Integrated forming method for multi-stage disc shaft structure
By using vacuum powder calcination and oscillating pressure sintering technology combined with ceramic jackets and gasket components in the preparation of multi-stage disc shaft structures, the problems of large material removal and long processing time are solved, and efficient and accurate multi-stage disc shafts are achieved Structural preparation significantly improves product performance and stability.
Patent Information
- Application Number
- CN202411288730.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The existing multi-stage disc shaft structure preparation process has problems such as large amount of material removal, long processing time, and unguaranteed processing accuracy.
Using a multi-stage disk-shaft structure integrated molding method, by filling the raw material powder into the ceramic jacket, setting up a multi-layer annular groove structure arranged in parallel and filling the gasket assembly, vacuum powder calcination and oscillation pressure sintering are performed, combining solid solution and Aging treatment forms an integrated multi-stage disc shaft structure.
It effectively reduces the waste of raw materials, shortens the processing cycle, improves processing accuracy and performance stability, reduces preparation costs, and avoids the problem of cracking of special-shaped parts during the molding process.
Smart Images

Figure CN118788967A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of disk-shaft manufacturing, and in particular to a method for integrating a multi-stage disk-shaft structure. Background Art
[0002] Small and medium-sized aircraft engines can effectively reduce the weight of the engine and reduce the manufacturing cost by reducing the number of parts. As the most severe load-bearing parts of the engine, the compressor and turbine disk-shaft system usually become the key components to ensure the reliable operation of the engine. The existing compressor and turbine disks are usually disk-shaft separated structures, which are connected and transmitted by gears or flanges. Not only are there many parts, but they are also expensive, and the reliability needs to be improved urgently. In recent years, in the development of advanced small and medium-sized aircraft engines, people have found that if the multi-stage disk-shaft system of the compressor and turbine is combined into one part, the number of parts can be effectively reduced, and the life and reliability can be improved. However, the current preparation method of such parts is usually to use rods with sufficient diameter size margin for machining. This method has the following disadvantages: during the processing of the rods, the amount of material removed between the disks is too large, resulting in a huge waste of raw materials, and due to the large amount of material removed, the processing time is too long, which doubles the preparation cycle, and improper control of the material removal process can easily lead to unstable processing accuracy and affect product performance, so it is urgent to improve. Summary of the invention
[0003] The technical problem solved by the present invention is to provide a method for integrated molding of a multi-stage disc-shaft structure, so as to solve the technical problems in the prior art of large material removal, long processing time and unguaranteed processing accuracy in the preparation process of the multi-stage disc-shaft structure.
[0004] The technical problem solved by the present invention is achieved by adopting the following technical solutions: A method for integrated molding of a multi-stage disk-shaft structure comprises the following steps: (1) The raw material powder is loaded into a ceramic sleeve, the ceramic sleeve is provided with a multi-layer annular groove structure arranged in parallel, the annular groove structure is filled with a gasket assembly, and after the gasket assembly is filled in the annular groove, it forms a cylindrical structure together with the ceramic sleeve; (2) placing the cylindrical structure in a matching sintering mold, the top and bottom of the sintering mold having piston pressure heads; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston pressure head to a median pressure and then applying an oscillating pressure load, the median pressure being 10 to 90 MPa, the oscillation frequency of the oscillating pressure load being in a range of 0.5 to 5 Hz, and the amplitude being in a range of 0 to 10 MPa; and the vacuum degree during the sintering process being less than or equal to 1×10 -5 Pa; cooling after sintering is completed; (3) Solution treatment and aging treatment are continued in the vacuum powder forging equipment, and then the product is cooled and taken out of the furnace to obtain an integrated multi-stage disc-shaft structure.
[0005] Furthermore, in step (1), the raw material powder is a high temperature alloy powder or a titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm.
[0006] Furthermore, in step (1), the material of the ceramic sheath is Si 3 N 4 、ZrO 2 or Al 2 O 3 One or more of the above, the thickness of the ceramic sheath is 2~5mm.
