the shielding material can penetrate to some extent between the carbon nanotubes in the outermost portion of the structure of the agglomerated carbon nanotubes to form a composite zone. However, as will be explained in more detail below, the thickness of the composite zone can be much less than 25 nm, for example <5 nm or less, leaving a core in which the agglomerated carbon nanotubes can remain uncoated. Confining the passivation composition to the outermost portion of the structure advantageously minimizes the total weight per unit volume of the electrode while maintaining current collection / distribution performance.
[0041] Typically, the passivation layer 10 comprises or consists essentially of a composition referred to as a first composition 10c, which has reduced reactivity toward carbon nanotubes, particularly defect sites, relative to the anode or cathode composition and the corresponding electrolyte composition with which the electrode is in contact. Preferably, the composition 10c is selected so as to have a significantly reduced, preferably negligible, electrochemical activity at normal operating potentials.
[0042] The inventors have discovered that the purpose of providing a closed passivation layer 10 for shielding carbon nanotubes 7 from direct contact with external materials while allowing electrons to be transported to / from the structure 6 of agglomerated carbon nanotubes can be achieved by a conductive composition.
[0043] Thus, in some embodiments, the first composition 10c (included in or consisting essentially of the passivation layer) includes or consists essentially of a metal, a metalloid, or a mixture of one or more metals and / or metalloids, such as an alloy.
[0044] The metal- and / or metalloid-based composition for the passivation layer 10 is generally selected from elements with an electronegativity > 1.5 on the Pauling scale. The preferred composition 10c may include or consist essentially of elements selected from the late d-block and early p-block of the periodic table (i.e., Groups 9 to 14 of the periodic table). In order to shield the carbon nanotubes 7 from direct contact with the electrode or electrolyte material (electroactive material) (e.g., anode metal composition), for example, metals selected from alkaline and / or alkaline earth metals, including but not limited to Li, Na, K and Mg, the metal- and / or metalloid-based composition for the shielding layer is preferably formed from a significantly more noble composition, which includes or preferably consists essentially of elements selected from nickel, copper, silver, gold, palladium, platinum and combinations thereof, and copper, nickel and their alloys are most preferred from a practical and / or economic point of view. In order to shield the carbon nanotubes 7 from direct contact with the cathode composition and / or electrolyte, similar compositions can be used in principle according to the findings, wherein aluminum is found to be particularly stable and copper is found to be less preferred because of its relatively low electrochemical stability, especially at high operating potentials (>3V). The thickness of the metal or metalloid-based passivation layer 10 is at least to provide a functionally closed, conformal covering layer. Suitable deposition techniques include deposition methods based on dry vapor deposition, such as physical vapor deposition (PVD) and atomic layer deposition (ALD), and optionally wet deposition techniques, such as electrochemical deposition or electroplating, to increase the thickness of the passivation layer 10. In absolute terms, a metal or metalloid-based passivation layer can already be formed with a thickness of about 2 nm. In order to reduce the density of point defects, the thickness is preferably>5 nm. Thicker layers, such as>10 nm,>25 nm, and even>100 nm, are effective. However, in order to minimize the contribution of the passivation layer to the overall quality of the electrode, the thickness of the metal or metalloid-based passivation layer is preferably <200 nm, such as in the range of 5 nm to 10 nm, 5 nm to 20 nm, 5 nm to 50 nm, 10 nm to 50 nm, or 10 nm to 100 nm.
[0045] The inventors surprisingly discovered that the purpose of providing an effective passivation layer 10 that shields the carbon nanotubes from direct contact with external materials while allowing electrons to be transported to / from the structure of the agglomerated carbon nanotubes can also be achieved by compositions that are generally considered to be electrically insulating, as long as these layers are functionally thin, allowing electrons to tunnel through the coating while shielding the underlying carbon nanotubes from direct contact with external materials. Therefore, in some embodiments, the first composition 10c includes or consists essentially of an electrically insulating composition, such as a metal and / or mixed metal oxide.
[0046] Suitable materials include metal oxides such as HfOx, ZrOx, LaOx, SiOx, AlOx, TiOx, mixed metal oxide compositions such as SrTiOx (STO) and BaSrTiOx (BST), and mixtures of metal oxides and / or mixed metal oxides. Particularly preferred materials include silicon oxide, aluminum oxide, titanium oxide and combinations thereof, conformal layers of which can be effectively provided by atomic layer deposition. The thickness of the insulator-based passivation layer is typically <5 nm. The minimum thickness is typically >1 nm. Advantageously, the conformal insulator-based passivation layer 10 can be as thin as five monolayers. Advantageously, it has been found that metal oxide-based passivation layers are particularly effective in shielding carbon nanotubes from the electrode and electrolyte compositions under both anodic and cathodic conditions.
