Magnetic-red fine refractory iron ore separation method

Through the combined action of nanobubbles and ultrasonic waves, the problem of low recovery efficiency of iron ore with particle size less than 325 mesh and insufficient nanobubble technology in traditional processes has been solved, and the efficient recovery and flotation effect of fine-grained refractory iron ore have been achieved, and the cost has been reduced. Equipment wear and tear.

CN118788482APending Publication Date: 2024-10-18ANSTEEL BEIJING RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410645374.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-11-03
Filing Date
2024-05-23
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The traditional crushing-stage grinding-gravity and magnetic flotation combined separation process is difficult to process iron ore with a particle size less than 325 mesh, and the recovery efficiency is low. The application of nano-bubble technology in flotation is insufficient, resulting in unsatisfactory flotation results and overloaded equipment. big.

Method used

Using the combined action of nanobubbles and ultrasonic waves, nanobubble pretreatment of flotation reagents and ultrasonic pretreatment of flotation slurry can strengthen the dispersion ability of flotation reagents, improve the flotation ability of fine-grained minerals and the relationship between useful minerals and veins. Stone separation effect.

Benefits of technology

It effectively improves the recovery rate of fine-grained refractory iron ore, reduces the grade of iron in flotation tailings, expands the processing capacity of the ore particle size range, and reduces the dosage of chemicals and equipment losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788482A_ABST
    Figure CN118788482A_ABST
Patent Text Reader

Abstract

The invention relates to a magnetic-hematite fine refractory iron ore separation method. The method comprises the specific steps that (1) fine particle magnetic-hematite mixed iron ore raw ore is crushed and screened, and an ore grinding product is obtained after ore grinding and screening; 2) performing weak magnetic and strong magnetic grading operation on the ore grinding product to obtain magnetic concentrate and magnetic tailings; (3) firstly, a flotation reagent is subjected to nanobubble pretreatment, the pretreated flotation reagent is added into the magnetic concentrate, and flotation feeding ore pulp is obtained; and (4) the flotation feeding ore pulp is subjected to ultrasonic pretreatment, then reverse flotation closed-circuit operation is conducted, and reverse flotation concentrate and reverse flotation tailings are obtained. According to the method, through pretreatment of the flotation reagent through the nano bubbles and pretreatment of the flotation feeding ore pulp through the ultrasonic waves, the dispersing capacity of the flotation reagent in the ore pulp is enhanced, and the flotation capacity of micro-fine particle minerals in the ore pulp and the separation effect of useful minerals and gangue minerals in the flotation process are improved; therefore, the recycling of the micro-fine particle refractory iron ore is effectively realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mineral processing, relates to a fine-grained refractory iron ore separation technology, and particularly relates to a magnetic-hematite fine-grained refractory iron ore separation method. Background Art

[0002] Iron ore is a relatively important industrial resource for the entire international community and has a huge impact on the national economy. However, with the reduction of iron ore resources and the decline in ore quality, the characteristics of iron ore resources such as "poor, fine and mixed" have gradually emerged, the ore particle size has become finer and finer, the grinding fineness has gradually increased, and the difficulty of flotation has continued to increase, making the traditional "crushing-stage grinding-gravity magnetic flotation combined separation" process difficult to adapt, and the recovery rate has been greatly reduced.

[0003] In recent years, with the development of nanobubble technology, the application of nanobubbles in mineral flotation has become more and more common, and the stable foam properties can improve the flotation recovery effect of fine-grained minerals. For example, the "new method for efficient recovery of fine-grained refractory iron ore by microbubble flotation" disclosed in the Chinese patent document with application number CN 115041293A shows that nano-microbubble flotation can achieve efficient recovery of fine iron minerals and improve the grade and recovery rate of concentrate. However, it has been shown in practice that the application of nanobubble technology in flotation also has certain shortcomings. First, the effect of nanobubbles will have a negative effect on the flotation of coarse-grained minerals, reducing the recovery rate and grade of coarse-grained mineral flotation. When the particle size range in the flotation slurry is large, it often leads to poor overall flotation effect. Second, the flotation effect is often not ideal when the flotation agent is pretreated with nanobubbles alone, and the pretreatment of the slurry with the addition of flotation agents with nanobubbles overloads the equipment, greatly increases the equipment loss rate, and is difficult to operate for a long time.

[0004] Therefore, the development of new fine-particle iron ore sorting methods is of great significance for making full use of the global lean iron ore resources, achieving efficient recovery of iron minerals, reducing the pressure of tailings storage, and maintaining the supply of high-quality iron ore raw materials. Summary of the invention

[0005] The existing "crushing-stage grinding-gravity magnetic flotation combined separation" process is limited to purifying iron ores with a particle size range of 200 to 325 meshes, while iron ores with a particle size less than 325 meshes are difficult to process, the recovery efficiency is extremely low, and the application of nano bubble technology in flotation still has defects and other problems. The present invention provides a fine-grained iron ore separation method based on the combined action of nano bubbles and ultrasound to effectively solve the recovery efficiency of fine-grained refractory iron ore. The purpose is to strengthen the dispersibility of flotation agents in the ore pulp through the pretreatment of flotation agents with nano bubbles and the pretreatment of flotation feed slurry with ultrasound, improve the flotation ability of fine-grained minerals in the ore pulp and the separation effect of useful minerals and gangue minerals in the flotation process, thereby effectively realizing the recycling of fine-grained refractory iron ore, improving the flotation recovery rate, and reducing the grade of iron in the flotation tailings.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] The chemical composition of the fine-grained magnetic-hematite mixed ore treated by the present invention is as follows by weight: TFe 25%-35%, CaO 0.1%-1.5%, MgO 0.1%-1.5%, SiO2 30%-40%, S 0.01%-0.1%, P 0.01%-0.1%, and the remainder is impurities.

