Large-particle micron-sized spherical silver powder with concentrated particle size distribution and preparation method and application of large-particle micron-sized spherical silver powder
By using a specific silver powder preparation method in TOPCon batteries, the problems of silver powder batch stability and uneven particle size distribution were solved, and narrow particle size distribution, large-particle micron-level spherical silver powder suitable for laser-enhanced contact optimization technology was prepared, meeting the requirements TOPCon battery needs.
Patent Information
- Application Number
- CN202410937067.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-18
AI Technical Summary
The existing micron spherical silver powder used in TOPCon batteries has problems with batch stability, small particle size and uneven distribution, making it difficult to meet the high requirements of laser-enhanced contact optimization technology.
A preparation method is adopted to prepare a silver ammonia solution by dissolving silver nitrate in deionized water, adding a fatty acid dispersant and a citrate solution, and then adding a reducing agent together with povidone in the reaction kettle to control the oxidation and reduction of the solution. The raw solution is stirred, centrifuged, dried and crushed at an equal speed and time to obtain large-particle micron-sized spherical silver powder with a concentrated particle size distribution.
The obtained silver powder has a narrow particle size distribution, uniform particles, large individual particles, and good batch stability and adaptability, and is suitable for large-scale production and application in TOPCon battery silver paste.
Smart Images

Figure CN118788959A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of silver powder preparation, and in particular relates to a micron-sized spherical silver powder with concentrated particle size distribution and a preparation method and application thereof. Background Art
[0002] TOPCon cells are a new type of solar cell technology based on N-type silicon substrates, with significant advantages such as high efficiency and low cost. Currently, TOPCon cells have become one of the mainstream technologies in the photovoltaic industry and are expected to continue to maintain their leading position in the next few years. The conversion efficiency of TOPCon cells has exceeded 25%, which is much higher than that of traditional P-type cells. In addition, the service life of TOPCon cells can be up to more than 25 years, with excellent reliability and stability, and can operate normally under various harsh environmental conditions.
[0003] However, TOPCon cells are not without challenges. First, their production process is relatively complex and requires high technical level and equipment. Secondly, the production of TOPCon cells requires a large amount of raw materials such as silicon wafers and silver paste. If the raw materials are insufficiently supplied, it may restrict their production and development. In addition, with the continuous emergence of other new battery technologies, TOPCon cells are facing fierce market competition. For example, BC cells have high single-sided efficiency and aesthetics in specific application scenarios, but the technical implementation difficulty and cost are relatively high. HJT cells have the advantages of high conversion efficiency, low attenuation performance and good temperature coefficient, and the manufacturing process is relatively simple. The cost is expected to be further reduced. It is regarded as one of the development directions of solar cell technology in the future. Perovskite cells have shown broad development prospects with their high conversion efficiency, low cost and flexible manufacturing, but they are still in the research and development stage. Overall, TOPCon cells will still have strong development potential in the future, and with the continuous advancement of technology and further reduction of costs, TOPCon cells are expected to occupy a larger share in the photovoltaic market. However, TOPCon cells also need to continue to innovate and improve to meet the challenges of other battery technologies.
[0004] As a conductive material used in the grid electrode of TOPCon batteries, silver powder plays an important role in the continuous innovation and improvement of TOPCon batteries. In recent years, with the continuous increase in the production and sales of TOPCon battery components, coupled with the progress in the localization of photovoltaic cell silver paste, especially the application of laser enhanced contact optimization (LECO) technology in the manufacture of TOPCon solar cells, many preparation technologies for matching micron-shaped spherical silver powders have emerged. However, the silver powders currently obtained have problems such as inconsistent batch stability, small silver powder particle size, and uneven distribution. With the gradual use and optimization of laser enhanced contact optimization (LECO) technology, the batch stability and adaptability of silver powder are required to be higher and higher. Therefore, in response to the changes in demand brought about by TOPCon battery silver paste, it is necessary to prepare a silver powder that can be mass-produced and has good batch stability and good adaptability. Summary of the invention
[0005] The present disclosure aims to solve at least one of the technical problems existing in the prior art, and provides a preparation method of large-particle micron-sized spherical silver powder with concentrated particle size distribution, and a preparation method and application thereof.