[0047] In a preferred embodiment, especially when the electrode 1 is used as part of an anode or as an anode, the electrode 1 further comprises a seed layer 20 covering the support element 4 for receiving an anode metal composition, such as Figure 1BAs shown. Advantageously, the seed layer can be deposited directly on the support element, i.e. without an intermediate bonding layer, so that the amount of dead material per unit volume is minimized. In order to further minimize the contribution to the total weight of the electrode, the seed layer 20 is preferably functionally thin, typically in the range of about 2 nm to about 100 nm or 200 nm, preferably 5 nm to 50 nm, wherein increasingly thicker seed layers reduce the density of point defects at the expense of increasing relative weight contribution. The seed layer 20 is typically formed of a composition 20c having a high degree of match with one or more anode metal compositions selected from alkali metals and alkaline earth metals. Therefore, the seed layer 20 can be understood to provide an effective wetting layer, improving the uniformity of the anode metal layer deposited or electroplated thereon. Thereby, localized or uneven anode metal deposition is reduced or even substantially avoided, and the occurrence of lithium dendrites and / or porous (mossy) anode metal layer growth can be reduced even during long battery cycles. Therefore, providing a seed layer 10 helps achieve the purpose of improving battery safety (mitigating dendrite formation), improving cycle life and power density (mitigating porous / mossy anode metal formation). Suitable compositions include materials that are generally considered to be lithium-loving, sodium-loving, potassium-loving, etc. In some embodiments, the seed layer 20 includes or is essentially composed of a seed composition 20c alloyed with the anode metal composition, for example, having a matching degree with the anode metal, allowing a mixture with a seed element content of >10 wt% (e.g., >50%, or even 0 to 100 wt%) to be formed therewith. Particularly preferred seed compositions 20c include zinc and zinc oxide, which are found to be easily reduced to metallic zinc, for example, when initially contacted with a more positive anode metal (e.g., Li or Na), or preferably by a previous reduction step involving hydrogen. Both Zn and ZnOx-based seed layers can be advantageously provided as substantially closed conformal covering layers, for example by ALD. Of course, if the electrode is planned to be used on the cathode side of an energy storage application or as an electrode on the cathode side, a seed layer of the anode metal is not required.
[0048] In a preferred embodiment, where the electrode is used as an anode or as part of an anode, the electrode further comprises an anode composition layer, typically an anode metal composition, or a cathode composition covering a plurality of support elements. For an anode composition, the electrode is also referred to herein as a prefilled anode or a prefilled 3D anode. For a cathode composition, the electrode is also referred to herein as a prefilled cathode or a prefilled 3D cathode.
[0049] Figure 2AA partial cross-sectional side view of an embodiment of an electrode 1 including an anode metal layer 30 is depicted. The anode metal layer includes or consists essentially of an anode metal composition 30c. As shown, the layer is provided directly on top of the seed layer 20 and forms a uniform covering layer on the support element. The anode metal layer 30 also extends between adjacent support elements in a direction along the adjacent support elements. By providing the anode metal composition 30c, the electrode can be advantageously configured as a pre-filled anode for energy storage applications (e.g., batteries).
[0050] In some embodiments, for example, Figure 2A As shown (left), the anode metal composition 30c layer is configured so that space is left at the gap structure 5i between adjacent support elements for subsequent battery layers, including one or more electrolytes and / or anode materials, to form a 3D battery structure, which can benefit from increased power density relative to a 2D layered battery structure due to the relatively shorter ion diffusion distances facilitated by the deposition of functional battery layers along the upright sidewalls of the support element 4.
[0051] In some preferred embodiments, the anode metal substantially fills the interstitial structure between adjacent upstanding support elements, e.g. Figure 2A (right) As shown, the support element 4 is substantially embedded in the anode metal composition 30c. The embodiment in which the support element 4 is substantially embedded in the anode metal composition 30c should be understood to constitute a planar 2D anode with an internal 3D current collecting element that provides distributed current collection and improved field uniformity, while benefiting from a passivation layer that provides chemical and mechanical stability, which can be used in battery storage applications. Compared with a 3D layered battery structure, a battery structure including a planar 2D anode can advantageously provide a relative capacity per unit volume.
[0052] Obviously, the anode metal composition may be provided directly onto the structure 6 of agglomerated carbon nanotubes, ie, without the passivation layer 10. However, such a configuration would not benefit from the advantages provided by the passivation layer disclosed herein, including improved structural and electrochemical stability.
[0053] Suitable anode materials include compositions comprising metal elements selected from the alkaline and / or alkaline earth classes.
[0054] Preferably, one or more of lithium, sodium, potassium and magnesium, wherein lithium is particularly preferred for energy storage applications that benefit from the maximum oxidation potential provided by Li. In some embodiments, the anode metal composition is an alloy including one or more elements selected from the alkaline and / or alkaline earth groups alloyed with one or more transition metal elements or metalloid elements (such as zinc). Alloying reduces the overall reactivity of the composition to oxidation, especially oxidation that occurs during electrode / battery manufacturing or assembly due to contact with the environment, at the expense of a theoretical loss in the total energy density and / or oxidation potential that can be achieved. The inventors have found that alloying an alkaline or alkaline earth-based anode metal composition with a relatively less reactive (less electronegative) metal composition (e.g., Li-Zn (90 / 10w / w) or Li-Zn (80 / 20)) may exceed the performance loss caused by oxidation of an anode metal composition consisting primarily of an alkaline or alkaline earth-based anode metal composition, particularly during manufacturing under conventional typical dry chamber manufacturing conditions (an environment with O2, N2 and CO2, but essentially no water vapor). Thus, in a preferred embodiment, the anode metal composition comprises an alloy of one or more metals selected from alkaline or alkaline earth based anode metal compositions, preferably lithium, and between 5 wt % and 30 wt % of a composition alloyed therewith, said composition comprising or consisting essentially of an element selected from Groups 12 to 14, preferably one or more of Zn, Sn, In, Al and Si, more preferably comprising at least Zn.