[0008] The iron phase composition of the fine-grained magnetic-hematite mixed ore treated by the present invention is as follows by weight: 25% to 35% hematite, 15% to 30% magnetite, 1% to 3% siderite, 0.1% to 1% pyrite, and the remainder is iron-containing silicate and other impurities.

[0009] Aiming at the above-mentioned fine-grained magnetic-hematite mixed iron ore, the present invention proposes a magnetic-hematite fine refractory iron ore separation method, the separation process includes crushing, grinding, magnetic separation, flotation dosing, and flotation; in the flotation dosing process, the flotation agent is pretreated with nanobubbles; in the flotation process, the flotation feed slurry is pretreated with ultrasonic waves, and the specific steps include:

[0010] 1) Grinding: The fine-grained magnetic-hematite mixed ore is crushed, screened, ground and screened to obtain the grinding product.

[0011] The fineness of the crushed product after the crushing-screening closed-circuit operation is ≤12mm, and the part >12mm is returned to the crusher for further crushing; after the crushed product undergoes the grinding-screening closed-circuit operation, the obtained grinding product has a particle size of ≤400 mesh, accounting for more than 85%.

[0012] 2) Magnetic separation: The ground ore products are subjected to weak magnetic and strong magnetic classification operations to obtain magnetic concentrate and magnetic tailings.

[0013] Among them, the concentrate obtained after weak magnetic treatment is classified, the concentrate with a particle size of less than 325 mesh enters the flotation pretreatment, and the concentrate with a particle size of ≥325 mesh is returned to the ball mill for regrinding; the tailings obtained after weak magnetic treatment are concentrated, the upper clear liquid enters the clarification tank, and the precipitated slurry enters the strong magnetic separation operation. The concentrate produced by the strong magnetic separation operation is combined with the weak magnetic separation concentrate, and enters the classification operation together to obtain the magnetic separation concentrate; the tailings from the strong magnetic separation operation are concentrated to obtain the magnetic separation tailings.

[0014] After the grinding products are subjected to weak magnetic and strong magnetic classification operations, the magnetic separation concentrate obtained contains 40% to 50% TFe by weight and the iron recovery rate is 70% to 90%.

[0015] 3) Flotation dosing: First, the flotation reagent is pretreated with nanobubbles, the mixed flotation reagent is cavitated to form nanobubbles in the flotation reagent, and the pretreated flotation reagent is added to the magnetic separation concentrate to obtain the flotation feed slurry.

[0016] The mixing method of flotation reagents is: first add inhibitor starch to the stirring barrel and stir for 2 to 3 minutes, the amount of starch added is 200 to 500 g / t magnetic concentrate; then add pH adjuster CaO and stir for 2 to 3 minutes, the amount of CaO added is 30 to 80 g / t magnetic concentrate; finally add collector sodium oleate and stir for 2 to 3 minutes, the amount of sodium oleate added is 100 to 150 g / t magnetic concentrate.

[0017] Nanobubble pretreatment uses a Venturi tube for cavitation to form nanobubbles in the flotation agent. The fluid velocity in the cavitation tube is greater than 12.5m / s, and the cavitation time is greater than 5min. The flotation agent pretreated with nanobubbles is mixed with the magnetic concentrate to form a flotation feed slurry.

[0018] 4) Flotation: The flotation feed slurry is ultrasonically pretreated, and then reverse flotation closed-circuit operation is carried out to obtain reverse flotation concentrate and reverse flotation tailings.

[0019] The ultrasonic equipment is placed in the flotation feed slurry, and the flotation feed slurry is pretreated by ultrasonic wave, the ultrasonic wave frequency is between 60 and 120 kHz, and the ultrasonic wave time is 15 to 30 minutes.

[0020] After ultrasonic pretreatment, the flotation feed slurry is subjected to reverse flotation closed-circuit operation to obtain reverse flotation concentrate and reverse flotation tailings. The reverse flotation closed-circuit operation preferably adopts one roughing, one fine and three sweeping operations.

[0021] The flotation feed pulp enters the flotation tank, and first undergoes reverse flotation roughing operation. The concentrate from reverse flotation roughing enters the reverse flotation selection process, and the tailings from reverse flotation roughing enter the reverse flotation scavenging process. When the concentrate enters the selection process, the reverse flotation roughing concentrate is watered to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 30% to 40%, and sodium oleate collector is added and stirred for 2 to 3 minutes. The amount of sodium oleate added is 20 to 50 g / t reverse flotation roughing concentrate pulp.

[0022] When the reverse flotation scavenging is carried out once, the concentrate obtained from the reverse flotation scavenging is returned to the flotation slurry for reverse flotation roughing again; when the reverse flotation roughing tailings are subjected to reverse flotation scavenging twice, the concentrate obtained from the reverse flotation scavenging is mixed with the reverse flotation roughing tailings, and the first reverse flotation scavenging is carried out together; when the reverse flotation roughing tailings are subjected to reverse flotation scavenging three times, the concentrate obtained from the reverse flotation scavenging is mixed with the reverse flotation roughing tailings, and the second reverse flotation scavenging is carried out together.

