Degradable piezoelectric artificial blood vessel and preparation method thereof
By designing a degradable piezoelectric artificial blood vessel and using the piezoelectric functional layer of the molecular ferroelectric material fiber membrane, the problems of non-degradability and insufficient mechanical strength of traditional piezoelectric sensors have been solved, and in-situ blood pressure monitoring and mechanical performance improvement have been achieved. Detection sensitivity and durability.
Patent Information
- Application Number
- CN202410811250.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Existing piezoelectric sensors are not degradable and require a second surgery to remove them, and are prone to loss of sensitivity. Moreover, the introduction of traditional piezoelectric materials reduces the mechanical strength and biocompatibility of artificial blood vessels, affecting the blood pressure monitoring effect.
A degradable piezoelectric artificial blood vessel is designed, including a first guiding layer, a piezoelectric functional layer and a second guiding layer. The piezoelectric functional layer uses a fiber membrane adsorbed with molecular ferroelectric materials. The fiber membrane is arranged along the circumference of the blood vessel. , avoiding direct contact between molecular ferroelectric materials and body fluids, improving detection sensitivity and mechanical properties.
It achieves in-situ real-time monitoring of postoperative blood pressure, improves the durability and detection sensitivity of molecular ferroelectric materials, enhances the mechanical properties of artificial blood vessels, avoids secondary operations, and reduces patient pain.
Smart Images

Figure CN118787481A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piezoelectric sensing and artificial blood vessel preparation, and in particular to a degradable piezoelectric artificial blood vessel and a preparation method thereof. Background Art
[0002] In the treatment of vascular diseases, artificial blood vessel replacement is the only solution to rescue high-risk critically ill patients, but artificial blood vessels often have risks such as anastomotic embolism and calcification after implantation. Vascular calcification reduces vascular elasticity and causes an increase in vascular elastic modulus, and thrombosis causes blood flow to slow down, both of which can lead to abnormally high blood pressure at the artificial blood vessel replacement site. Therefore, early detection of postoperative abnormalities, timely warnings, and effective intervention are the key to improving the success rate of artificial blood vessel replacement surgery.
[0003] Currently, abnormal blood pressure is mainly detected by implanting piezoelectric sensors with real-time blood pressure monitoring function.
[0004] However, existing piezoelectric sensors have the following defects: 1) Traditional piezoelectric materials such as piezoelectric ceramics represented by lead zirconate titanate (PZT) and barium titanate (BTO) contain heavy metal elements, poor biological activity, low degree of endothelialization, and poor compliance, while piezoelectric polymers represented by polyvinylidene fluoride (PVDF) are usually non-degradable. The above materials do not meet the requirements of artificial blood vessels and are usually directly implanted in blood vessels, requiring a second surgery to remove; 2) The introduction of hard piezoelectric materials such as piezoelectric ceramics will reduce the mechanical strength of flexible artificial blood vessels, making them prone to cracking and failure under multiple blood pressure shocks; 3) After the piezoelectric sensor enters the body fluid environment, since the body fluid environment is a non-insulating system containing electrolytes, it is easy to cause the bound charge generated by the piezoelectric material in the piezoelectric sensor to be neutralized, seriously affecting its sensitivity, and even causing the sensor to fail, affecting the monitoring effect. Summary of the invention
[0005] The main purpose of the present invention is to provide a degradable piezoelectric artificial blood vessel and a preparation method thereof, aiming to solve the problems in the prior art that implantable piezoelectric sensors are non-degradable, require secondary surgery to remove, and are prone to loss of sensitivity.
[0006] To achieve the above object, the present invention provides a degradable piezoelectric artificial blood vessel, comprising:
[0007] The first guiding layer is arranged in a tubular shape, which defines a pipeline channel for blood circulation and is used to guide blood flow, cell adhesion and tissue repair;
[0008] a piezoelectric functional layer, which is sleeved on the outer side of the first guide layer, and the piezoelectric functional layer is used to convert the radial force signal of the blood pressure into an electrical signal; and
[0009] A second guiding layer is arranged on the outer side of the piezoelectric functional layer, and the second guiding layer is used to fix the piezoelectric functional layer and guide cell adhesion and tissue repair;
[0010] Wherein, the piezoelectric functional layer comprises a fiber membrane adsorbed with molecular ferroelectric material, and at least part of the fibers in the fiber membrane are arranged along the circumference of the blood vessel.
[0011] In one embodiment, the thickness of the first guide layer is 30 μm to 100 μm; and / or,
[0012] The thickness of the piezoelectric functional layer is 100 μm to 200 μm; and / or,
[0013] The thickness of the second guide layer is 20 μm to 50 μm; and / or,
[0014] The inner diameter of the degradable piezoelectric artificial blood vessel is 2-6 mm.
[0015] In one embodiment, the piezoelectric functional layer further includes electrodes, wires and a waterproof layer, the electrodes and the wires are arranged on both sides of the fiber membrane, and the waterproof layer is arranged on a side of the electrode away from the fiber membrane.