[0055] It will be appreciated that the anode metal layer may be suitably provided by known deposition methods, for example as a conformal cover layer or to substantially fill a gap structure, including but not limited to dry vapor deposition methods such as PVD and ALD, wet deposition processes such as fused deposition and electroplating.
[0056] Alternatively, the electrode can be manufactured without an anode metal layer. Such an electrode can be used on the anode side of an energy storage application (e.g., a lithium metal battery) by providing the anode metal through an in-situ electroplating process (conditioning step) by electroplating the anode metal onto the support by reducing the metal ions in the electrolyte composition. Electrodes without an anode metal layer can advantageously benefit from a relatively increased shelf life compared to pre-filled embodiments.
[0057] Still further alternatively, the anode or cathode composition may be provided as particles, for example by deposition as a slurry with a volatile carrier. Thus, in some embodiments, the electrode comprises particles of the anode material that at least partially fill the gap structure between the upstanding support elements. Thus, in some embodiments, the electrode comprises particles of the cathode material that at least partially fill the gap structure between the upstanding support elements. It should be understood that for embodiments comprising a covering layer having particles of anode material, the support element may advantageously also include one or more functional conformal layers (e.g., a seed layer) as described herein to improve the uniformity of electroplating of the anode metal (e.g., lithium) (e.g., during the battery charging process), and / or an electrically insulating cap 50 to reduce the electric field near the tip of the support structure.
[0058] In order to improve the electrical contact and / or ionic contact with the anode material and cathode material, respectively, in particular for electrodes comprising particles of anode material (or cathode material), the electrode is preferably further provided with a corresponding catholyte or anolyte composition. The catholyte / anolyte can advantageously bridge the ion / electron condition path between the electrode and the overlying diaphragm structure and / or solid or semi-solid electrolyte. For electrodes comprising a particulate anode / cathode material composition, the anolyte / cathode electrolyte can advantageously fill the remaining void volume between the particles, thereby further improving the electron / ion conduction between adjacent particles.
[0059] In some preferred embodiments, if the electrode comprises an anode metal composition layer, the electrode may advantageously further comprise an anode passivation layer.
[0060] Figure 2B Depicted Figure 2A A partial cross-sectional side view (left) of an embodiment of the electrode 1 is shown, further comprising an anode passivation layer 40. The anode passivation layer 40 comprises or consists essentially of a passivation composition 40c. The anode passivation layer 40 forms a conformal covering layer that shields the underlying anode metal composition 30c from direct contact with the environment. Obviously, for embodiments in which the support element 4 is substantially embedded in the anode metal composition 30c, the anode passivation layer 40 can be provided with similar benefits (e.g., as Figure 2A (shown on the right).
[0061] In order to protect the underlying anode while minimizing its electrochemical activity, the passivation layer is formed of a composition comprising or consisting essentially of an anode metal or at least an anode metal ion conductive or miscible composition having a relatively reduced reactivity to one or more (preferably all) of O2, N2, CO2 and H2O. Anode metal conductivity or anode metal ion conductive or miscible composition can be understood as a composition having a non-zero solubility by weight (usually at least 5%, more preferably, for example, >10% or >25%) to an alkaline and / or alkaline earth metal based anode metal composition and / or corresponding ions included in the anode layer. Suitable compositions include compositions comprising or consisting essentially of an element selected from Groups 12 to 14, preferably one or more of Zn, Sn, In, Al and Si, which have been found to be alloyable with the desired anode metal composition (e.g., Li, Na, Li / Na) while having a relatively reduced reactivity to at least one of O2, N2, CO2 and H2O. Most preferably, the passivation composition includes at least Zn, which is found to be particularly effective in shielding the underlying anode metal (such as Li) from degradation by O2, N2, H2O and CO2, and is suitable for layer deposition by dry deposition techniques including PVD and ALD. The passivation layer is preferably suitably thin to mitigate the reaction of the underlying anode metal composition with environmental components. Preferably, the thickness of the layer is at least 5 nm. To mitigate the point defect density, the layer can be thicker, such as>10 nm. To minimize the total weight contribution of the anode passivation layer, the thickness is preferably about 250 nm, such as 5 nm to 200 nm, 10 nm to 100 nm or 20 nm to 50 nm. In some embodiments, the passivation layer substantially includes one or more of Sn, Zn or Al, with a thickness ranging from 5 nm to 250 nm. The inventors have found that each of Sn, Zn or Al provides sufficient solubility for anode metals such as lithium and sodium, while mitigating their oxidation during electrode manufacturing and / or battery assembly under dry chamber conditions, while having a negligible effect on power density.
[0062] It should be appreciated that given the mutual solubility of the compositions comprising anode metal layer 30 and anode passivation layer 40, it may be difficult to discern a clear transition / boundary between the anode passivation layer and the anode metal layer, particularly as battery cycling (charge / discharge) increases.