[0023] By adopting the above method, the reverse flotation concentrate obtained contains TFe of 65.5% to 68% by weight, and the iron recovery rate is 70% to 90%.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention adopts the combined action of nanobubbles and ultrasonic waves to separate magnetic-red fine refractory iron ore. Compared with the conventional stage grinding, coarse and fine separation, magnetic separation-anion reverse flotation process, the ore particle size range is wider, especially for the iron ore with a particle size less than 325 mesh, it can still be effectively processed.

[0026] 2. The present invention adopts the combined action of nanobubbles and ultrasound to separate magnetic-hematite fine and refractory iron ore. Compared with the conventional stage grinding, coarse and fine separation, magnetic separation-anion reverse flotation process, the present invention adds a nanobubble and ultrasonic combined pretreatment process before flotation, which can better prevent the fine-grained minerals from becoming muddy and adhering to the surface of large-grained minerals during the flotation process, resulting in poor concentrate recovery rate, high iron grade in tailings and other problems, and can reduce the dosage of reagents.

[0027] 3. Compared with the single nanobubble pretreatment process, the method of separating magnetic-red fine refractory iron ore by the combined action of nanobubbles and ultrasound used in the present invention can effectively improve the emulsification and dispersion degree of flotation reagents, make the flotation reagents adhere to the mineral surface more evenly, reduce the impact strength of the nanobubble generating device, and reduce equipment loss. The combined action of ultrasound can reduce the adhesion of fine particles on the surface of useful minerals, prevent the mineral surface from being covered, and further enhance the selective dissolution of the mineral surface, which plays a positive role in the flotation of coarse-grained minerals, thereby having a positive impact on the separation of useful minerals and gangue minerals.

[0028] 4. In the method for separating magnetic-hematite fine refractory iron ore by the combined action of nanobubbles and ultrasound adopted in the present invention, when the ultrasonic frequency is between 60kHz and 120kHz and the ultrasonic time is between 15min and 30min, it will not cause strong turbulence of the slurry to affect the action of nanobubbles, but can enhance the dispersion of nanobubbles in the slurry and the collision probability between mineral particles and nanobubbles, so that the ultrasonic technology and nanobubble flotation play a synergistic role.

[0029] 5. The present invention provides a resource recovery process for the development and utilization of the same type of complex and difficult to select lean iron ore, which can effectively improve the recovery rate of fine particles and has important industrial significance for the effective utilization of global fine iron ore resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only for illustration and are not intended to limit the present invention.

[0032] The magnetic-hematite mixed iron ore used in the embodiment of the present invention is a mineral produced in Anshan, Liaoning, China. The ore is mined from a mining field and crushed by a jaw crusher.

[0033] In the embodiment of the present invention, the magnetic separator selected for weak magnetic operation is a drum magnetic separator, and the magnetic separator selected for strong magnetic operation is a Slon vertical ring high gradient magnetic separator.

[0034] The ball mill used in the embodiment of the present invention is an XMCQ type porcelain-lined ball mill, and the equipment used for reverse flotation is an XFLB type micro closed-circuit continuous flotation machine.

[0035] The crusher used in the embodiment of the present invention is a laboratory-grade jaw crusher.

[0036] The nano bubble generating device used in the embodiment of the present invention is a venturi tube type circulating cavitation device.

[0037] The ultrasonic generating device used in the embodiment of the present invention is a 60L multi-frequency ultrasonic cleaner.

[0038] The inhibitor starch, pH regulator CaO and collector sodium oleate used in the examples of the present invention are all analytically pure.

[0039] Embodiment 1:

[0040] In this example, the magnetic-hematite mixed iron ore from Anshan, Liaoning, China is selected. Figure 1 In the process flow shown, after the closed-loop operation of crushing and screening, materials with a particle size of ≤12 mm are obtained, and the ore with a particle size of >12 mm is returned to the crusher for further crushing; the chemical composition of the crushed material contains TFe 30.8%, CaO 0.59%, MgO 0.23%, SiO235.3%, S 0.018%, P 0.035%, and the remainder is impurities.

[0041] The crushed products are subjected to a closed-circuit grinding and screening process of semi-autogenous grinding and ball milling to obtain grinding products with a mesh size of ≤400, accounting for 86%.

[0042] The grinding products are subjected to weak magnetic and strong magnetic classification operations to obtain magnetic concentrate and magnetic tailings. Among them, the concentrate obtained after weak magnetic treatment is classified, and those with less than 325 mesh enter the flotation pretreatment, and those with ≥325 mesh are returned to the ball mill for re-grinding; the tailings obtained after weak magnetic treatment are concentrated, and the upper clear liquid enters the clarification tank, and the precipitated slurry enters the strong magnetic separation operation. The concentrate produced by the strong magnetic separation operation is combined with the weak magnetic separation concentrate and enters the classification operation together, which is the magnetic separation concentrate; the tailings from the strong magnetic separation operation are concentrated to obtain magnetic separation tailings.

[0043] The magnetic separation concentrate obtained by the above method contains 43.8% TFe by weight, with an iron recovery rate of 88.3% and the remainder being impurities.

[0044] The final iron concentrate TFe grade and TFe recovery rate under five different pretreatment conditions were compared.

[0045] (1) Nanobubble and ultrasonic combined pretreatment, ultrasonic frequency 75 kHz, ultrasonic time 16 min.