[0016] The present invention also provides a method for preparing the above-mentioned degradable piezoelectric artificial blood vessel, comprising the following steps:
[0017] S10, mixing the oriented fiber film with a molecular ferroelectric material solution, drying, and precipitating crystals to obtain a piezoelectric functional layer;
[0018] S20, obtaining a first guide layer and a second guide layer, and nesting the piezoelectric functional layer between the first guide layer and the second guide layer, so that the first guide layer, the piezoelectric functional layer, and the second guide layer are sequentially adhered and inseparable, thereby obtaining a degradable piezoelectric artificial blood vessel.
[0019] In one embodiment, in step S10: the oriented fiber membrane comprises a single oriented fiber membrane; and / or,
[0020] The raw material of the oriented fiber membrane includes natural polymer materials, and the natural polymer materials include at least one of silk fibroin, cellulose, chitosan, collagen, hyaluronic acid and gelatin.
[0021] In one embodiment, the oriented fiber membrane is prepared by electrospinning technology.
[0022] In one embodiment, the inner diameter of the metal needle of the electrospinning technique is 0.4 to 0.6 mm; and / or,
[0023] The electrospinning technique has a push rate of 1.0 to 2.0 mL / h; and / or,
[0024] The spinning voltage of the electrospinning technology is 10 to 15 kV; and / or,
[0025] The receiving distance of the electrospinning technology is 10 to 15 cm; and / or,
[0026] The spinning temperature of the electrospinning technology is 20-40°C; and / or,
[0027] The spinning humidity of the electrospinning technology is less than 5%.
[0028] In one embodiment, in step S10: the molecular ferroelectric material includes any one of ImClO4 and [Hdabco]ClO4; and / or,
[0029] The mass concentration of the molecular ferroelectric material in the molecular ferroelectric material solution is 0.05-0.6 g / mL.
[0030] In one embodiment, in step S20:
[0031] The method for obtaining the first guide layer comprises electrospinning technology; and / or,
[0032] The method for obtaining the second guide layer comprises electrospinning technology; and / or,
[0033] The raw material of the first guide layer includes at least one of polylactic acid and polycaprolactone; and / or,
[0034] The material of the second guide layer includes at least one of polylactic acid and polycaprolactone.
[0035] The present invention proposes a degradable piezoelectric artificial blood vessel and a preparation method thereof, wherein the degradable piezoelectric artificial blood vessel comprises a first guide layer, which is arranged in a tubular shape and defines a pipeline channel for blood circulation, and is used to guide blood flow, cell adhesion and tissue repair; a piezoelectric functional layer, which is sleeved on the outside of the first guide layer, and the piezoelectric functional layer is used to convert the force signal of blood pressure into an electrical signal; and a second guide layer, which is arranged on the outside of the piezoelectric functional layer, and the second guide layer is used to fix the piezoelectric functional layer and guide cell adhesion and tissue repair; the above design avoids direct contact between molecular ferroelectric materials and body fluid environment, facilitates molecular ferroelectric materials to play the function of in vivo signal extraction, improves the durability of molecular ferroelectric materials and the sensitivity and accuracy of detection, and can realize in-situ real-time monitoring of postoperative blood pressure. Molecular ferroelectric materials are bio-friendly materials with good sensitivity, which improves the sensitivity of blood pressure detection. The piezoelectric functional layer comprises a modified molecular ferroelectric material fiber membrane, wherein some fibers are arranged along the radial direction of the blood vessel, which enhances the mechanical properties of the artificial blood vessel and improves its resistance to radial blood pressure impact and durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0037] Figure 1 This is a physical picture of the degradable piezoelectric artificial blood vessel in Example 4 provided by the present invention implanted into a rabbit's carotid artery;
[0038] Figure 2 This is a schematic diagram of the structure of the degradable piezoelectric artificial blood vessel provided in Example 1 of the present invention;
[0039] Figure 3 This is a schematic diagram of the structure of the piezoelectric functional layer in the degradable piezoelectric artificial blood vessel in Example 1 provided by the present invention;
[0040] Figure 4 The polarization hysteresis loop diagram and dielectric constant diagram of the ImClO4 material in Example 4 provided by the present invention;
[0041] Figure 5 This is a graph showing the toxicity test results of different concentrations of ImClO4 on human umbilical vein endothelial cells in Example 4 provided by the present invention;
[0042] Figure 6 This is a graph showing the toxicity test results of different concentrations of ImClO4 on smooth muscle cells in Example 4 provided by the present invention;
[0043] Figure 7 This is a microscopic morphology of a fiber membrane with a single orientation in Example 4 provided by the present invention;
[0044] Figure 8 The tensile strain curves of the oriented and non-oriented fiber membranes in Example 4 provided by the present invention;
[0045] Fig. 9 A real-time electrical signal diagram of the degradable piezoelectric artificial blood vessel according to Example 4 of the present invention following the blood flow after being implanted into the body;
[0046] Fig.10 This is a diagram showing the natural degradation results of the degradable piezoelectric artificial blood vessel in Example 4 provided by the present invention in an environment of 0.5M sodium hydroxide and 37°C.