[0063] Alternatively or additionally, the anode passivation layer may include a stable solid electrolyte interface (SEI) composition. SEI compositions are known in the art and may be formed due to an irreversible reaction between components of the anode metal and a corresponding electrolyte composition. In the present disclosure, it is particularly contemplated to provide a stable SEI coating by reacting with a dedicated electrolyte composition using a dedicated wet electrochemical deposition process. A number of related reports on the formation of stable SEI layers (Section 3.3) and lithium alloys (Section 3.1) are discussed in Gu et al., Engineering Reports 2021, 3:e12339, which are also incorporated herein by reference.
[0064] Figure 3A Provides such as Figure 2B A cross-sectional top view of an electrode is shown, illustrating a support element 4 comprising a conformal cover layer stack, including a seed layer 20, an anode metal layer 30, and an anode passivation layer 40. In this particular embodiment, the structure 6 of agglomerated carbon nanotubes is shaped as an isolated column having a circular cross-section. Although isolated structures in general, and isolated columns in particular, may be preferably used to provide a maximum surface area to volume ratio, it should be understood that the present disclosure should not be construed as being limited to only such structures. The inventors also expressly contemplate isolated structures of different shapes, such as having square or different polygonal cross-sections, but also contemplate structures having elongated cross-sectional dimensions in a direction along the conductive substrate current collector, such as walls, and even interconnected structures (such as interconnected wall segments), such as Figure 7B Hexagonally interconnected wall segments are shown. The interconnected structure may provide a particular benefit of relatively increased mechanical stability, for example, against bending and / or delamination, compared to isolated pillar structures.
[0065] In order to mitigate cracking or structural damage, the lateral dimensions of isolated or interconnected structures are preferably no more than 10 mm. Typically <1 mm. By limiting the lateral dimensions of the interconnected structures, it is possible to allow bending of the underlying substrate, in fact even the entire electrode, without losing basic functionality. In a preferred embodiment, the structure 6 of agglomerated carbon nanotubes is divided into sectors, each sector being separated by adjacent sectors spanning gaps. Therefore, in a preferred embodiment, the structure 6 of agglomerated carbon nanotubes is divided into sectors with lateral spacing according to the substrate bending axis. The size of the gap is typically within a lower limit of about 5 μm. Preferably, the gap is ultimately equal to the height of the carbon nanotube, for example 5 μm to 100 μm. Further spacing can support a smaller bending radius. The upper limit can be as large as several millimeters or more. Typically, the range of spacing is 5 μm to 2000 μm, preferably 50 μm to 1000 μm, and more preferably 100 μm to 500 μm.
[0066] Alternatively or additionally, for example Figure 5AAs shown, upstanding support elements 4 may be provided on opposing surfaces of the conductive substrate current collector. Figure 5A An embodiment is shown, comprising a conductive substrate current collector 3, comprising a flexible polymer carrier film 3c, which has been coated with copper films 3-1, 3-2 on opposite faces. Both faces of the conductive substrate current collector 3 have been provided with corresponding elements 4-1, 4-2 of the upright support elements 4 disclosed herein.
[0067] The support elements on opposite sides of the substrate may be coated with the same electrode material (e.g. the anode or cathode composition is the same or similar on both sides). Alternatively, one side of the support element may be provided with an anode material and the other side may be provided with a cathode material (e.g. in the case of a bipolar stack). In the case of a bipolar stack, layer 3-1 and layer 3-2 typically do not comprise the same metal (Cu). Instead, it is preferred that one side is coated with Cu and the other side is coated with another metal, preferably Al. It will be appreciated that this choice may depend on the voltage of the electrode material.
[0068] In some preferred embodiments, the electrode further comprises an electrically insulating cap. Figure 3B , Figure 4A and Figure 4B Various embodiments of a 3D anode including an electrically insulating cap are depicted. Cap 40 covers a top sector s5 of a support element. By covering the top sector of the conductive support element, the electric field at a location near the top sector of the upright support element is effectively reduced. Reducing the electric field near the top sector of the support element 4 can advantageously mitigate uneven anode metal (e.g., lithium) deposition during battery cycling. Mitigating uneven anode metal deposition near the top of the support structure can reduce or eliminate dendrite formation that can lead to short circuit conditions. According to further discoveries, mitigating uneven anode metal deposition near the top of the support structure can improve the uniformity of anode metal deposition along the uncoated sidewall sectors of the structure, which improves cycle life and / or power density during battery operation.
[0069] The cap is preferably formed of a metal or mixed metal oxide or other dielectric inorganic composition 50c. The higher the dielectric constant, the thinner the capping layer is for a given insulating effect. Preferably, the dielectric constant of the insulating composition 50c is at least about 1, more preferably, k>10 or even k>100. Suitable compositions include SiOx, AlOx, TiOx, HfOx, ZrOx, LaOx and mixed metal oxide compositions such as STO (SrTiOx), BST (BaSrTiOx), and mixtures thereof. A non-limiting description of exemplary dielectric compositions can be found in IEEE Trans. Advanced Packaging 25 (3) 454 (2002) (Jain et al.), which is incorporated herein by reference. It should be understood that the insulating cap is deposited by, for example, a dry vapor deposition method, so that the bottom of the support is substantially not covered by the cap. Typically, the cap is confined to the top of the support element. Typically, the cap extends a distance <25% of the length of the carbon nanotube over the sidewall length of the support element.