[0007] Furthermore, in step (2), the sintering mold is a hollow cylindrical structure, the sintering mold and the piston-type pressure head are both made of graphite, and the inner diameter of the sintering mold matches the outer diameter of the ceramic sleeve. Furthermore, in step (1), the gasket assembly includes a circular gasket, which is composed of at least two independently arranged gasket blocks, and the upper and lower surfaces of the two gasket blocks are both provided with protruding sub-gasket blocks, and the gasket assembly fully fills the annular groove structure. Preferably, the gasket material is graphite, Si 3 N 4 、ZrO 2 and Al 2 O 3 A bulk material.
[0008] Furthermore, in step (2), the sintering temperature is 1100~1300°C, and the sintering time is 1~3h; the heating rate during the sintering process is 5~100°C / min; after the sintering is completed, forced cooling is performed, and the cooling rate of the forced cooling is 5~10°C / min.
[0009] Furthermore, in step (3), the solution treatment temperature is 1100-1250°C and the time is 2-6 hours; the aging treatment temperature is 600-800°C and the time is 5-15 hours.
[0010] Furthermore, in step (3), the vacuum degree during the solution treatment and aging treatment is less than or equal to 1×10 -5 Pa.
[0011] Furthermore, in step (2) and step (3), cooling is performed by a composite forced cooling method of water circulation and argon gas injection.
[0012] Beneficial effects: The multi-stage disk-shaft structure integrated molding method described in the present invention has a small amount of material removal, avoiding the waste of raw materials. Its multiple processes can be completed in the vacuum powder forging equipment, without the need to frequently change the processing site, effectively reducing the process links, shortening the processing cycle, and reducing the pollution caused by the transfer process; the unique design of the ceramic sleeve combined with the gasket assembly solves the problem of uneven force during the molding process, resulting in cracking and poor mechanical properties of special-shaped parts, and in the sintering process, vacuum sintering and constant pressure plus oscillating load sintering process are adopted to effectively realize the replacement of forging with pressure for powder high-temperature alloys. In the sintering process, the sample is deformed and strengthened to refine its grain structure, improve its density, and ensure the organization and performance of the sample. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic diagram of the structure of the ceramic sleeve in the present invention.
[0014] Figure 2 It is a schematic structural diagram of the cross section of the gasket assembly in the present invention.
[0015] Figure 3 It is a structural schematic diagram of the sintering mold in the present invention.
[0016] Among them: 1. Ceramic sleeve; 2. Annular groove; 3. Gasket assembly; 4. Gasket block; 5. Sub-gasket block; 6. Die body; 7. Sintering cavity; 8. Piston pressure head. DETAILED DESCRIPTION
[0017] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.
[0018] The ceramic sleeve 1 used in each embodiment of the present invention is as follows Figure 1 and Figure 3 As shown, the ceramic sleeve 1 is provided with parallel multi-layer annular grooves 2, and the annular grooves 2 are filled with gasket components 3; the gasket components used are as shown in FIG. Figure 2 and Figure 3 As shown, the gasket assembly 3 includes a circular gasket, which is composed of at least two independently arranged gasket blocks 4. The upper and lower surfaces of the two gasket blocks 4 are both provided with protruding sub-gasket blocks 5. The gasket assembly 3 fully fills the annular groove 2 structure.
[0019] Sintering mold Figure 3 As shown, it includes a mold body 6, which includes a cylindrical structure with a sintering cavity 7. A piston-type pressure head 8 is arranged at the top and bottom of the sintering cavity 7. The mold body 6 and the piston-type pressure head 8 are both made of graphite. The ceramic sleeve 1 is placed in the sintering cavity 7, and the inner diameter of the sintering cavity 7 matches the outer diameter of the ceramic sleeve 1.
[0020] Example 1 The multi-stage disk-shaft structure integrated molding method described in this embodiment includes the following steps: (1) The raw material powder is loaded into a ceramic sleeve, wherein the raw material powder is a titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm; wherein the material of the ceramic sleeve is Si 3 N 4 The thickness of the ceramic sleeve is 5 mm. The ceramic sleeve is provided with parallel multi-layer annular groove structures, and the annular groove structures are filled with gasket components. After the gasket components are filled in the annular grooves, they form a solid cylindrical structure with the ceramic sleeve; (2) placing the cylindrical structure in a matching sintering mold; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston-type pressure head to the median pressure and then applying an oscillating pressure load. In this embodiment, the median pressure is 30 MPa, the oscillation frequency range of the oscillating pressure load is 0.6 Hz, and the amplitude range is 5 MPa; maintaining a vacuum degree of 1×10 -5 Pa; the heating rate during the sintering process is 50℃ / min, and the temperature is raised from room temperature to 1100℃ and then sintered for 3h; forced cooling is performed after sintering; the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 8℃ / min; (3) Solution treatment and aging treatment are continued in the vacuum powder forging equipment. The vacuum degree is maintained at 1×10 -5 Pa; the solution treatment temperature is 1100℃ and the time is 6h; the aging treatment temperature is 800℃ and the time is 5h; then it is forced cooled and taken out of the furnace, and the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 8℃ / min; after taking out of the furnace, an integrated multi-stage disc-shaft structure is obtained.