[0047] Description of Figure Numbers:
[0048] 100. Degradable piezoelectric artificial blood vessel; 1. First guiding layer; 2. Piezoelectric functional layer; 21. Fiber membrane; 22. Electrode; 23. Wire; 24. Waterproof layer; 3. Second guiding layer.
[0049] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0050] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0051] In the treatment of vascular diseases, artificial blood vessel replacement is the only solution to rescue high-risk and critically ill patients, but artificial blood vessels often have risks such as embolism and calcification after being implanted in the body. Vascular calcification reduces vascular elasticity and causes an increase in vascular elastic modulus, and thrombosis causes blood flow to slow down, both of which can lead to abnormally high blood pressure at the site of artificial blood vessel replacement. Therefore, early detection of postoperative abnormalities, timely warnings, and effective intervention are the key to improving the success rate of artificial blood vessel replacement surgery.
[0052] At present, abnormal blood pressure is mainly detected by implanting intelligent artificial blood vessels with real-time blood pressure monitoring function. This type of degradable piezoelectric artificial blood vessels can realize in situ blood pressure monitoring.
[0053] However, the existing degradable piezoelectric artificial blood vessels have the following defects: 1) Traditional piezoelectric materials such as piezoelectric ceramics represented by lead zirconate titanate (PZT) and barium titanate (BTO) contain heavy metal elements, poor biological activity, low endothelialization, and poor compliance, while piezoelectric polymers represented by polyvinylidene fluoride (PVDF) are usually non-degradable. The above materials do not meet the requirements of artificial blood vessels and are usually directly implanted in blood vessels, requiring a secondary operation to remove; 2) The rigidity of traditional piezoelectric materials is much greater than that of natural blood vessels in the human body. The implantation of hard piezoelectric materials such as piezoelectric ceramics may reduce the flexibility of flexible artificial blood vessels. The mechanical strength of the blood vessels causes the blood vessels to become stiff, making them prone to cracking and failure under repeated blood pressure shocks; 3) A basic property of piezoelectric materials is the ability to generate electric charges under mechanical stress (i.e., piezoelectric effect). After the piezoelectric sensor is implanted in the body fluid environment, since the body fluid environment is a non-insulating system containing electrolytes such as sodium ions, the bound charges generated on the surface of the piezoelectric material in the piezoelectric sensor can easily attract and combine with counter-ions in the body fluid, resulting in rapid charge neutralization, which will not only weaken or even eliminate the original piezoelectric effect, but also seriously affect its sensitivity, and even cause the sensor to fail, affecting the monitoring effect.
[0054] In view of this, the present invention provides a degradable piezoelectric artificial blood vessel 100, comprising:
[0055] The first guiding layer 1 is arranged in a tubular shape, which defines a pipeline channel for blood circulation and is used to guide blood flow, cell adhesion and tissue repair;
[0056] a piezoelectric functional layer 2, which is sleeved on the outer side of the first guide layer 1, and the piezoelectric functional layer 2 is used to convert the radial force signal of the blood pressure into an electrical signal; and,
[0057] A second guiding layer 3 is arranged on the outer side of the piezoelectric functional layer 2, and the second guiding layer 3 is used to fix the piezoelectric functional layer 2 and guide cell adhesion and tissue repair;
[0058] The piezoelectric functional layer 2 includes a fiber membrane 21 on which molecular ferroelectric material is adsorbed, and at least part of the fibers in the fiber membrane 21 are arranged along the circumference of the blood vessel.
[0059] In the technical solution of the present invention, the degradable piezoelectric artificial blood vessel 100 includes a first guide layer 1, which is arranged in a tubular shape and defines a pipeline channel for blood circulation, which is used to guide blood flow, cell adhesion and tissue repair; a piezoelectric functional layer 2, which is sleeved on the outside of the first guide layer 1, and the piezoelectric functional layer 2 is used to convert the radial force signal of blood pressure into an electrical signal; and a second guide layer 3, which is arranged on the outside of the piezoelectric functional layer 2, and the second guide layer 3 is used to fix the piezoelectric functional layer 2 and guide cell adhesion and tissue repair; the above design avoids direct contact between molecular ferroelectric materials and the body fluid environment, facilitates the molecular ferroelectric materials to play the function of in vivo signal extraction, improves the durability of molecular ferroelectric materials and the sensitivity and accuracy of detection, and can realize in situ real-time monitoring of postoperative blood pressure. Among them, the piezoelectric functional layer 2 includes a fiber membrane 21 modified with molecular ferroelectric material, and at least part of the fibers in the fiber membrane 21 are arranged along the radial direction of the blood vessel, which enhances the mechanical properties of the artificial blood vessel, increases the ability of the artificial blood vessel to resist radial blood pressure impact, and improves the durability of the artificial blood vessel; the molecular ferroelectric material is a bio-friendly material with good sensitivity, which improves the sensitivity of blood pressure detection. Figure 1 This is a real picture of the degradable piezoelectric artificial blood vessel 100 of the present invention implanted in a rabbit's carotid artery.