[0006] In one aspect of the present disclosure, a method for preparing large-particle micron-sized spherical silver powder with a concentrated particle size distribution is provided, the preparation method comprising:
[0007] Dissolve silver nitrate in deionized water at room temperature, and add ammonia water to prepare a silver ammonia solution;
[0008] Dissolve the reducing agent in deionized water at room temperature, add sodium hydroxide solution to adjust the pH to 8-10, and obtain a reducing solution;
[0009] Dissolving a fatty acid dispersant in an alcohol solution, preparing a certain amount of citrate solution with deionized water, adding the solution to the silver ammonia solution, and mixing the mixture with mechanical stirring to obtain an oxidizing solution;
[0010] Deionized water and povidone were added into the reaction kettle, stirring was started, and after the povidone was thoroughly dissolved, the oxidizing solution and the reducing solution were added into the reaction kettle at an equal speed, and silver powder was obtained through stirring, centrifugation, drying and crushing.
[0011] Optionally, the mass ratio of the silver nitrate to the ammonia water is 10:8-10:11.
[0012] Optionally, the fatty acid dispersant is added in an amount of 2-5% by weight of the silver nitrate.
[0013] Optionally, the fatty acid dispersant is one or more of linoleic acid, lauric acid, oleic acid, caprylic acid, stearic acid, and palmitic acid.
[0014] Optionally, the citrate solution is added in an amount of 0.2-1% by weight of the silver nitrate.
[0015] Optionally, the added amount of the povidone is 20-30% of the weight of the silver nitrate.
[0016] Optionally, the oxidation liquid and the reduction liquid are added to the reactor at a speed of 10-15 L / min, and the addition time is 3-5 minutes;
[0017] The cumulative amount of the oxidizing liquid added to the reaction kettle is 40-70L; wherein the silver content is 2-3kg;
[0018] The cumulative amount of the reducing solution added to the reactor is 35-55L.
[0019] Optionally, the reducing solution, the oxidizing solution and the povidone solution added to the reaction kettle are all maintained at 35-40° C. before the reaction.
[0020] Another aspect of the present disclosure provides a large-particle micron-sized spherical silver powder with a concentrated particle size distribution, which is prepared by the preparation method described above.
[0021] Another aspect of the present disclosure is to apply the large-particle micron-sized spherical silver powder with concentrated particle size distribution described above to TOPCon battery silver paste.
[0022] The present disclosure proposes a preparation method of a large-particle micron-sized spherical silver powder with a concentrated particle size distribution, and its preparation method and application. The preparation method includes: dissolving silver nitrate in deionized water at room temperature, adding ammonia water to prepare a silver ammonia solution; dissolving a reducing agent in deionized water at room temperature, adding sodium hydroxide solution to adjust the pH to 8-10, and obtaining a reducing solution; dissolving a fatty acid dispersant in an alcohol solution, and then preparing a certain amount of citrate solution with deionized water, adding them together to the silver ammonia solution, mechanically stirring and mixing evenly, and obtaining an oxidizing solution; adding deionized water and polyvidone to a reactor, starting stirring, and after the polyvidone is thoroughly dissolved, adding the oxidizing solution and the reducing solution to the reactor at an equal speed, stirring, centrifuging, drying, and crushing to obtain silver powder. The present invention uses silver ammonia solution as a silver source, and under the protection of adding one or more dispersants, accurately controls the mixing time of an oxidizing solution and a reducing solution and the reaction amount of a single batch, so as to obtain micron-sized large-particle spherical silver particles with a narrow particle size distribution. The obtained silver powder particles are quasi-spherical, have a narrow particle size distribution, are uniform in particles, and have large individual particles. In addition, the obtained silver powder has good batch stability and adaptability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flowchart of a method for preparing large-particle micron-sized spherical silver powder with concentrated particle size distribution according to an embodiment of the present disclosure;
[0024] Figure 2 This is a SEM image of the silver powder prepared in Example 1 of the present disclosure;
[0025] Figure 3 This is a SEM image of the silver powder prepared in Example 2 of the present disclosure;
[0026] Figure 4 This is the SEM image of the silver powder prepared in Example 3 of the present disclosure. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the disclosure. The described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure.