[0070] In one embodiment, the cap is provided directly on the passivation layer. Alternatively, or in addition, the cap may be provided directly on the seed layer ( Figure 4B )、Anode metal layer( Figure 4A ) or anodic passivation layer ( Figure 3B ). Preferably, the cap covers the anode metal, such as Figure 4A and Figure 3B When the cap is provided on the anode metal layer or the anode passivation layer, the anode metal 30 below the cap 40 can act as a buffer layer, supplementing the potential anode metal loss that occurs during battery operation.
[0071] As for the passivation layer 10 and the anode passivation layer 40, the cap 50 is preferably functionally thin so as to minimize the total contribution of insulating material per unit volume while significantly reducing the electron conduction to the top of the support element. Typically, the thickness of the cap layer 50 is in the range of 5 nm to 200 nm, such as 10 nm to 100 nm or 10 nm to 50 nm, whereby the thickness of the high-k dielectric composition (e.g., k>10) can be advantageously at the lower end of the above range, such as 5 nm to 20 nm or 5 nm to 10 nm.
[0072] In other embodiments, the electrode 1 further comprises an electrolyte. Figure 5B An embodiment is shown comprising an electrolyte 60 covering the support element 4. The illustrated embodiment also comprises a conformal stack of functional layers including a seed layer 20, an anode metal layer 30 and an anode passivation layer 40 (represented as a single layer for clarity).
[0073] The electrolyte 60 is usually applied to the electrode including the pre-filled amount of the anode metal composition, i.e., covering the anode metal layer. Preferably, in order to protect the anode composition from reacting with the environment, the anode layer is protected by an anode passivation layer. Alternatively, the electrolyte 60 can be applied to the electrode without pre-filling a certain amount of anode metal 30 and an anode passivation layer 40. In this case, the anode composition can be electroplated from the electrolyte to the support element by an in-situ electroplating process. The electrolyte 60 can be a solid electrolyte layer, a liquid electrolyte or a so-called semi-solid electrolyte, which includes mobile ions dispersed in a solid matrix (e.g., a polymer network (e.g., a gel) or a porous ceramic network), such as an ionic liquid and / or ions dissolved in a suitable solvent. For embodiments in which one or more subsequent layers are to be deposited on the electrolyte, a solid or semi-solid electrolyte may be particularly preferred. The electrode configuration of the present disclosure includes a substantially closed passivation layer, which advantageously allows or supports the application of a semi-solid electrolyte, and even enables the application of a liquid electrolyte having a relatively higher ion mobility than a solid electrolyte.
[0074] In some embodiments, for example, as shown, the electrolyte fills the remaining elongated gap regions between the supports. Alternatively, a solid or semi-solid electrolyte can be provided as a conformal cover layer covering the supports, so that subsequent battery layers can be provided in the remaining gap regions. In a preferred embodiment, the subsequent battery layer is an electrolyte with a relatively high ionic conductivity (e.g., a liquid electrolyte) to increase the ion diffusion rate within the structure.
[0075] It should be understood that the electrolyte 60 may also be provided as a planar layer, optionally in combination with an analyte composition, for example from an embodiment in which the electrode is configured as a planar 2D anode with an integrated 3D current collector, e.g. Figure 2A (right) shown.
[0076] Other aspects relate to an energy storage device, such as a lithium metal battery, comprising an electrode 1 disclosed herein. Advantageously, the electrode can be used in one or more of the cathode side and the anode side of the energy storage device.
[0077] Fig. 6A An exploded side view of a battery 100 including an electrode 1 disclosed herein is schematically shown. In one embodiment, for example, as shown, the electrode is included on the anode side of the battery. The cathode side can be a conventional cathode 120 including a current collector and a cathode composition. Alternatively or in addition, the electrode 1 can also be used on the cathode side of the battery, for example by providing the cathode composition above and / or between the upright support elements 4. For embodiments in which the electrode 1 is used as a current collector at the anode side of an energy storage application, the passivation layer 10 also protects the underlying carbon nanotubes. Obviously, the seed layer and the anode passivation layer are eliminated.
[0078] The separator 110 provided between the anode and the cathode physically separates the cathode from the anode, thereby preventing short circuiting while supporting ion transport. The separator 110 may include or consist essentially of an electrolyte layer, such as Figure 5B A solid or semi-solid electrolyte layer is shown. Alternatively or in addition, the separator can be provided as a porous support structure including a liquid electrolyte composition. In order to improve wetting and ion transport, a cathode electrolyte composition can be provided at the interface between the cathode and cathode sides of the separator 110, respectively. Alternatively or in addition, an anolyte composition can be provided at the relative interface between the anode and anode sides of the separator. In a preferred embodiment, the energy storage device includes a composite solid electrolyte membrane separating the anode and cathode. As explained, the anode and / or cathode can be provided as a planar 2D electrode with an integrated current collector. Alternatively, one or more of the anode and cathode, optionally both, can be configured as a conformal stacked 3D electrode comprising multiple layers of the battery.