[0046] Before pretreating the flotation agent with nanobubbles, add inhibitor starch to the stirring barrel and stir for 3 minutes. The amount of starch added is 300g / t of magnetic concentrate. Then add pH adjuster CaO and stir for 3 minutes. The amount of CaO added is 40g / t of magnetic concentrate. Finally, add collector sodium oleate and stir for 3 minutes. The amount of sodium oleate added is 120g / t of magnetic concentrate.

[0047] Then the flotation reagent is passed into the venturi tube for cavitation, forming nanobubbles in the flotation reagent to achieve nanobubble pretreatment of the slurry. The cavitated slurry is the flotation feed slurry. The fluid velocity in the cavitation tube is 13m / s, and the cavitation time is 6min.

[0048] The ultrasonic equipment is placed in the flotation feed slurry, and the flotation feed slurry is pretreated by ultrasound, with an ultrasonic frequency of 75kHz and an ultrasonic time of 16min.

[0049] After ultrasonic treatment, the flotation feed pulp enters the flotation tank, and first undergoes reverse flotation roughing operation. The reverse flotation roughing concentrate enters the concentration process, and the reverse flotation roughing tailings enter the scavenging process. When the concentrate undergoes reverse flotation concentration, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 35%. At the same time, the collector sodium oleate is added and stirred for 3 minutes. The amount of sodium oleate added is 20g / t reverse flotation roughing concentrate pulp. When the reverse flotation rougher tailings are subjected to the first reverse flotation scavenging, the concentrate obtained from the first reverse flotation scavenging is returned to the flotation slurry and reverse flotation rougher is subjected to the second reverse flotation scavenging; when the reverse flotation rougher tailings are subjected to the second reverse flotation scavenging, the concentrate obtained from the second reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the first reverse flotation scavenging is carried out together; when the reverse flotation rougher tailings are subjected to the third reverse flotation scavenging, the concentrate obtained from the third reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the second reverse flotation scavenging is carried out together.

[0050] The composition of the reverse flotation concentrate of the magnetic-hematite mixed iron ore obtained by the above method contains TFe66.5% by weight, the iron recovery rate is 79.4%, and the remainder is impurities.

[0051] (2) Single nanobubble pretreatment

[0052] Before pretreating the flotation agent with nanobubbles, add inhibitor starch to the stirring barrel and stir for 3 minutes. The amount of starch added is 300g / t of magnetic concentrate. Then add pH adjuster CaO and stir for 3 minutes. The amount of CaO added is 40g / t of magnetic concentrate. Finally, add collector sodium oleate and stir for 3 minutes. The amount of sodium oleate added is 120g / t of magnetic concentrate.

[0053] Then the flotation reagent is passed into the venturi tube for cavitation, forming nanobubbles in the flotation reagent to achieve nanobubble pretreatment of the slurry. The cavitated slurry is the flotation feed slurry. The fluid velocity in the cavitation tube is 13m / s, and the cavitation time is 6min.

[0054] After the nanobubble pretreatment, the flotation feed pulp is directly put into the flotation tank without ultrasonic treatment, and the reverse flotation roughing operation is first carried out. The reverse flotation roughing concentrate enters the concentration process, and the reverse flotation roughing tailings enter the scavenging process. When the concentrate is subjected to reverse flotation concentration, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 35%, and the collector sodium oleate is added and stirred for 3 minutes. The amount of sodium oleate added is 20g / t reverse flotation roughing concentrate pulp. When the reverse flotation rougher tailings are subjected to the first reverse flotation scavenging, the concentrate obtained from the first reverse flotation scavenging is returned to the flotation slurry and reverse flotation rougher is subjected to the second reverse flotation scavenging; when the reverse flotation rougher tailings are subjected to the second reverse flotation scavenging, the concentrate obtained from the second reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the first reverse flotation scavenging is carried out together; when the reverse flotation rougher tailings are subjected to the third reverse flotation scavenging, the concentrate obtained from the third reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the second reverse flotation scavenging is carried out together.

[0055] The composition of the magnetic-hematite mixed iron ore reverse flotation concentrate obtained by the above method contains TFe60.3% by weight, the iron recovery rate is 66.8%, and the remainder is impurities. The comparative example uses nanobubble pretreatment of the ore pulp alone, and the iron recovery rate is low.

[0056] (3) No pre-processing is used

[0057] Add inhibitor starch to the mixing barrel and stir for 3 minutes. The amount of starch added is 300g / t magnetic concentrate. Then add pH adjuster CaO and stir for 3 minutes. The amount of CaO added is 40g / t magnetic concentrate. Finally, add collector sodium oleate and stir for 3 minutes. The amount of sodium oleate added is 120g / t magnetic concentrate.

[0058] The stirred pulp is directly introduced into the flotation tank, and reverse flotation roughing operation is first carried out. The concentrate from reverse flotation roughing enters the selection process, and the tailings from reverse flotation roughing enter the scavenging process. When the concentrate is reverse flotation selected, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 35%. At the same time, the collector sodium oleate is added and stirred for 3 minutes. The amount of sodium oleate added is 20g / t reverse flotation roughing concentrate pulp. When the reverse flotation rougher tailings are subjected to the first reverse flotation scavenging, the concentrate obtained from the first reverse flotation scavenging is returned to the flotation slurry and reverse flotation rougher is subjected to the second reverse flotation scavenging; when the reverse flotation rougher tailings are subjected to the second reverse flotation scavenging, the concentrate obtained from the second reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the first reverse flotation scavenging is carried out together; when the reverse flotation rougher tailings are subjected to the third reverse flotation scavenging, the concentrate obtained from the third reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the second reverse flotation scavenging is carried out together.