[0028] like Figure 1 As shown, in one aspect of the present disclosure, a method S100 for preparing large-particle micron-sized spherical silver powder with concentrated particle size distribution is provided, which specifically comprises the following steps S110 to S140:
[0029] S110. Dissolve silver nitrate in deionized water at room temperature, and add ammonia water to prepare a silver ammonia solution.
[0030] In some preferred embodiments, the mass ratio of silver nitrate to ammonia water is in the range of 10:8-10:11, more preferably in the range of 10:8-10:9, which is conducive to obtaining silver powder with a narrow particle size distribution.
[0031] It should be noted that in step S110, the silver nitrate is dry and analytically pure, with a pH value of 5-6, and the ammonia water is a 25-28% analytically pure ammonia water solution.
[0032] S120, dissolving the reducing agent in deionized water at room temperature, adding sodium hydroxide solution to adjust the pH to 8-10, and obtaining a reducing solution.
[0033] In some preferred embodiments, the reducing agent is ascorbic acid (VC), hydrazine hydrate, sodium borohydride or ascorbic acid, more preferably ascorbic acid, and the ascorbic acid is of pharmaceutical grade.
[0034] In other preferred embodiments, the pH value is preferably within a narrow range of 9-9.5. By controlling the pH value of the solution, it is advantageous to obtain silver powder with a narrow particle size distribution.
[0035] S130, dissolving a fatty acid dispersant in an alcohol solution, and then preparing a certain amount of citrate solution with deionized water, adding the two solutions into the silver ammonia solution, and mechanically stirring and mixing them evenly to obtain an oxidizing solution.
[0036] In some preferred embodiments, the fatty acid dispersant is one or more of linoleic acid, lauric acid, oleic acid, caprylic acid, stearic acid, and palmitic acid, for example, preferably one or a mixture of 2-3 thereof, more preferably a mixture of stearic acid and palmitic acid.
[0037] In other preferred embodiments, the amount of fatty acid dispersant added is determined according to the content of silver nitrate added, wherein the amount of fatty acid dispersant added is 2-5% of the weight of silver nitrate, and the more preferred range is 3.5-4.5%. The fatty acid dispersant has strong hydrophobicity, which can prevent the silver powder particles from aggregating and growing in the synthesis stage, and can reduce the surface tension of the silver powder during the high-temperature drying process of the silver powder, thereby making the silver powder surface have good wettability, and finally making the powder have good fluidity.
[0038] In other preferred embodiments, the citrate used in the citrate solution is sodium citrate, potassium citrate, trisodium citrate, etc., and the added amount is determined according to the content of the added silver nitrate. The added amount of the citrate solution is 0.2-1% of the weight of the silver nitrate, and the more preferred range is 0.5-0.8%.
[0039] In this embodiment, by mixing the citrate solution with the dispersant, the anisotropic growth of the crystals can be suppressed, and the separation of the spherical particles and the prevention of excessive growth can be ensured, thereby ensuring that the product silver particles have a spherical morphology.
[0040] S140. Add deionized water and povidone into a reactor and start stirring. After the povidone is thoroughly dissolved, add the oxidizing solution and the reducing solution into the reactor at an equal speed. Continue stirring for 5 minutes after adding. Then, centrifuge and wash until the conductivity of the effluent is less than 50 μs / cm. Dry, use a swing crusher for preliminary crushing, and then use an air flow device to grind to obtain a finished powder.
