Preparation method for controllable nucleation of micro-nano silver powder

By introducing a synthetic control liquid and specific reaction conditions, the problems of complex preparation process of front-side silver powder and insufficient surface roughness of the silver powder are solved, and the controllable nucleation preparation of micro-nano silver powder with high surface roughness and strong sintering activity is achieved, which is suitable for large-scale Production and demand for front-side silver paste for solar cells.

CN118788975APending Publication Date: 2024-10-18DONGFANG ELECTRIC CHENGDU INTELLIGENT TECH CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410865449.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the existing technology, the preparation process of front-side silver powder is complicated and it is difficult to control the reaction conditions, resulting in a cumbersome preparation process, low repetition rate, and difficulty in adapting to large-scale production. Moreover, the surface roughness and sintering activity of the prepared silver powder are insufficient to meet the needs of the front-side of solar cells. Silver paste’s demand for powder.

Method used

By introducing a synthetic control liquid, nucleation sites are provided to inhibit homogeneous nucleation and promote heterogeneous nucleation. Specific silver nitrate and reducing agent purity, pH value adjustment and stirring conditions are used to control the reaction between silver nitrate and reducing solution. Micro-nano silver powder with high surface roughness is formed.

Benefits of technology

It achieves controllable nucleation preparation of silver powder, improves the repeatability and sintering activity of batch preparation, is suitable for large-scale production, meets the powder demand for silver paste on the front of solar cells, and ensures the consistency and high quality of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788975A_ABST
    Figure CN118788975A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method for controllable nucleation of micro-nano silver powder, and relates to the technical field of micro-nano silver powder preparation.A specific preparation method is adopted for preparing synthetic control liquid, nucleation point positions are provided for silver nitrate and a reduction solution in the reaction process through introduction of the synthetic control liquid, homogeneous nucleation is inhibited, heterogeneous nucleation is promoted, and the micro-nano silver powder is prepared. The influence caused by other condition factors in the silver powder preparation process is greatly reduced, the micro-nano silver powder prepared through the method is good in consistency, high in sphericity degree, few in control step and suitable for batch and large-scale production, and due to the fact that the reaction control liquid has a strong leading effect on silver powder synthesis and is high in adaptability to downstream slurry application, the micro-nano silver powder prepared through the method is good in uniformity and good in sphericity degree. The particle size parameter of the prepared silver powder can be adjusted only by adjusting and controlling the addition amount of the reaction control liquid, quantitative indexes are provided for silver powder parameter adjustment and control, and the obtained micro-nano silver powder has certain surface roughness and sintering activity and can meet the requirement of front silver paste of a solar cell for powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of micro-nano silver powder preparation, and in particular to a method for preparing micro-nano silver powder with controllable nucleation. Background Art

[0002] With the development of society, the demand for energy is increasing day by day. Solar energy has become one of the preferred new energy technologies developed and utilized by countries around the world. Solar photovoltaic power generation is a technology that directly converts solar energy into electrical energy. With its clean, environmentally friendly and widely distributed characteristics, it has become the most widely used form of solar energy utilization technology.

[0003] With the rapid development of the photovoltaic and electronics industries, the demand for silver paste with silver powder as the main functional material has increased year by year. Taking the photovoltaic industry as an example, silver powder is mainly used in the preparation of front and back silver pastes for solar cells. According to statistics from the China Photovoltaic Industry Association: China's consumption of silver powder for photovoltaics in 2020 was about 1,650 tons, and it is expected that the demand for silver powder for photovoltaics will reach 2,572 tons by 2025. Therefore, the optimization of the silver powder preparation process and the improvement of the powder are imminent. Compared with the silver powder used for the back silver paste, the front electrode requires a high aspect ratio and a narrower line width. Therefore, the silver powder used requires a certain surface roughness and sintering activity. Surface roughening can meet good thixotropic properties during printing, and high sintering activity can ensure good electrical properties under narrow line width conditions. Therefore, the preparation process of the front silver powder is significantly different from that of the back silver powder.

[0004] The current preparation process of positive silver powder involves two processes: silver powder nucleation and growth. It is necessary to strictly control the concentration of reactants, reaction pH, ambient temperature, reaction rate and time during the reaction process, resulting in a cumbersome preparation process, low repetition rate, and difficulty in adapting to large-scale production.

[0005] Therefore, there is an urgent need for a controllable reaction that can reduce the influence of other conditions on the reaction to form micron powders, prepare micron powders with good batch repeatability, high sintering activity, quantify the preparation process of micron powders, and adapt to large-scale production process preparation methods to meet the needs of batch preparation of micro-nano silver powders. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing micro-nano silver powder with controllable nucleation, so that the obtained silver powder has a certain surface roughness and sintering activity, and the reaction is controllable and the batch preparation has good repeatability. At the same time, the obtained silver powder can meet the demand for powder of the front silver paste of solar cells.