[0059] The composition of the magnetic-hematite mixed iron ore reverse flotation concentrate obtained by the above method contains 60.1% TFe by weight, 60.5% iron recovery, and the remainder is impurities. This comparative example is the case where no pretreatment conditions are used, and the iron recovery is low at this time.

[0060] (4) Nanobubble and ultrasonic combined pretreatment, ultrasonic frequency 20 kHz, ultrasonic time 10 min.

[0061] Before pretreating the flotation agent with nanobubbles, add inhibitor starch to the stirring barrel and stir for 3 minutes. The amount of starch added is 300g / t of magnetic concentrate. Then add pH adjuster CaO and stir for 3 minutes. The amount of CaO added is 40g / t of magnetic concentrate. Finally, add collector sodium oleate and stir for 3 minutes. The amount of sodium oleate added is 120g / t of magnetic concentrate.

[0062] Then the flotation reagent is passed into the venturi tube for cavitation, forming nanobubbles in the flotation reagent to achieve nanobubble pretreatment of the slurry. The cavitated slurry is the flotation feed slurry. The fluid velocity in the cavitation tube is 13m / s, and the cavitation time is 6min.

[0063] The ultrasonic equipment is placed in the flotation feed slurry, and the flotation feed slurry is pretreated by ultrasound, with an ultrasonic frequency of 20 kHz and an ultrasonic time of 10 minutes.

[0064] After ultrasonic treatment, the flotation feed pulp enters the flotation tank, and first undergoes reverse flotation roughing operation. The reverse flotation roughing concentrate enters the concentration process, and the reverse flotation roughing tailings enter the scavenging process. When the concentrate undergoes reverse flotation concentration, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 35%. At the same time, the collector sodium oleate is added and stirred for 3 minutes. The amount of sodium oleate added is 20g / t reverse flotation roughing concentrate pulp. When the reverse flotation rougher tailings are subjected to the first reverse flotation scavenging, the concentrate obtained from the first reverse flotation scavenging is returned to the flotation slurry and reverse flotation rougher is subjected to the second reverse flotation scavenging; when the reverse flotation rougher tailings are subjected to the second reverse flotation scavenging, the concentrate obtained from the second reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the first reverse flotation scavenging is carried out together; when the reverse flotation rougher tailings are subjected to the third reverse flotation scavenging, the concentrate obtained from the third reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the second reverse flotation scavenging is carried out together.

[0065] The composition of the reverse flotation concentrate of the magnetic-hematite mixed iron ore obtained by the above method contains 61.2% TFe by weight, the iron recovery rate is 69.5%, and the remainder is impurities.

[0066] (5) Nanobubble and ultrasonic combined pretreatment, ultrasonic frequency 150 kHz, ultrasonic time 40 min.

[0067] Before pretreating the flotation agent with nanobubbles, add inhibitor starch to the stirring barrel and stir for 3 minutes. The amount of starch added is 300g / t of magnetic concentrate. Then add pH adjuster CaO and stir for 3 minutes. The amount of CaO added is 40g / t of magnetic concentrate. Finally, add collector sodium oleate and stir for 3 minutes. The amount of sodium oleate added is 120g / t of magnetic concentrate.

[0068] Then the flotation reagent is passed into the venturi tube for cavitation, forming nanobubbles in the flotation reagent to achieve nanobubble pretreatment of the slurry. The cavitated slurry is the flotation feed slurry. The fluid velocity in the cavitation tube is 13m / s, and the cavitation time is 6min.

[0069] The ultrasonic equipment is placed in the flotation feed slurry, and the flotation feed slurry is pretreated by ultrasound, with an ultrasonic frequency of 150 kHz and an ultrasonic time of 40 minutes.

[0070] After ultrasonic treatment, the flotation feed pulp enters the flotation tank, and first undergoes reverse flotation roughing operation. The reverse flotation roughing concentrate enters the concentration process, and the reverse flotation roughing tailings enter the scavenging process. When the concentrate undergoes reverse flotation concentration, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 35%. At the same time, the collector sodium oleate is added and stirred for 3 minutes. The amount of sodium oleate added is 20g / t reverse flotation roughing concentrate pulp. When the reverse flotation rougher tailings are subjected to the first reverse flotation scavenging, the concentrate obtained from the first reverse flotation scavenging is returned to the flotation slurry and reverse flotation rougher is subjected to the second reverse flotation scavenging; when the reverse flotation rougher tailings are subjected to the second reverse flotation scavenging, the concentrate obtained from the second reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the first reverse flotation scavenging is carried out together; when the reverse flotation rougher tailings are subjected to the third reverse flotation scavenging, the concentrate obtained from the third reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the second reverse flotation scavenging is carried out together.

[0071] The composition of the reverse flotation concentrate of the magnetic-hematite mixed iron ore obtained by the above method contains 62.7% TFe by weight, the iron recovery rate is 69.4%, and the remainder is impurities.

[0072] Through the comparative analysis of the flotation concentrate indicators under five different conditions in Table 1, it can be seen that when the ultrasonic frequency is between 60 and 120 kHz and the ultrasonic time is 15 to 30 min, the combined pretreatment of nanobubbles and ultrasound can increase the TFe grade of the flotation concentrate by more than 5% and the TFe recovery rate of the flotation concentrate by more than 12% compared with other pretreatment conditions, which has a significant effect on improving the separation effect of fine-grained lean iron ore.