[0021] Example 2 The multi-stage disk-shaft structure integrated molding method described in this embodiment includes the following steps: (1) The raw material powder is loaded into a ceramic sleeve, wherein the raw material powder is a titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm; wherein the material of the ceramic sleeve is Si 3 N 4 The thickness of the ceramic sleeve is 4 mm. The ceramic sleeve is provided with parallel multi-layer annular groove structures, and the annular groove structures are filled with gasket components. After the gasket components are filled in the annular grooves, they form a solid cylindrical structure with the ceramic sleeve; (2) placing the cylindrical structure in a matching sintering mold; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston pressure head to the median pressure and then applying an oscillating pressure load. In this embodiment, the median pressure is 40 MPa, the oscillation frequency range of the oscillating pressure load is 0.5 Hz, and the amplitude range is 10 MPa; maintaining a vacuum degree of 1×10 -5 Pa; the heating rate during sintering is 35℃ / min, and the temperature is raised from room temperature to 1200℃ and then sintered for 2h; forced cooling is performed after sintering; the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 10℃ / min; (3) Solution treatment and aging treatment are continued in the vacuum powder forging equipment. The vacuum degree is maintained at 1×10 -5 Pa; the solution treatment temperature is 1200℃ and the time is 4h; the aging treatment temperature is 650℃ and the time is 6h; then it is forced cooled and taken out of the furnace, and the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 10℃ / min; after taking out of the furnace, an integrated multi-stage disc-shaft structure is obtained.
[0022] Example 3 The multi-stage disk-shaft structure integrated molding method described in this embodiment includes the following steps: (1) The raw material powder is loaded into a ceramic sleeve, wherein the raw material powder is a titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm; wherein the material of the ceramic sleeve is Si 3 N 4 The thickness of the ceramic sleeve is 4 mm. The ceramic sleeve is provided with parallel multi-layer annular groove structures, and the annular groove structures are filled with gasket components. After the gasket components are filled in the annular grooves, they form a solid cylindrical structure with the ceramic sleeve; (2) placing the cylindrical structure in a matching sintering mold; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston pressure head to the median pressure and then applying an oscillating pressure load. In this embodiment, the median pressure is 50 MPa, the oscillation frequency range of the oscillating pressure load is 0.5 Hz, and the amplitude range is 4 MPa; maintaining a vacuum degree of 1×10 -5 Pa; the heating rate during the sintering process is 60℃ / min, and the temperature is raised from room temperature to 1300℃ and then sintered for 1h; forced cooling is performed after sintering; the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 6℃ / min; (3) Solution treatment and aging treatment are continued in the vacuum powder forging equipment. The vacuum degree is maintained at 1×10 -5Pa; the solution treatment temperature is 1250℃ and the time is 2h; the aging treatment temperature is 600℃ and the time is 15h; then it is forced cooled and taken out of the furnace, and the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 6℃ / min; after taking out of the furnace, an integrated multi-stage disc-shaft structure is obtained.
[0023] Comparative Example 1 The difference between this control example and Example 1 is that in step (2), no oscillating pressure load is used, but only a constant pressure of 30 MPa is used, and the rest is the same.
[0024] Comparative Example 2 The difference between this comparative example and comparative example 1 is that in step (2), the vacuum degree is greater than 1×10 -5 Pa, the rest are the same.
[0025] Comparative Example 3 In this comparative example, the diameter of the raw material powder is dispersed in the range of 300-400 μm, and the rest is the same as that of Example 1.
[0026] Comparative Example 4 In this comparative example, the multi-stage disc-shaft structure is processed by conventional forging cylindrical blank removal processing.