[0060] As a new type of ferroelectric material, molecular ferroelectrics have the characteristics of solution preparation, no need for high-temperature sintering, low cost, and simple process. Most molecular ferroelectrics can be dissolved in inorganic solutions and are suitable for use as degradable and recyclable electronic products. The molecular ferroelectric material can spontaneously convert mechanical energy into electrical energy without the need for external power supply.
[0061] In some embodiments of the present invention, the thickness of the first guide layer 1 is 30 μm to 100 μm. The thickness of the first guide layer 1 can be 30 μm, 50 μm or 100 μm. The thickness of the first guide layer 1 within a suitable range can ensure cell adhesion and test sensitivity; when the first guide layer 1 is too thick, the blood flow impact will cause part of the radial pressure to be absorbed by it, thereby weakening the force on the piezoelectric functional layer 2, thereby reducing the sensitivity of the test.
[0062] In some embodiments of the present invention, the thickness of the piezoelectric functional layer 2 is 100 μm to 200 μm. The thickness of the piezoelectric functional layer 2 can be 100 μm, 150 μm or 200 μm. The thickness of the piezoelectric functional layer 2 within a suitable range can ensure good test sensitivity and vascular mechanical properties.
[0063] In some embodiments of the present invention, the thickness of the second guide layer 3 is 20 μm to 50 μm. The thickness of the second guide layer 3 can be 20 μm, 30 μm or 50 μm. The thickness of the second guide layer 3 within a suitable range can ensure good waterproofness and mechanical properties of the blood vessel.
[0064] In some embodiments of the present invention, the inner diameter of the degradable piezoelectric artificial blood vessel 100 is 2 to 6 mm. The inner diameter of the degradable piezoelectric artificial blood vessel 100 can be 2 mm, 5 mm or 6 mm. The inner diameter within a suitable range can ensure that the piezoelectric artificial blood vessel can efficiently extract signals in vivo, and also help promote the adhesion and growth of endothelial cells, thereby maintaining the biocompatibility and functionality of the inner wall of the blood vessel.
[0065] In some embodiments of the present invention, the piezoelectric functional layer 2 further includes an electrode 22 , a wire 23 and a waterproof layer 24 , the electrode 22 and the wire 23 are arranged on both sides of the fiber membrane 21 , and the waterproof layer 24 is arranged on the side of the electrode 22 away from the fiber membrane 21 .
[0066] The electrode 22 includes a molybdenum electrode, which combines the characteristics of biocompatibility and degradability.
[0067] The wire 23 includes a molybdenum wire. Molybdenum is a metal with strong corrosion resistance and good biocompatibility, and is particularly suitable as a conductive path in a humid environment in the body. The high melting point and good conductivity of molybdenum ensure that electrical signals can be stably transmitted even in a complex or dynamic physiological environment, providing a reliable connection guarantee for the effective operation of the piezoelectric functional layer 2.
[0068] The waterproof layer 24 includes a polylactic acid film, which is a dense and hydrophobic degradable material. As the waterproof layer 24, the polylactic acid film has good biocompatibility. The waterproof layer 24 wraps the fiber membrane 21 modified with molecular ferroelectric materials, which can avoid the contact between the molecular ferroelectric materials in the fiber membrane 21 modified with molecular ferroelectric materials and the blood environment or body fluid environment, and avoid the dissolution of molecular ferroelectric materials in water, thereby reducing the probability of leakage failure of the molecular ferroelectric materials, improving the charge utilization rate, and improving the stability of the molecular ferroelectric materials and the sensor sensitivity.
[0069] The present invention also provides a method for preparing the above-mentioned degradable piezoelectric artificial blood vessel 100, comprising the following steps:
[0070] S10, mixing the oriented fiber film with the molecular ferroelectric material solution, drying, and precipitating crystals to obtain a piezoelectric functional layer 2;
[0071] S20, obtaining a first guide layer 1 and a second guide layer 3, and nesting the piezoelectric functional layer 2 between the first guide layer 1 and the second guide layer 3, so that the first guide layer 1, the piezoelectric functional layer 2, and the second guide layer 3 are sequentially adhered and inseparable, thereby obtaining a degradable piezoelectric artificial blood vessel 100.
[0072] Step S10 includes the following steps:
[0073] S11, immersing the oriented fiber film in a molecular ferroelectric solution, drying, and precipitating crystals to obtain a piezoelectric film;
[0074] S12, fixing the wire 23 and the electrode 22 on both sides of the piezoelectric film to obtain a first piezoelectric functional layer;
[0075] S13, fixing the waterproof layer 24 on both sides of the first piezoelectric functional layer to obtain the piezoelectric functional layer 2.
[0076] In step S11, the thickness of the oriented fiber film is 100-200 μm, preferably 200 μm. The oriented fiber film is immersed in a molecular ferroelectric solution and dried and crystallized to prepare a piezoelectric film, so that the oriented fiber film guides the molecular ferroelectric orientation crystallization, thereby enhancing the piezoelectric performance of the piezoelectric functional film.