[0073] Table 1 Comparative analysis of flotation concentrate indicators under five different pretreatment conditions

[0074]

[0075] Embodiment 2:

[0076] In this example, the magnetic-hematite mixed iron ore from Anshan, Liaoning, China is selected. Figure 1 In the process flow shown, after the closed-loop operation of crushing and screening, materials with a particle size of ≤12 mm are obtained, and the ore with a particle size of >12 mm is returned to the crusher for further crushing; the chemical composition of the crushed material contains TFe 31.5%, CaO 0.35%, MgO 0.85%, SiO237.2%, S 0.016%, P 0.032%, and the remainder is impurities.

[0077] The crushed products are subjected to a closed-circuit grinding and screening process of semi-autogenous grinding and ball milling to obtain grinding products with a mesh size of ≤400, accounting for 89%.

[0078] The grinding products are subjected to weak magnetic and strong magnetic classification operations to obtain magnetic concentrate and magnetic tailings. Among them, the concentrate obtained after weak magnetic treatment is classified, and those with less than 325 mesh enter the flotation pretreatment, and those with ≥325 mesh are returned to the ball mill for re-grinding; the tailings obtained after weak magnetic treatment are concentrated, and the upper clear liquid enters the clarification tank, and the precipitated slurry enters the strong magnetic separation operation. The concentrate produced by the strong magnetic separation operation is combined with the weak magnetic separation concentrate and enters the classification operation together, which is the magnetic separation concentrate; the tailings from the strong magnetic separation operation are concentrated to obtain magnetic separation tailings.

[0079] The magnetic concentrate obtained by the above method contains 42.6% TFe by weight, with an iron recovery rate of 87.5% and the remainder being impurities.

[0080] Before pretreating the flotation agent with nanobubbles, add inhibitor starch to the stirring barrel and stir for 2 minutes. The amount of starch added is 250g / t of magnetic concentrate. Then add pH adjuster CaO and stir for 2 minutes. The amount of CaO added is 60g / t of magnetic concentrate. Finally, add collector sodium oleate and stir for 2 minutes. The amount of sodium oleate added is 140g / t of magnetic concentrate.

[0081] Then the flotation reagent is passed into the venturi tube for cavitation, forming nanobubbles in the flotation reagent to achieve nanobubble pretreatment of the slurry. The cavitated slurry is the flotation feed slurry. The fluid velocity in the cavitation tube is 15m / s, and the cavitation time is 8min.

[0082] Ultrasonic equipment is introduced into the flotation feed slurry to pretreat the flotation feed slurry using ultrasound. The ultrasonic frequency is 90 kHz and the ultrasonic time is 18 minutes.

[0083] The flotation feed pulp after ultrasonic pretreatment is put into the flotation tank, and reverse flotation roughing operation is first carried out. The concentrate of reverse flotation roughing enters the selection process, and the tailings of reverse flotation roughing enter the scavenging process. When the concentrate is reverse flotation selection, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 40%, and the collector sodium oleate is added and stirred for 2 minutes. The amount of sodium oleate added is 30g / t reverse flotation roughing concentrate pulp. When the reverse flotation rougher tailings are subjected to the first reverse flotation scavenging, the concentrate obtained from the first reverse flotation scavenging is returned to the flotation slurry and reverse flotation rougher is subjected to the second reverse flotation scavenging; when the reverse flotation rougher tailings are subjected to the second reverse flotation scavenging, the concentrate obtained from the second reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the first reverse flotation scavenging is carried out together; when the reverse flotation rougher tailings are subjected to the third reverse flotation scavenging, the concentrate obtained from the third reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the second reverse flotation scavenging is carried out together.

[0084] The composition of the reverse flotation concentrate of the magnetic-hematite mixed iron ore obtained by the above method contains TFe66.9% by weight, the iron recovery rate is 81%, and the remainder is impurities.

[0085] Embodiment 3:

[0086] In this example, the magnetic-hematite mixed iron ore from Anshan, Liaoning, China is selected. Figure 1 In the process shown in the figure, after the closed-loop operation of crushing and screening, materials with a particle size of ≤12 mm are obtained, and the ore with a particle size of >12 mm is returned to the crusher for further crushing; the chemical composition of the crushed material contains TFe 28.9%, CaO 0.85%, MgO 0.19%, SiO237.8%, S 0.013%, P 0.028%, and the remainder is impurities.

[0087] The crushed products are subjected to a closed-circuit grinding and screening process of semi-autogenous grinding and ball milling to obtain grinding products with a mesh size of ≤400, accounting for 86%.

[0088] The grinding products are subjected to weak magnetic and strong magnetic classification operations to obtain magnetic concentrate and magnetic tailings. Among them, the concentrate obtained after weak magnetic treatment is classified, and those with less than 325 mesh enter the flotation pretreatment, and those with ≥325 mesh are returned to the ball mill for re-grinding; the tailings obtained after weak magnetic treatment are concentrated, and the upper clear liquid enters the clarification tank, and the precipitated slurry enters the strong magnetic separation operation. The concentrate produced by the strong magnetic separation operation is combined with the weak magnetic separation concentrate and enters the classification operation together, which is the magnetic separation concentrate; the tailings from the strong magnetic separation operation are concentrated to obtain magnetic separation tailings.

[0089] The magnetic separation concentrate obtained by the above method contains 41.3% TFe by weight, the iron recovery rate is 86.6%, and the remainder is impurities.