[0079] The conductive substrate current collector 3 having respective upstanding standoff elements 4-1, 4-2 on opposite faces of the substrate may be advantageously used in energy storage products such as secondary batteries.
[0080] When opposite sides of the support elements are covered with the same electrode material (e.g., the anode or cathode composition on both sides is the same or similar), an energy storage device can be provided in which the support elements are arranged in parallel. In the parallel stack, the ionic current flows vertically from the negative electrode to the positive electrode, and the current flows vertically in the plane along the current collector to the external terminal tab (Tab).
[0081] When opposite sides of the support elements are covered on one side by an anode material and on the other side by a cathode material, an energy storage device may be provided, wherein the support elements are arranged in series (a so-called bipolar configuration).
[0082] Parallel bipolar battery stacks using planar or plate-based current collectors / bipolar plates are known in the art. Mei-Ching Pang et al. (J. Electrochem. Soc., 2021 167 160555) provide a "Comparative study of bipolar parallel solid-state lithium metal battery stacks based on thermal coupling models".
[0083] In some embodiments, an energy storage device, such as a lithium battery, is provided, comprising a plurality of electrodes 1 as disclosed herein, having upright support elements 4 on opposite sides of a conductive substrate current collector 3, wherein opposite sides of the substrate are covered with the same electrode material (i.e., anode or cathode composition), whereby the electrodes are arranged and stacked to form a parallel interconnected stack.
[0084] In a preferred embodiment, an energy storage device, such as a lithium battery, is provided, which includes a plurality of electrodes 1 as disclosed herein, wherein the electrodes 1 have upright support elements on opposite sides of a conductive substrate current collector 3, wherein one side of the opposite sides is provided with anode material and the other side is provided with cathode material, and wherein the electrodes are stacked according to a bipolar configuration.
[0085] The inventors have found that bipolar stacking advantageously generates less heat than parallel stacking, thereby allowing for relatively more relaxed thermal management. In addition, the inventors have found that bipolar stacking can advantageously provide higher power and / or more uniform power distribution because the entire stack surface area can be used to transfer current from one unit cell to an adjacent unit cell. In addition, the bipolar configuration can have a relatively high energy density because the thickness of the substrate can be relatively reduced, thereby producing a relatively high ratio of battery active components per unit volume.
[0086] For the case of bipolar staking, the conductive substrate current collector 3 preferably comprises or is substantially formed of aluminum, which is then covered / coated with a metal coating (preferably Cu) along the anode side (3-2). In a preferred embodiment, the conductive substrate current collector 3 is a flexible bimetallic foil, such as a single-sided copper-coated aluminum foil.
[0087] Advantageously, the thickness of the foil may be much lower than 200 μm, such as <100 μm or less, such as <50 μm, 5 to 50 μm or 5 to 20 μm.
[0088] It should be understood that adjacent electrodes may be separated by a solid electrolyte layer (eg, a composite solid electrolyte membrane disclosed herein) and / or other separators known in the art.
[0089] Figure 6B and Figure 6C Other aspects of the electrodes disclosed herein are shown, including a particulate anode / cathode composition comprising a plurality of discrete anode / cathode composition particles. The particulate anode / cathode composition fills the interstitial structure between adjacent upright support elements 4. To achieve electrical contact, the particulate anode / cathode composition may include an electrically conductive and / or ionically conductive matrix. Advantageously, the particulate anode / cathode composition may be deposited from a slurry including a volatile carrier liquid, for example, after the passivation layer 10 is deposited. Figure 6B An embodiment is shown in which the electrode 1 is configured as an anode, whereby the interstitial structures 5i between adjacent support elements are filled with particles comprising or consisting essentially of an anode metal composition 30c (e.g., Li). The support element 4 may advantageously include a seed layer 20 (not shown) to improve uniformity of anode metal plating during battery cycling. Figure 6CAn embodiment is shown in which the electrode 1 is configured as a cathode, whereby the interstitial structures 5i between adjacent support elements are filled with particles comprising or consisting essentially of a cathode composition 120c. For the anode, the structure 6 of agglomerated carbon nanotubes is protected from direct contact with the cathode material and / or the electrolyte by a passivation layer 10c-2. In contrast to the anode-side application, the passivation layer 10c-2 preferably comprises or consists essentially of aluminum 10c-2.