[0041] In some preferred embodiments, in step S140, the reducing liquid, oxidizing liquid and povidone solution added to the reaction kettle are all kept at 35-40° C. before the reaction, that is, all liquids are kept at 35-40° C. before the reaction. In this way, the silver ammonia solution and the alkaline ascorbic acid solution can obtain silver powder with spherical particles and large single particles under rapid reaction conditions.
[0042] In other preferred embodiments, in step S140, the processing pressure of the airflow equipment used is 0.6-0.8 MPa.
[0043] In other preferred embodiments, the amount of polyvidone added is 20-30% of the weight of silver nitrate, and the more preferred range is 25-28%. In addition, the K value of the polyvidone used is 12-60, and the more preferred K value is 15-30. Povidone can protect and prevent the silver particles generated in the water system from agglomeration, so that the product silver particles form a spherical or quasi-spherical shape. The purpose of adding a significantly excessive amount of polyvidone to the system is to allow it to form excessive adsorption on each crystal face of the silver particles, thereby balancing the thermodynamic energy of each crystal face of the silver particles to inhibit the anisotropic growth of the crystal, further protecting and preventing the silver particles generated in the water system from agglomeration, and promoting the product silver particles to form a spherical or quasi-spherical shape.
[0044] In other preferred embodiments, the oxidizing liquid and the reducing liquid are metered into the reactor by a high-precision peristaltic pump, and the addition amount of the two is the same in each batch, wherein the addition rate is 10-15 L / min, and the cumulative addition of each batch is completed in 3-5 minutes. The cumulative addition amount of reducing liquid in each batch is preferably 35-55 L, and the cumulative addition amount of oxidizing liquid material in each batch is preferably 40-70 L, and the silver content of a single batch is 2-3 kg. More preferably, the cumulative amount of oxidizing liquid material in each batch is 50-60 L, and the silver content of a single batch is 2.3-2.6 kg.
[0045] In this embodiment, by controlling the liquid addition speed, the rate at which silver ions are reduced in each reaction stage can be adjusted to control the particle size and morphology of the silver powder generated in the mixed reaction liquid, and the prepared silver powder has the characteristics of large particle size and controllable morphology. At the same time, by accurately controlling the mixing time of the oxidizing liquid and the reducing liquid and the single batch reaction amount, it is beneficial to obtain micron-sized large-particle spherical silver particles with a narrow particle size distribution.
[0046] It should be noted that the feeding-reaction-discharging process given in the above step S140 is a production batch. After discharging, feeding is performed again to start the second batch of production, and so on. Multiple batches of silver powder production can be achieved to improve production efficiency.
[0047] It should be further explained that in order to realize the design and synthesis of large-particle silver powder and achieve quantitative control of the size of silver particles, it is necessary to select appropriate reaction routes and process conditions. At the same time, in order to obtain a spherical morphology, it is also necessary to suppress the anisotropic growth of crystals. Based on this, the present disclosure adopts a liquid phase chemical reduction preparation method for large-particle micron-sized silver powder that can accurately control the particle size distribution of silver powder under normal temperature and pressure reaction conditions and is suitable for large-scale production. Silver ammonia solution is used as the silver source, ascorbic acid is used as the reducing agent, and under the protection of adding one or more dispersants, in each batch of production, by accurately controlling the mixing time of the oxidizing solution and the reducing solution, the single batch reaction amount, and the type and amount of the dispersant, the particle size distribution of the silver powder can be accurately controlled within a certain range, and micron-sized large-particle spherical silver particles with a narrow particle size distribution can be obtained. The obtained silver powder has good batch stability and adaptability.
[0048] Another aspect of the present disclosure provides a micron-sized spherical silver powder with concentrated particle size distribution and large particles, which is formed by the preparation method described above. Please refer to the above description for the specific preparation process, which will not be repeated here.
[0049] In this embodiment, the obtained silver powder particle size distribution is as follows: D10 is 1.2-1.3 μm, D50 is 1.7-2.0 μm, D90 is 2.2-3.0 μm, D100 is less than 5.5 μm, and the tap density is 6.3 g / cm 3 Above, specific surface area 0.25-0.35m 2 / g, and the burning loss is 0.15-0.20%.