[0027] The multi-stage disk-shaft structures prepared in Examples 1-3 and Comparative Examples 1-4 were tested and compared, and the structures are shown in Table 1.
[0028] Among them: room temperature stretching adopts the room temperature test method for metal material tensile test recorded in GB / T 228-2010; high temperature stretching adopts the high temperature tensile test method for metal materials recorded in GB / T 4338-2006; fatigue resistance test adopts the axial equal amplitude low cycle fatigue test method for metal materials recorded in GB / T15248-2008; grain size adopts the metal average grain size determination method recorded in GB / T 6394-2017.
[0029] Table 1
[0030] As shown in Table 1, the technical solution of the present invention is compared with the traditional method recorded in Reference Example 4, and the preparation cycle is shortened by more than 50%, and the raw material utilization rate is as high as 90%, which is far better than the 30% of the traditional method, greatly reducing the preparation cost, and the grain size, density and mechanical properties are not significantly different from the products prepared by the traditional method, but in actual operation, among the multiple products produced in the same batch, the yield rate of the method described in the present invention is significantly greater than that of the products prepared by the traditional method, without cracking, and the processing accuracy and performance are more stable. As shown in Reference Examples 1 to 3, the technical solution of the present invention is the result of the joint cooperation of the processing procedure and parameter control. When the processing procedure or parameter control is improper, the effect is not ideal.
[0031] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for integrated molding of a multi-stage disk-shaft structure, characterized in that: The steps include: (1) The raw material powder is loaded into a ceramic sleeve, the ceramic sleeve is provided with a multi-layer annular groove structure arranged in parallel, the annular groove structure is filled with a gasket assembly, and the gasket assembly is filled in the annular groove to form a cylindrical structure with the ceramic sleeve; (2) placing the cylindrical structure in a matching sintering mold, wherein the top and bottom of the sintering mold have piston-type pressure heads; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston-type pressure head to a median pressure and then applying an oscillating pressure load, wherein the median pressure is 10 to 90 MPa, the oscillation frequency range of the oscillating pressure load is 0.5 to 5 Hz, and the amplitude range is 0 to 10 MPa; the vacuum degree during the sintering process is less than or equal to 1×10 -5 Pa; cooling after sintering; (3) Solution treatment and aging treatment are continued in the vacuum powder forging equipment, and then the product is cooled and taken out of the furnace to obtain an integrated multi-stage disc-shaft structure.
2. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (1), the raw material powder is a high temperature alloy powder or a titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm.
3. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (1), the material of the ceramic sheath is one or more of Si3N4, ZrO2 or Al2O3, and the thickness of the ceramic sheath is 2-5 mm.
4. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (2), the sintering mold is a hollow cylindrical structure, the sintering mold and the piston-type pressure head are both made of graphite, and the inner diameter of the sintering mold matches the outer diameter of the ceramic sleeve.
5. The method for integrated molding of a multi-stage disk-shaft structure according to claim 4, characterized in that: In step (1), the gasket assembly includes a circular gasket, which is composed of at least two independently arranged gasket blocks, and the upper and lower surfaces of the two gasket blocks are both provided with protruding sub-gasket blocks, and the gasket assembly fully fills the annular groove structure; wherein the gasket material is one of graphite, Si3N4, ZrO2 and Al2O3 block materials.
6. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (2), the sintering temperature is 1100°C~1300°C, and the sintering time is 1~3h; the heating rate during the sintering process is 5~100°C / min; after the sintering is completed, forced cooling is performed, and the cooling rate of the forced cooling is 5~10°C / min.
7. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (3), the solution treatment temperature is 1100-1250°C and the time is 2-6 hours; the aging treatment temperature is 600-800°C and the time is 5-15 hours.
8. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (3), the vacuum degree during the solution treatment and aging treatment is less than or equal to 1×10 -5 Pa.
9. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (2) and step (3), cooling adopts a composite forced cooling method of water circulation and argon gas filling.
Citation Information
Patent Citations
Automobile brake disc and manufacturing method thereof
CN105041921A
Preparation method of automobile brake disc
CN112658260A
Ceramic discs and round bars, methods of manufacture and articles thereof
CN115135434A
Low-melting-point powder auxiliary brazing filler metal forming device
CN116765400A
Process of manufacture of articles from ceramic powder
RU2121410C1
Cited By