[0090] Other aspects relate to methods of making the electrodes disclosed herein. Fig. 7A Schematically shown, method 200 includes at least the following steps: providing 205 a 3D composite substrate current collector having a conductive substrate current collector including a plurality of laterally distributed agglomerated carbon nanotube structures that are substantially parallel oriented in a direction away from the substrate; and forming a plurality of laterally distributed conductive support elements having upright sidewalls by covering the agglomerated carbon nanotube structures with a passivation layer of a first composition at 210, the passivation layer being used to shield the carbon nanotubes from direct contact with an electroactive material (e.g., an anode metal) while allowing electrons to be transported to / from the agglomerated carbon nanotube structures. The agglomerated tube structures may be appropriately covered by the first composition using known dry deposition methods, including but not limited to atomic layer deposition (ALD), spatial atomic layer deposition (sALD), and physical vapor deposition (PVD), such as ionized physical vapor deposition (iPVD). ALD-based methods can advantageously form a conformal capping layer that encapsulates the underlying carbon nanotubes after only a few deposition cycles (e.g., >5 deposition cycles), thereby producing a thin passivation layer (<5 nm) that has suitable conductivity even for materials that are traditionally considered to be electrical insulators (e.g., SiOx and AlOx). Optionally, after the deposition of the first composition, a reduction step (e.g., under a hydrogen environment) can be performed to at least partially convert the (reduced) composition (e.g., ZnO) into a relatively more conductive metallic form. Alternatively or in addition, the passivation layer, in particular the first composition based on the SEI, can be provided by a wet deposition method (including but not limited to electroplating).
[0091] After the passivation layer deposition 210, the process may subsequently include the step of depositing 220 a seed layer on the formed upstanding support elements. As mentioned above, the seed layer may conveniently be deposited directly on the passivation layer by a dry deposition method.
[0092] In some embodiments, the method includes the step of depositing 230 an anode metal layer, preferably directly deposited on the formed seed layer. The anode metal layer can be deposited by known methods, including but not limited to dry deposition methods such as ALD and PVD, and wet deposition methods such as electroplating. Alternatively, the anode or cathode composition can be deposited as particles from a slurry including a suitable volatile carrier solvent, such as Figure 6B shown.
[0093] In some preferred embodiments, the method further comprises covering 240 the anode metal layer or particles with an anode passivation layer. The anode passivation layer may be provided by a dry deposition process, optionally followed by or in combination with a reduction process (eg, using hydrogen) to reduce the formed oxide to a metallic composition.
[0094] In other or further preferred embodiments, the method includes the step of covering 250 the top of the upright scaffolding element by an electrically insulating cap. The cap may be suitably provided by a dry deposition method (or by ALD), such as physical vapor deposition at a shallow angle, to mitigate deposition of the insulator along the base of the structure, thereby controlling the device to restrict deposition to the top of the scaffolding element, for example by underexposing the structure (e.g., for a limited time and / or concentration) to achieve complete conformal coverage of the scaffolding element. In some embodiments, for example, Fig. 7A and Figure 3B As shown, the cap is provided after providing the anode passivation layer. Alternatively or in addition, between step 230 and step 240 (e.g., Figure 4A ), between step 220 and step 230 (for example, as Figure 4B The cap may be provided as shown) or between step 210 and step 220, i.e. directly on the formed upright support element.
[0095] A substrate current collector having a conductive substrate current collector can be formed by methods known in the art, the conductive substrate current collector comprising a plurality of laterally distributed agglomerated carbon nanotube structures that are substantially parallel oriented in a direction away from the substrate, including micropatterning of dense carbon nanotube structures. In a preferred embodiment, a plurality of laterally distributed agglomerated carbon nanotube structures that are substantially parallel oriented in a direction away from the substrate are formed, including a step of growing 202 carbon nanotubes from a buffer layer provided along a surface of the conductive substrate current collector, the buffer layer comprising an oxide layer and a catalyst or seed particles distributed for growing carbon nanotubes. After growing the carbon nanotubes, an aggregate structure of carbon nanotubes can be formed by agglomerating 203 the formed single carbon nanotube forest into a condensed aggregate structure, for example by known methods including thermal aggregation and capillary agglomeration, for example by exposure to a volatile solvent and then evaporating the solvent.
[0096] The degree of aggregation (DOA) can be characterized as the percentage of the void fraction between adjacent carbon nanotubes within the structure relative to the initial void fraction (i.e., before densification). Here, DOA = 0% corresponds to a non-aggregated condition with a 100% void fraction (virgin carbon nanotubes (VACNT)). Therefore, in a preferred embodiment, the DOA is at least 5%, preferably >20%, and most preferably greater, such as >40% or even greater than 60%. The smaller the remaining void fraction within the agglomerated structure, the greater its structural integrity and the greater the volume fraction of active material in the device.
[0097] In order to control the size and spacing of the carbon nanotube structure, the method may include patterning 201 the buffer layer, for example, by a micro-patterning method such as mask lithography.
[0098] Figure 7B (Left) schematically shows a partial top view of a conductive substrate current collector 3, which includes a patterned buffer layer 7b and individual vertically oriented carbon nanotubes 7 grown from the buffer layer before aggregation. Figure 7B (Right) shows the same area after capillary aggregation. As shown, the carbon nanotubes are aggregated in hexagonal wall segments with a relatively high density of carbon nanotubes per unit area (the void volume between adjacent carbon nanotubes is significantly reduced). Of course, the aggregation method can be used to make a wide range of structures in addition to the embodiment shown.
[0099] For clarity and simplicity of description, features are described herein as part of the same or different embodiments; however, it should be understood that the scope of the present invention may include embodiments having a combination of all or some of the described features.