[0050] Another aspect of the present disclosure provides an application of the large-particle micron-sized spherical silver powder with a concentrated particle size distribution as described above, for example, applying it to TOPCon battery silver paste, and of course, it can also be applied to other conductive pastes.
[0051] It should be understood that TOPCon battery silver paste, in addition to the silver powder mentioned above, should also include other components such as glass powder, organic resin, organic binder, etc. Of course, it can also be used in combination with other silver powders. Those skilled in the art can make adaptive adjustments according to actual needs.
[0052] The silver powder disclosed in the present invention has an extremely low burn-in value (low surface organic content) and a relatively high tap density while ensuring good fluidity of the silver powder. It has good adaptability and can be used as a basic silver powder in combination with silver powders with other characteristics in LECO silver paste to meet the needs of TOPCon batteries.
[0053] The preparation method of large-particle micron-sized spherical silver powder with concentrated particle size distribution will be further described below in conjunction with specific examples:
[0054] Example 1
[0055] The method for preparing the large-particle micron-sized spherical silver powder with concentrated particle size distribution in this example comprises the following steps:
[0056] S1. Weigh 3800g of national standard analytical pure silver nitrate and put it into the oxidation solution preparation kettle, add 55L of room temperature deionized water, start stirring, and add 3040g of analytical pure ammonia solution (25-28%) after dissolution and clarification, stir, and stir for another 5 minutes after the solution becomes clear to obtain solution A.
[0057] S2. Weigh 130 g of palmitic acid, add 1.1 L of analytical grade alcohol and stir to dissolve, to obtain solution B; weigh 20 g of trisodium citrate, add 300 mL of deionized water and stir to dissolve, to obtain solution C; add solution B and solution C to solution A, stir for 10 minutes, to obtain oxidizing solution D.
[0058] S3. Weigh 3300g of ascorbic acid and put it into a reducing solution preparation kettle, add 50L of deionized water at room temperature, stir, and stir for 5 minutes after the solution becomes clear and transparent; prepare a 5% sodium hydroxide solution, start stirring, and use a peristaltic pump to slowly add it to the ascorbic acid solution. Stop adding when the pH meter shows 9.5, and stir for 10 minutes to obtain reducing solution E.
[0059] S4. Add 20L of deionized water and 950g of povidone (K value 28) into the reactor and start stirring. After the povidone is thoroughly dissolved, add the oxidizing solution D and the reducing solution E by air compression. The addition rate of both is 12L / min and both are added simultaneously within 4 minutes. Continue stirring for 5 minutes after addition. Then centrifuge and wash until the outlet water conductivity is below 50μs / cm, dry, use a swing crusher for preliminary crushing, and then use air flow equipment to grind to obtain the finished powder.
[0060] As shown in Table 1 and Figure 1 As shown in the figure, the silver powder particles prepared in Example 1 are spherical, with narrow particle size distribution, uniform particles, and large single particles. The D10 of the silver powder particles is 1.384 μm, the D50 is 1.918 μm, the D90 is 2.628 μm, the D100 is 4.459 μm, and the specific surface area is 0.286 m 2 / g, tap density is 6.56g / cm 3 , the burning loss is 0.17%.
[0061] Example 2
[0062] The method for preparing the large-particle micron-sized spherical silver powder with concentrated particle size distribution in this example comprises the following steps:
[0063] S1. Weigh 3600g of national standard analytical pure silver nitrate and put it into the oxidation solution preparation kettle, add 50L of room temperature deionized water, start stirring, and add 3600g of analytical pure ammonia solution (25-28%) after dissolution and clarification, stir, and stir for another 5 minutes after the solution becomes clear to obtain solution A.
[0064] S2. Weigh 126 g of stearic acid, add 1 L of analytical grade alcohol and stir to dissolve, to obtain solution B; weigh 18 g of sodium citrate, add 200 mL of deionized water and stir to dissolve, to obtain solution C; add solution B and solution C to solution A, stir for 10 minutes, to obtain oxidizing solution D.