[0077] In step S12, the fixing method includes hot pressing technology, the temperature of the hot pressing is 100-120°C, and the time of the hot pressing is 5-10 minutes. The temperature of the hot pressing can be 100°C, 110°C or 120°C, and the time of the hot pressing can be 5 minutes, 7 minutes or 10 minutes. The temperature and time of the hot pressing can be within a suitable range to ensure that the wire 23 and the electrode 22 are more closely attached to the piezoelectric film, exert its piezoelectric effect, and improve the detection sensitivity.
[0078] In step S13 , the preparation method of the waterproof layer 24 includes a solution casting film forming method. Compared with the first guide layer 1 and the second guide layer 3 , the waterproof layer 24 is denser.
[0079] In step S10, the drying temperature is 20-70°C, and the drying temperature can be 30°C, 50°C or 70°C. The drying temperature within a suitable range can ensure the dryness of the piezoelectric functional layer 2, which is beneficial for subsequent implantation in a living body. Preferably, the drying temperature is 20-40°C.
[0080] It should be noted that in step S10, the fibers in the oriented fiber membrane may be unidirectional or multidirectional, ie, have multiple orientations, as long as the ability of the artificial blood vessel to resist radial blood pressure shock is increased.
[0081] In the technical solution of the present invention, preferably, all the materials used are biocompatible and degradable in vivo, which is beneficial to postoperative cell regeneration. After completing the function of early monitoring, they can be naturally degraded in the body without the need for a secondary operation to remove them, thereby improving the success rate of the operation and reducing the patient's pain.
[0082] In some embodiments of the present invention, in step S10: the oriented fiber membrane includes a single oriented fiber membrane. Compared with other membranes containing randomly oriented or multi-oriented fibers, the single oriented fiber membrane is characterized in that all fibers are neatly arranged in the same direction, and the single orientation of the fibers can significantly enhance the tensile strength and elastic modulus of the membrane along the fiber orientation direction. This is because the arrangement of the fibers forms a highly ordered structure that can more effectively disperse stress, reduce the generation and expansion of cracks, and thus improve the overall durability of the material. Secondly, the fibers are arranged in the same direction, guiding the molecular ferroelectric solution to crystallize along the fiber arrangement, enhancing the orientation of the molecular ferroelectric, and thus improving the piezoelectric performance.
[0083] In some embodiments of the present invention, in step S10, the raw material of the oriented fiber film includes natural polymer materials, and the natural polymer materials include at least one of silk fibroin, cellulose, chitosan, collagen, hyaluronic acid and gelatin. That is, the natural polymer materials can contain any one of silk fibroin, cellulose, chitosan, collagen, hyaluronic acid and gelatin, and can also contain two or more of silk fibroin, cellulose, chitosan, collagen, hyaluronic acid and gelatin at the same time, all belonging to the protection scope of the present invention. By arranging the oriented fiber film, the mechanical properties and conductive properties of the oriented fiber film are better.
[0084] In some embodiments of the present invention, the preparation method of the oriented fiber membrane includes electrospinning technology. Compared with other methods, the diameter of the fiber prepared by electrospinning technology can be as low as nanometer level, which is conducive to enhancing the sensing performance of the fiber.
[0085] In some embodiments of the present invention, the inner diameter of the metal needle of the electrospinning technology is 0.4-0.6 mm; the injection speed of the electrospinning technology is 1.0-2.0 mL / h; the spinning voltage of the electrospinning technology is 10-15 kV; the receiving distance of the electrospinning technology is 10-15 cm; the spinning temperature of the electrospinning technology is 20-40°C; and the spinning humidity of the electrospinning technology is <5%.
[0086] The inner diameter of the metal needle can be 0.4mm, 0.5mm or 0.6mm; the injection speed can be 1.0-2.0mL / h, 1.0-2.0mL / h or 1.0-2.0mL / h; the spinning voltage can be 10-15kV, 10-15kV or 10-15kV; the receiving distance can be 10-15cm, 10-15cm or 10-15cm; the spinning temperature can be 20-40℃, 20-40℃ or 20-40℃; the spinning humidity can be 4%, 3% or 1%. The parameters of the above electrospinning technology can ensure the spinning of stable, continuous and uniform fiber bundles within a suitable range.
[0087] In some embodiments of the present invention, in step S10, the molecular ferroelectric material includes any one of ImClO4 and [Hdabco]ClO4. [Hdabco]ClO4 is triethylenediamine perchlorate; ImClO4 is imidazole perchlorate. ImClO4 has excellent piezoelectric properties, and its piezoelectric voltage constant g 33 =257×10 -3 Vm / N, about the same as traditional lead zirconate titanate (PZT, g 33 =40×10 -3 Vm / N) is 6 times that of piezoelectric ceramics. ImClO4 has an ultra-low coercive field (Ec = 6.4 kV / cm, such as Figure 4 ), which is 100 times smaller than the non-degradable piezoelectric polymer PVDF (Ec=700kV / cm), which means that ImClO4 only needs a very small external electric field to be fully polarized and exhibit excellent piezoelectric properties. At the same time, ImClO4 has good cell compatibility and blood compatibility. When ImClO4 is used as an analytical ferroelectric material, the degradable piezoelectric artificial blood vessel 100 obtained achieves high-sensitivity blood pressure detection while not affecting the full degradation characteristics and mechanical strength of the artificial blood vessel.