[0090] Before pretreating the flotation agent with nanobubbles, add inhibitor starch to the stirring barrel and stir for 2.5 minutes. The amount of starch added is 500g / t magnetic concentrate. Then add pH adjuster CaO and stir for 2.5 minutes. The amount of CaO added is 60g / t magnetic concentrate. Finally, add collector sodium oleate and stir for 2.5 minutes. The amount of sodium oleate added is 100g / t magnetic concentrate.

[0091] Then the flotation reagent is passed into the venturi tube for cavitation, forming nanobubbles in the flotation reagent to achieve nanobubble pretreatment of the slurry. The cavitated slurry is the flotation feed slurry. The fluid velocity in the cavitation tube is 16m / s, and the cavitation time is 10min.

[0092] Ultrasonic equipment is introduced into the flotation feed slurry to pretreat the flotation feed slurry using ultrasound. The ultrasound frequency is 100 kHz and the ultrasound time is 20 minutes.

[0093] The flotation feed pulp after ultrasonic pretreatment is put into the flotation tank, and reverse flotation roughing operation is first carried out. The concentrate of reverse flotation roughing enters the selection process, and the tailings of reverse flotation roughing enter the scavenging process. When the concentrate is reverse flotation selection, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 30%, and the collector sodium oleate is added and stirred for 2.5 minutes. The amount of sodium oleate added is 40g / t reverse flotation roughing concentrate pulp. When the reverse flotation rougher tailings are subjected to the first reverse flotation scavenging, the concentrate obtained from the first reverse flotation scavenging is returned to the flotation slurry and reverse flotation rougher is subjected to the second reverse flotation scavenging; when the reverse flotation rougher tailings are subjected to the second reverse flotation scavenging, the concentrate obtained from the second reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the first reverse flotation scavenging is carried out together; when the reverse flotation rougher tailings are subjected to the third reverse flotation scavenging, the concentrate obtained from the third reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the second reverse flotation scavenging is carried out together.

[0094] The composition of the reverse flotation concentrate of the magnetic-hematite mixed iron ore obtained by the above method contains 67.2% TFe by weight, the iron recovery rate is 80.5%, and the remainder is impurities.

[0095] Embodiment 4:

[0096] In this embodiment, magnetic-hematite mixed iron ore from Anshan, Liaoning, China is selected, and after closed-circuit crushing and screening operations, materials with a particle size of ≤12 mm are obtained, and ores with a particle size of >12 mm are returned to the crusher for re-crushing; the chemical composition of the crushed material, by weight percentage, contains TFe 30.8%, CaO 0.59%, MgO 0.23%, SiO2 35.3%, S 0.018%, P 0.035%, and the remainder is impurities.

[0097] The crushed products are subjected to a closed-circuit grinding and screening process of semi-autogenous grinding and ball milling to obtain grinding products with a mesh size of ≤400, accounting for 86%.

[0098] The grinding products are subjected to weak magnetic and strong magnetic classification operations to obtain magnetic concentrate and magnetic tailings. Among them, the concentrate obtained after weak magnetic treatment is classified, and those with less than 325 mesh enter the flotation pretreatment, and those with ≥325 mesh are returned to the ball mill for re-grinding; the tailings obtained after weak magnetic treatment are concentrated, and the upper clear liquid enters the clarification tank, and the precipitated slurry enters the strong magnetic separation operation. The concentrate produced by the strong magnetic separation operation is combined with the weak magnetic separation concentrate and enters the classification operation together, which is the magnetic separation concentrate; the tailings from the strong magnetic separation operation are concentrated to obtain magnetic separation tailings.

[0099] The magnetic separation concentrate obtained by the above method contains 43.8% TFe by weight, with an iron recovery rate of 88.3% and the remainder being impurities.

[0100] Before pretreating the flotation agent with nanobubbles, add starch as an inhibitor to the stirring barrel and stir for 3 minutes. The amount of starch added is 300g / t of magnetic concentrate. Then add CaO as a pH adjuster and stir for 3 minutes. The amount of CaO added is 40g / t of magnetic concentrate. Finally, add sodium oleate as a collector and stir for 3 minutes. The amount of sodium oleate added is 150g / t of magnetic concentrate.

[0101] Then the flotation reagent is passed into the venturi tube for cavitation, forming nanobubbles in the flotation reagent to achieve nanobubble pretreatment of the slurry. The cavitated slurry is the flotation feed slurry. The fluid velocity in the cavitation tube is 13m / s, and the cavitation time is 6min.

[0102] Ultrasonic equipment is introduced into the flotation feed slurry to pretreat the flotation feed slurry using ultrasound. The ultrasonic frequency is 75 kHz and the ultrasonic time is 16 minutes.

[0103] The flotation feed pulp after ultrasonic pretreatment is put into the flotation tank, and reverse flotation roughing operation is first carried out. The concentrate of reverse flotation roughing enters the selection process, and the tailings of reverse flotation roughing enter the scavenging process. When the concentrate is reverse flotation selection, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate pulp with a weight concentration of 35%, and the collector sodium oleate is added and stirred for 3 minutes. The amount of sodium oleate added is 20g / t reverse flotation roughing concentrate pulp. When the reverse flotation rougher tailings are subjected to the first reverse flotation scavenging, the concentrate obtained from the first reverse flotation scavenging is returned to the flotation slurry and reverse flotation rougher is subjected to the second reverse flotation scavenging; when the reverse flotation rougher tailings are subjected to the second reverse flotation scavenging, the concentrate obtained from the second reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the first reverse flotation scavenging is carried out together; when the reverse flotation rougher tailings are subjected to the third reverse flotation scavenging, the concentrate obtained from the third reverse flotation scavenging is mixed with the reverse flotation rougher tailings and the second reverse flotation scavenging is carried out together.