[0100] In interpreting the appended claims, it should be understood that the word "comprising" does not exclude the presence of other elements or actions than those listed in a given claim; the word "a" or "an" preceding an element does not exclude the presence of a plurality of such elements; any figure numerals in the claims do not limit their scope; some "devices" may be represented by the same or different items or structures or functions implemented; unless otherwise specifically stated, any of the disclosed devices or parts thereof may be combined together or separated into further parts. Where one claim refers to another claim, this may represent a synergistic advantage achieved by a combination of their respective features. However, the mere fact that certain measures are recited in mutually different claims does not mean that a combination of these measures cannot be used simultaneously. Therefore, the present embodiment may include all working combinations of the claims, wherein each claim may in principle refer to any preceding claim unless the context clearly excludes it.
Claims
1. An electrode (1), comprising: A 3D composite current collector (2) comprises a conductive substrate current collector (3), wherein the conductive substrate current collector has a plurality of laterally distributed conductive upright support elements (4); wherein the support element (4) comprises a structure (6) of agglomerated carbon nanotubes (7) oriented substantially in parallel in a direction away from the substrate, wherein the structure of agglomerated carbon nanotubes is covered by a passivation layer (10) for shielding the carbon nanotubes (7) from direct contact with electrode material and / or electrolyte material, wherein the passivation layer (10) consists of a first composition (10c) that allows electrons to be transported to or from the structure of agglomerated carbon nanotubes; Wherein, the first composition (10c) comprises a metal or metal alloy selected from aluminum, nickel, copper, silver, gold, palladium, platinum or a combination of two or more thereof, preferably aluminum; or The first composition (10c) includes an electrical insulator having a thickness and a resistivity configured to form a tunnel junction with the agglomerated carbon nanotube structure (6).
2. The electrode according to claim 1, wherein The thickness of the electrical insulator is in the range of 1 nm to 5 nm.
3. An electrode according to any one of the preceding claims, wherein The electrode (1) comprises a seed layer (20) covering the support element (4), the seed layer being adapted to receive an anode metal composition (30c).
4. The electrode according to claim 3, wherein The seed layer (20) includes a composition (20c) selected for alloying with the anode metal composition (30c).
5. The electrode according to any one of the preceding claims, further comprising an anode metal layer (30) covering a plurality of the support elements (4).
6. The electrode according to claim 5, further comprising an anode passivation layer (40), wherein: The anode passivation layer (40) includes a metal or metalloid composition (40c) alloyed with the anode metal composition (30c).
7. The electrode according to any of the preceding claims, further comprising an electrically insulating cap (50) covering the top (s4) of the support element (4).
8. The electrode according to claim 7, wherein The electrical insulating cap (50) is arranged on the anode passivation layer (40), between the anode metal layer (30) and the anode passivation layer (40), or on the seed layer (20).
9. The electrode according to any of the preceding claims, further comprising an electrolyte (60) covering the support element (4).
10. An electrode according to claim 1 or 2, comprising particles of anode or cathode material (30c, 120c).
11. An electrode according to any one of the preceding claims, wherein The height of the agglomerated carbon nanotube structure (6) is in the range of 5 μm to 50 μm; The lateral dimension (w2) (thickness) of the structure (6) of the agglomerated carbon nanotubes is in the range of 0.1 μm to 20 μm; and The spacing distance (w1) between the opposite side walls (5) is in the range of 0.2 μm to 20 μm.
12. The electrode (1) according to any one of the preceding claims, wherein The conductive substrate (3) is provided as a flexible metal foil or a metal-coated flexible carrier.
13. The electrode (1) according to any one of the preceding claims, wherein The structure (6) of agglomerated carbon nanotubes is segmented into sectors having lateral spacings that are aligned with the substrate bending axis.
14. An electrode (1) according to any one of the preceding claims, comprising respective support elements (4-1, 4-2) on opposite sides of the conductive substrate (3).
15. An energy storage device (100) comprising an electrode (1) according to any one of the preceding claims.
16. The energy storage device according to claim 15, wherein: The storage device includes a composite solid electrolyte membrane separating opposing anode and cathode sides of the storage device.
17. An energy storage device according to claims 15 to 16, comprising a plurality of electrodes according to claim 14 arranged in a bipolar battery stack.
18. A manufacturing method comprising: A 3D composite substrate current collector (2) is provided, the 3D composite substrate current collector having a conductive substrate current collector (3), the conductive substrate current collector comprising a structure (6) of a plurality of laterally distributed agglomerated carbon nanotubes (7) oriented substantially in parallel in a direction away from the substrate, and forming a plurality of laterally distributed conductive support elements (4) having upright sidewalls (5) by covering the structure of agglomerated carbon nanotubes with a passivation layer (10) of a first composition (10c), the passivation layer being used to shield the carbon nanotubes (7) from direct contact with electrode materials or electrolyte materials while allowing electrons to be transported to or from the structure of agglomerated carbon nanotubes; Wherein, the first composition (10c) comprises a metal or metal alloy selected from aluminum, nickel, copper, silver, gold, palladium, platinum or a combination of two or more thereof, preferably aluminum; or The first composition (10c) includes an electrical insulator having a thickness and a resistivity configured to form a tunnel junction with the agglomerated carbon nanotube structure (6).
Citation Information
Patent Citations
Anode structure for a lithium metal battery
US10741835B1