[0088] In some embodiments of the present invention, in step S10, the mass concentration of the molecular ferroelectric material in the molecular ferroelectric material solution is 0.05-0.6 g / mL. The mass concentration of the molecular ferroelectric material in the molecular ferroelectric material solution can be 0.05 g / mL, 0.2 g / mL or 0.6 g / mL. The mass concentration within a suitable range can ensure that the degradable piezoelectric artificial blood vessel 100 material has good mechanical strength and durability. Preferably, the concentration is 0.4 g / mL.
[0089] In some embodiments of the present invention, in step S20, the method for obtaining the first guide layer 1 includes electrospinning technology, and the method for obtaining the second guide layer 3 includes electrospinning technology. The size of the first guide layer 1 and the second guide layer 3 can be better controlled by electrospinning technology.
[0090] It should be noted that the porous luminal surface of the artificial blood vessel plays an important role in stabilizing the endothelium and helping cell infiltration: the porous luminal surface enhances the penetration of the tissue surrounding the graft and plays an anchoring role.
[0091] In some embodiments of the present invention, in step S20, the raw material of the first guide layer 1 includes at least one of polylactic acid and polycaprolactone, and the raw material of the second guide layer 3 includes at least one of polylactic acid and polycaprolactone. That is, the raw material of the first guide layer 1 can be polylactic acid, polycaprolactone, or a mixture of polylactic acid and polycaprolactone. Preferably, when the raw material of the first guide layer 1 is a mixture of polylactic acid and polycaprolactone, the mass ratio of the polylactic acid to the polycaprolactone is 1:1.5, and the mass ratio of the polylactic acid to the polycaprolactone can be 1:1, 1:1.5 or 1:2. The mass ratio within a suitable range can ensure that the first guide layer 1 has biocompatibility and degradability while improving the compliance of the artificial blood vessel. Similarly, the raw material of the second guide layer 3 can be polylactic acid, polycaprolactone, or a mixture of polylactic acid and polycaprolactone. When the raw materials of the first guide layer 1 and the second guide layer 3 are both a mixture of polylactic acid and polycaprolactone, the mass ratio of polylactic acid to polycaprolactone in the second guide layer 3 and the first guide layer 1 can be different or the same. Preferably, the mass ratio is 1:1.5.
[0092] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0093] Example 1
[0094] A degradable piezoelectric artificial blood vessel 100, comprising:
[0095] The first guiding layer 1 is arranged in a tubular shape, which defines a pipeline channel for blood circulation and is used to guide blood flow, cell adhesion and tissue repair;
[0096] a piezoelectric functional layer 2, which is sleeved on the outer side of the first guide layer 1, and the piezoelectric functional layer 2 is used to convert the radial force signal of the blood pressure into an electrical signal; and,
[0097] A second guiding layer 3 is arranged on the outer side of the piezoelectric functional layer 2, and the second guiding layer 3 is used to fix the piezoelectric functional layer 2 and guide cell adhesion and tissue repair;
[0098] The piezoelectric functional layer 2 includes a fiber membrane 21 modified with ImClO4, and fibers in the fiber membrane 21 are arranged along the radial direction of the blood vessel.
[0099] The thickness of the first guide layer 1 is 30 μm; the thickness of the piezoelectric functional layer 2 is 100 μm; the thickness of the second guide layer 3 is 20 μm; and the inner diameter of the degradable piezoelectric artificial blood vessel 100 is 2 mm.
[0100] The structural schematic diagram of the degradable piezoelectric artificial blood vessel 100 and the structural schematic diagram of the piezoelectric functional layer 2 of this embodiment are shown in FIG. Figure 1 and Figure 2 shown.
[0101] Example 2
[0102] Compared with Example 1, except that the thickness of the first guide layer 1 is 50 μm, the thickness of the piezoelectric functional layer 2 is 155 μm, the thickness of the second guide layer 3 is 33 μm, and the inner diameter of the degradable piezoelectric artificial blood vessel 100 is 3.5 mm, the rest are the same as Example 1.
[0103] Example 3
[0104] Compared with Example 1, except that the thickness of the first guide layer 1 is 100 μm, the thickness of the piezoelectric functional layer 2 is 200 μm, the thickness of the second guide layer 3 is 50 μm, and the inner diameter of the degradable piezoelectric artificial blood vessel 100 is 6 mm, the rest are the same as Example 1.