[0104] The composition of the reverse flotation concentrate of the magnetic-hematite mixed iron ore obtained by the above method contains 66.2% TFe by weight, the iron recovery rate is 85.5%, and the remainder is impurities.

Claims

1. A magnetic-red fine refractory iron ore separation method, comprising crushing, grinding, magnetic separation, flotation dosing, and flotation; characterized in that: The flotation reagent is pretreated with nanobubbles during flotation dosing; the flotation feed pulp is pretreated with ultrasonic waves during flotation. The specific steps include: 1) Grinding: crushing, screening, grinding and screening the fine-grained magnetic-hematite mixed ore to obtain the grinding product; 2) Magnetic separation: The grinding products are subjected to weak magnetic and strong magnetic classification operations to obtain magnetic concentrate and magnetic tailings; 3) Flotation dosing: First, the flotation reagent is pretreated with nanobubbles, the mixed flotation reagent is cavitated to form nanobubbles in the flotation reagent, and the pretreated flotation reagent is added to the magnetic separation concentrate to obtain the flotation feed slurry; 4) Flotation: The flotation feed slurry is ultrasonically pretreated, and then reverse flotation closed-circuit operation is carried out to obtain reverse flotation concentrate and reverse flotation tailings.

2. A magnetic-red fine refractory iron ore separation method according to claim 1, characterized in that: The nanobubble pretreatment adopts a venturi tube to perform cavitation to form nanobubbles in the flotation reagent. The fluid velocity in the venturi tube is greater than 12.5 m / s, and the cavitation time is greater than 5 min.

3. A magnetic-red fine refractory iron ore separation method according to claim 1, characterized in that: The ultrasonic pretreatment has an ultrasonic frequency of 60kHz≤120kHz and an ultrasonic time of 15min≤30min.

4. A magnetic-red fine refractory iron ore separation method according to claim 1, characterized in that: The flotation reagents in the above step 3) are mixed as follows: first, starch is added to a stirring barrel and stirred for 2 to 3 minutes, the amount of starch added is 200 to 500 g / t of magnetic concentrate; then, CaO is added and stirred for 2 to 3 minutes, the amount of CaO added is 30 to 80 g / t of magnetic concentrate; finally, sodium oleate is added and stirred for 2 to 3 minutes, the amount of sodium oleate added is 100 to 150 g / t of magnetic concentrate.

5. The method for separating magnetic-red fine refractory iron ore according to claim 1, characterized in that: The fineness of the crushed product after the closed-circuit operation of crushing and screening is ≤12mm. After the crushed product is subjected to the closed-circuit operation of grinding and screening, more than 85% of the grinding products have a particle size of ≤400 mesh; after the grinding products are subjected to weak magnetic and strong magnetic classification operations, the magnetic separation concentrate obtained contains 40% to 50% TFe by weight, and the iron recovery rate is 70% to 90%.

6. A magnetic-red fine refractory iron ore separation method according to claim 1, characterized in that: In the reverse flotation closed-circuit operation, the concentrate from the reverse flotation roughing enters the reverse flotation cleaning process, and the tailings from the reverse flotation roughing enters the reverse flotation scavenging process; When the concentrate enters the concentration process, the reverse flotation roughing concentrate is added with water to prepare a reverse flotation roughing concentrate slurry with a weight concentration of 30% to 40%, and sodium oleate is added and stirred for 2 to 3 minutes. The amount of sodium oleate added is 20 to 50 g / t of reverse flotation roughing concentrate slurry.

7. A magnetic-red fine refractory iron ore separation method according to claim 1 or 6, characterized in that: In the reverse flotation closed-circuit operation, when the reverse flotation scavenging is performed once, the concentrate obtained by the reverse flotation scavenging is returned to the flotation slurry, and reverse flotation roughing is performed again; when the reverse flotation roughing tailings are subjected to the reverse flotation scavenging twice, the concentrate obtained by the reverse flotation scavenging twice is mixed with the reverse flotation roughing tailings, and the first reverse flotation scavenging is performed together; When the reverse flotation rougher tailings are subjected to three reverse flotation scavengings, the concentrates obtained from the three reverse flotation scavengings are mixed with the tailings from the first reverse flotation scavenging and are subjected to the second reverse flotation scavenging together.

8. The method for separating magnetic-red fine refractory iron ore according to claim 1, characterized in that: The obtained reverse flotation concentrate contains TFe of 65.5% to 68% by weight, and the iron recovery rate is 70% to 90%.

9. A magnetic-red fine refractory iron ore separation method according to claim 1, characterized in that: The chemical composition of the fine-grained magnetic-hematite mixed ore is calculated by weight percentage as follows: TFe 25%-35%, CaO 0.1%-1.5%, MgO 0.1%-1.5%, SiO2 30%-40%, S 0.01%-0.1%, P 0.01%-0.1%, and the remainder is impurities.

10. A magnetic-red fine refractory iron ore separation method according to claim 1, characterized in that: The iron phase composition of the fine-grained magnetic-hematite mixed ore is as follows by weight: 25% to 35% hematite, 15% to 30% magnetite, 1% to 3% siderite, 0.1% to 1% pyrite, and the remainder is iron-containing silicate and other impurities.

Citation Information

Cited By

  • Method for fine-fraction desulfurization of high-sulfur bauxite

    CN119951674A