[0065] S3. Weigh 3200 g of ascorbic acid and put it into a reducing solution preparation kettle, add 45 L of deionized water at room temperature, stir, and stir for 5 minutes after the solution becomes clear and transparent; prepare a 5% sodium hydroxide solution, start stirring, and use a peristaltic pump to slowly add it to the ascorbic acid solution. Stop adding when the pH meter shows 9, and stir for 10 minutes to obtain reducing solution E.
[0066] S4. Add 20L of deionized water and 900g of povidone (K value 25) into the reactor and start stirring. After the povidone is thoroughly dissolved, add the oxidizing solution D and the reducing solution E by air compression. The addition rate of both is 13L / min and both are added simultaneously within 4 minutes. Continue stirring for 5 minutes after addition. Then centrifuge and wash until the outlet water conductivity is below 50μs / cm, dry, use a swing crusher for preliminary crushing, and then use air flow equipment to grind to obtain the finished powder.
[0067] As shown in Table 1 and Figure 2 As shown in the figure, the silver powder particles prepared in Example 2 are spherical, with narrow particle size distribution, uniform particles, and large single particles. The D10 of the silver powder particles is 1.277 μm, the D50 is 1.738 μm, the D90 is 2.379 μm, the D100 is 3.94 μm, and the specific surface area is 0.293 m 2 / g, tap density is 6.58g / cm 3 , the burning loss is 0.17%.
[0068] Example 3
[0069] The method for preparing the large-particle micron-sized spherical silver powder with concentrated particle size distribution in this example includes the following steps:
[0070] S1. Weigh 3800g of national standard analytical pure silver nitrate and put it into the oxidation solution preparation kettle, add 55L of room temperature deionized water, start stirring, and add 3240g of analytical pure ammonia solution (25-28%) after dissolution and clarification, stir, and stir for another 5 minutes after the solution becomes clear to obtain solution A.
[0071] S2. Weigh 150 g of oleic acid, add 1 L of analytical grade alcohol and stir to dissolve, to obtain solution B; weigh 17 g of potassium citrate, add 300 mL of deionized water and stir to dissolve, to obtain solution C; add solution B and solution C to solution A, stir for 10 minutes, to obtain oxidizing solution D.
[0072] S3. Weigh 3300g of ascorbic acid and put it into a reducing solution preparation kettle, add 50L of deionized water at room temperature, stir, and stir for 5 minutes after the solution becomes clear and transparent; prepare a 5% sodium hydroxide solution, start stirring, and use a peristaltic pump to slowly add it to the ascorbic acid solution. Stop adding when the pH meter shows 9, and stir for another 10 minutes to obtain reducing solution E.
[0073] S4. Add 20L of deionized water and 1000g of povidone (K value 28) into the reactor and start stirring. After the povidone is thoroughly dissolved, add the oxidizing solution D and the reducing solution E by air compression. The addition rate of both is 10L / min and both are added simultaneously within 4 minutes. Continue stirring for 5 minutes after addition. Then centrifuge and wash until the outlet water conductivity is below 50μs / cm, dry, use a swing crusher for preliminary crushing, and then use air flow equipment to grind to obtain the finished powder.
[0074] As shown in Table 1 and Figure 3 As shown in the figure, the silver powder particles prepared in Example 3 are spherical, with narrow particle size distribution, uniform particles, and large single particles. The D10, D50, D90, and D100 of the silver powder particles are 1.251 μm, 1.761 μm, 2.515 μm, and 4.446 μm, respectively, and the specific surface area is 0.277 m 2 / g, tap density is 6.4g / cm 3 , the burn loss is 0.15%.