[0105] Example 4
[0106] A method for preparing a degradable piezoelectric artificial blood vessel 100 comprises the following steps:
[0107] 1) Dissolve the regenerated silk fibroin in hexafluoroisopropanol, and add polycaprolactone to make a mixed solution; in this example, the mass fraction of the regenerated silk fibroin is 15%, the mass fraction of polycaprolactone is 5%, and the solvent is hexafluoroisopropanol; the electrospinning receiving substrate is aluminum foil, and the electrospinning parameters are: the inner diameter of the metal needle is 0.5 mm, the injection speed is 2.0 mL / h, the spinning voltage is 15 kV, the receiving distance is 15 cm, the spinning temperature is 40°C, and the thickness of the degradable nanofiber membrane is 100 μm.
[0108] 2) Cut the fiber membrane into a 3 cm × 3 cm square, completely immerse it in a molecular ferroelectric ImClO4 solution, dry it, and precipitate crystals to obtain a piezoelectric film. The concentration of the ImClO4 solution is 0.5 g / mL, and the immersion time is 30 minutes. The crystallization temperature is 50°C and the time is 15 minutes.
[0109] 3) Hot-pressing the wire 23 and the electrode 22 on both sides of the piezoelectric film to obtain the first piezoelectric functional layer. The electrode used is a 2cm×2cm polylactic acid-polypyrrole electrode, the wire is a molybdenum wire, the hot-pressing temperature is 120°C, and the time is 5 minutes.
[0110] 4) Prepare a polylactic acid film waterproof layer 24 with a thickness of 50 μm by solution casting, fix the polylactic acid film waterproof layer 24 on both sides of the first piezoelectric functional layer, and seal it with a sealing machine to complete the packaging of the first piezoelectric functional layer to obtain the piezoelectric functional layer 2.
[0111] 5) Dissolve polylactic acid in hexafluoroisopropanol to prepare a mixed solution, wherein the mass fraction of polylactic acid is 15%. Replace the spinning machine receiver with a metal rod with a diameter of 2 mm, and the electrospinning voltage is 10 kV. Prepare the first guide layer 1 and the second guide layer 3 with an inner diameter of 2 mm and a thickness of 50 μm.
[0112] 6) The piezoelectric functional layer 2 obtained in step 4) is rolled into a tube shape and fixed between the first guide layer 1 and the second guide layer 3 obtained in step 5).
[0113] Example 5
[0114] Compared with Example 4, there are the following differences:
[0115] In step 1), polycaprolactone is replaced by polylactic acid, the mass fraction of regenerated silk fibroin is 10%, the mass fraction of polylactic acid is 5%, and the inner diameter of the metal needle is 0.4 mm;
[0116] In step 2), the crystallization temperature is 40°C and the time is 20 minutes;
[0117] In step 3), the hot pressing temperature is 100° C. and the time is 8 minutes;
[0118] In step 5), the spinning machine receiver was replaced with a metal rod with a diameter of 2.5 mm.
[0119] Comparative Example 1
[0120] Compared with Example 4, Comparative Example 1 is the same as Example 4 except that a non-oriented fiber membrane is used.
[0121] Performance Testing
[0122] The hysteresis loop of the ImClO4 material in Example 4 was tested using the Sawyer-Tower method. The results are as follows: Figure 4 shown.
[0123] Depend on Figure 4 It can be seen that imidazole perchlorate is a standard square hysteresis loop, and the saturation polarization intensity is 9.6μC / cm at room temperature (293K). 2 , ImClO4 can reach saturation polarization under an electric field of 15kV / cm, which is 2 orders of magnitude lower than that of ferroelectric polymers, indicating that the saturation polarization electric field of ImClO4 is lower than that of ferroelectric polymers. Since ImClO4 has a lower saturation polarization electric field, the material exhibits ultra-high electrocaloric strength.
[0124] The biocompatibility of the imidazole perchlorate material in Example 4 was tested by CCK-8 cytotoxicity test. Figure 5 , Figure 6 shown.
[0125] Depend on Figure 5 It can be seen that imidazole perchlorate concentration of 1 mg / mL is considered to have no toxicity to endothelial cells; Figure 6 It can be seen that imidazole perchlorate at a concentration of 0.1 mg / mL is considered to have no toxicity to smooth muscle cells.
[0126] The fiber membrane 24 in Example 4 was observed by electron microscope, and the results were as follows: Figure 7 shown.
[0127] Depend on Figure 7 It can be seen that the fibers form a uniformly oriented structure.
[0128] The fiber membrane 24 in Example 4 and Comparative Example 1 was subjected to mechanical testing, the testing method being tensile testing, and the results are as follows: Figure 8 shown.
[0129] Depend on Figure 8 It can be seen that the oriented spinning method gives the spun membrane stronger mechanical properties.
[0130] After the degradable piezoelectric artificial blood vessel 100 in Example 4 was implanted into a living body through a rabbit carotid artery replacement surgery, the real-time electrical signal graph along with blood flow was detected. Fig. 9 shown.
[0131] Depend on Fig. 9 It can be seen that the integrated piezoelectric blood vessel can detect the heart rate, and through calculation, it can match the heart rate of the rabbit under anesthesia.
[0132] The degradable piezoelectric artificial blood vessel 100 in Example 4 was placed in a 0.5M sodium hydroxide and 37°C environment for natural degradation. The results are as follows: Fig.10 shown.
[0133] Depend on Fig.10 It can be seen that the degradable piezoelectric artificial blood vessel 100 structure is almost completely degraded after 4 days.
[0134] In summary, the degradable piezoelectric artificial blood vessel 100 provided by the present invention has good biocompatibility, strong mechanical properties and blood pressure resistance, and detection sensitivity.
[0135] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A degradable piezoelectric artificial blood vessel, characterized in that: include: The first guiding layer is arranged in a tubular shape, which defines a pipeline channel for blood circulation and is used to guide blood flow, cell adhesion and tissue repair; A piezoelectric functional layer is sleeved on the outer side of the first guide layer, and the piezoelectric functional layer is used to convert the radial force signal of the blood pressure into an electrical signal; as well as, A second guiding layer is arranged on the outer side of the piezoelectric functional layer, and the second guiding layer is used to fix the piezoelectric functional layer and guide cell adhesion and tissue repair; Wherein, the piezoelectric functional layer comprises a fiber membrane adsorbed with molecular ferroelectric material, and at least part of the fibers in the fiber membrane are arranged along the circumference of the blood vessel.
2. The degradable piezoelectric artificial blood vessel according to claim 1, characterized in that: The thickness of the first guide layer is 30 μm to 100 μm; and / or, The thickness of the piezoelectric functional layer is 100 μm to 200 μm; and / or, The thickness of the second guide layer is 20 μm to 50 μm; and / or, The inner diameter of the degradable piezoelectric artificial blood vessel is 2-6 mm.
3. The degradable piezoelectric artificial blood vessel according to claim 1, characterized in that: The piezoelectric functional layer further comprises an electrode, a wire and a waterproof layer. The electrode and the wire are arranged on both sides of the fiber membrane, and the waterproof layer is arranged on a side of the electrode away from the fiber membrane.
4. A method for preparing a degradable piezoelectric artificial blood vessel according to any one of claims 1 to 3, characterized in that: The following steps are involved: S10, mixing the oriented fiber film with a molecular ferroelectric material solution, drying, and precipitating crystals to obtain a piezoelectric functional layer; S20, obtaining a first guide layer and a second guide layer, and nesting the piezoelectric functional layer between the first guide layer and the second guide layer, so that the first guide layer, the piezoelectric functional layer, and the second guide layer are sequentially adhered and inseparable, thereby obtaining a degradable piezoelectric artificial blood vessel.
5. The method for preparing a degradable piezoelectric artificial blood vessel according to claim 4, characterized in that: In step S10: the oriented fiber membrane includes a single oriented fiber membrane; and / or, The raw material of the oriented fiber membrane includes natural polymer materials, and the natural polymer materials include at least one of silk fibroin, cellulose, chitosan, collagen, hyaluronic acid and gelatin.
6. The method for preparing a degradable piezoelectric artificial blood vessel according to claim 5, characterized in that: The preparation method of the oriented fiber membrane includes electrostatic spinning technology.
7. The method for preparing a degradable piezoelectric artificial blood vessel according to claim 6, characterized in that: The inner diameter of the metal needle of the electrospinning technology is 0.4 to 0.6 mm; and / or, The electrospinning technique has a push rate of 1.0 to 2.0 mL / h; and / or, The spinning voltage of the electrospinning technology is 10 to 15 kV; and / or, The receiving distance of the electrospinning technology is 10 to 15 cm; and / or, The spinning temperature of the electrospinning technology is 20-40°C; and / or, The spinning humidity of the electrospinning technology is less than 5%.
8. The method for preparing a degradable piezoelectric artificial blood vessel according to claim 4, characterized in that: In step S10: the molecular ferroelectric material includes any one of ImClO4 and [Hdabco]ClO4; and / or, The mass concentration of the molecular ferroelectric material in the molecular ferroelectric material solution is 0.05-0.6 g / mL.
9. The method for preparing a degradable piezoelectric artificial blood vessel according to claim 4, characterized in that: In step S20: The method for obtaining the first guide layer comprises electrospinning technology; and / or, The method for obtaining the second guide layer comprises electrospinning technology; and / or, The raw material of the first guide layer includes at least one of polylactic acid and polycaprolactone; and / or, The material of the second guide layer includes at least one of polylactic acid and polycaprolactone.
Citation Information
Patent Citations
Artificial blood vessel capable of simulating natural blood vessel to release electric signals, and preparation method thereof
CN111938867A
Novel small-diameter degradable artificial blood vessel and construction method thereof
CN112156229A
Piezoelectric sensor and preparation method and recycling and degrading method thereof
CN113091776A
Artificial blood vessel and preparation method thereof
CN116549170A
Vascular prosthesis and method for production thereof
US20050137675A1
Cited By
Silk fibroin-based piezoelectric material as well as preparation method and application thereof
CN120737363A
High-flexibility small-caliber piezoelectric artificial blood vessel sensor and in-situ preparation method thereof
CN122535145A
A high-flexibility small-bore piezoelectric artificial blood vessel sensor and an in-situ preparation method thereof
CN122535145B