[0075] Table 1 Parameters of the silver powder obtained in Examples 1-3
[0076]
[0077] The present disclosure provides a large-particle micron-sized spherical silver powder with a concentrated particle size distribution and a preparation method and application thereof, which have the following beneficial effects compared with the prior art:
[0078] First, the present invention is carried out under normal temperature and pressure reaction conditions, which is safe and controllable. By accurately controlling the mixing time of the oxidizing solution and the reducing solution, the single batch reaction amount, and the type and addition amount of the dispersant, the particle size distribution of the silver powder can be accurately controlled within a certain range, and micron-sized large-particle spherical silver powder with a narrower particle size distribution can be obtained. In addition, the obtained silver powder has good batch stability and adaptability, and is suitable for large-scale production.
[0079] Second, the silver powder particles obtained in the present invention are spherical, have a narrow particle size distribution, are uniform in particle size, and have large individual particles.
[0080] Third, the silver powder obtained in the present invention has an extremely low burn-in value (low surface organic content) and a high tap density while ensuring good fluidity of the silver powder. It has good adaptability and can be used as a basic silver powder in combination with silver powders with other characteristics in LECO silver paste to meet the needs of TOPCon batteries.
[0081] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.
Claims
1. A method for preparing large-particle micron-sized spherical silver powder with concentrated particle size distribution, characterized in that: The preparation method comprises: Dissolve silver nitrate in deionized water at room temperature, and add ammonia water to prepare a silver ammonia solution; Dissolve the reducing agent in deionized water at room temperature, add sodium hydroxide solution to adjust the pH to 8-10, and obtain a reducing solution; Dissolving a fatty acid dispersant in an alcohol solution, preparing a certain amount of citrate solution with deionized water, adding the solution to the silver ammonia solution, and mechanically stirring and mixing to obtain an oxidizing solution; Deionized water and povidone were added into the reaction kettle, stirring was started, and after the povidone was thoroughly dissolved, the oxidizing solution and the reducing solution were added into the reaction kettle at an equal speed, and silver powder was obtained through stirring, centrifugation, drying and crushing.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the silver nitrate to the ammonia water is 10:8-10:
11.
3. The preparation method according to claim 1, characterized in that: The added amount of the fatty acid dispersant is 2-5% of the weight of the silver nitrate.
4. The preparation method according to claim 1, characterized in that: The fatty acid dispersant is one or more of linoleic acid, lauric acid, oleic acid, caprylic acid, stearic acid and palmitic acid.
5. The preparation method according to claim 1, characterized in that: The amount of the citrate solution added is 0.2-1% of the weight of the silver nitrate.
6. The preparation method according to claim 1, characterized in that: The added amount of the povidone is 20-30% of the weight of the silver nitrate.
7. The preparation method according to claim 1, characterized in that: The oxidation liquid and the reduction liquid are added into the reactor at a speed of 10-15 L / min, and the addition time is 3-5 minutes; The cumulative amount of the oxidizing liquid added to the reaction kettle is 40-70L; wherein the silver content is 2-3kg; The cumulative amount of the reducing solution added to the reactor is 35-55L.
8. The preparation method according to claim 1, characterized in that: The reducing solution, the oxidizing solution and the polyvidone solution added to the reaction kettle are all kept at 35-40° C. before the reaction.
9. A large-particle micron-sized spherical silver powder with a concentrated particle size distribution, characterized in that: The method is prepared by any one of claims 1 to 8.
10. The large-particle micron-sized spherical silver powder with concentrated particle size distribution as claimed in claim 9 is used in TOPCon battery silver paste.
Citation Information
Patent Citations
Silver powder for electrode paste on front surface of solar cell and preparation method and application
CN107042316A
Method for preparing high-dispersibility and high-sphericity superfine silver powder on large scale
CN107661986A
Method for preparing silver powder with high specific surface area for TOPCON solar cell
CN116713475A
Micron silver powder for N-type photovoltaic cell silver paste and preparation method of micron silver powder
CN117620198A
Spherical silver powder and preparation method therefor, and conductive paste
WO2023173627A1
Cited By
Silver powder for TOPcon and preparation method thereof
CN120438636A
Preparation method of sphere-like silver powder and sphere-like silver powder
CN120984891A