[0007] The present invention is achieved through the following technical solutions: A method for preparing micro-nano silver powder with controllable nucleation comprises the following steps: S1, dissolving silver nitrate in deionized water, maintaining the solution temperature at 25-50°C, adding an acidic reagent and adjusting the pH value of the solution to 3.0-6.0, to obtain an oxidation solution A1, wherein the concentration of silver nitrate in the oxidation solution A1 is 0.1-3.0 mol / L; separately taking 1-10% of the mass of silver nitrate in the A1 solution and dissolving it in deionized water, to obtain an oxidation solution A2, wherein the concentration of silver nitrate in the oxidation solution A2 is 0.1-3.0 mol / L; S2, dissolving a reducing agent in deionized water, maintaining the solution temperature at 25-50°C, adding an alkaline agent and adjusting the pH value of the solution to 2.0-6.0, to obtain a reducing solution B1, wherein the reducing agent concentration in the reducing solution B1 is 0.1-1.0 mol / L; dissolving another reducing agent of 1-10% of the reducing agent mass in the B1 solution in deionized water, to obtain a reducing solution B2; wherein the reducing agent concentration in the reducing solution B2 is 0.1-1.0 mol / L; S3, taking 6-10% of the mass of silver nitrate in the oxidation solution A1 in step S1 and dissolving it in deionized water to obtain a synthetic dispersant C1, wherein the amount of deionized water added is 20-50 times the mass of the dispersant; taking 500-800% of the mass of silver acid in the oxidation solution A2 in step S1 and dissolving it in deionized water to obtain a synthetic dispersant C2, wherein the amount of deionized water added is 10-20 times the mass of the dispersant; S4, adding the reducing solution B2 to the control dispersant C2, stirring for 20-40 minutes to obtain a synthetic control liquid precursor, adding the oxidizing solution A2 to the synthetic control liquid precursor, stirring for 5-25 hours, to obtain a synthetic control liquid D; S5. Add synthetic control liquid D containing 20-200% of the mass of silver nitrate in oxidizing solution A1 to oxidizing solution A1, add synthetic dispersant C1 to reducing solution B1, stir for 3-5 minutes respectively, transport oxidizing solution A1 mixed with synthetic control liquid D and reducing solution B1 with synthetic dispersant C1 to reactor respectively, stir for 25-40 minutes, let stand for 10-30 minutes to obtain micro-nano silver powder solution, wash with centrifuge until the conductivity of micro-nano silver powder solution is less than 10μs / cm, dry, and pulverize to obtain micro-nano silver powder with high surface roughness.

[0008] Furthermore, the purity of the silver nitrate used in each step is 99.5-99.9%, and the purity of the reducing agent is 99.0%-99.9%.

[0009] Furthermore, in step S1, the acidic reagent for adjusting the pH value is one or more of nitric acid, acetic acid, carbonic acid, and phenol.

[0010] Furthermore, in step S2, the reducing agent is one or more of ascorbic acid, hydrazine hydrate, glucose, acetone and formaldehyde.

[0011] Furthermore, in step S2, the alkaline reagent for adjusting the pH value is one or more of sodium hydroxide, potassium hydroxide, and ammonia water.

[0012] Furthermore, in step S3, the dispersant is one or more of polyvinyl pyrrolidone, gelatin, hexadecyltrimethylammonium bromide, gum arabic, cellulose, polyethylene glycol and polyvinyl alcohol, and the dispersants added to the synthetic dispersant C1 and the control dispersant C2 are the same type of reagents.

[0013] Furthermore, in step S4, the stirring rate of the synthesis control liquid D is 100-200 r / min, and the insulation temperature is 20-60°C.

[0014] Furthermore, in step S4, the synthesis control liquid D forms nano nucleation sites by slow reaction, and the particle size of the nucleation sites is 30-80 nm; when the silver nitrate content in the oxidation solution A1 is constant, the size of the micro-nano powder can be controlled by controlling the amount of synthesis control liquid D added.

[0015] Furthermore, in step S5, a peristaltic pump is used to transport the oxidizing solution A1 mixed with the synthetic control liquid D and the reducing solution B1 added with the synthetic dispersant C1 into the reactor. The flow rate of the peristaltic pump is 11-16 L / min, the insulation temperature of the reactor is 25-30°C, and the stirring rate is 300-1000 r / min.

[0016] Furthermore, the diameters of the Y-tube and the peristaltic pump are 5-80 cm, and the discharge rate of the peristaltic pump is 10-30 L / min.

[0017] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. The present invention is different from the existing silver powder preparation technology. It provides a new preparation method of micro-nano silver powder with controllable nucleation. It introduces a new synthetic control liquid to provide nucleation sites for silver nitrate and reducing solution during the reaction, inhibits homogeneous nucleation, promotes heterogeneous nucleation, and greatly reduces the influence of other conditions and factors on powder nucleation during the silver powder preparation process. The prepared silver powder has good consistency, high sphericity, fewer control steps, and is suitable for large-scale batch production.

[0018] 2. In the present invention, in the preparation process steps, the reaction control liquid has a strong dominant effect on the synthesis of silver powder and is highly adaptable to downstream slurry applications. The particle size parameters of the prepared silver powder can be adjusted by simply adjusting the amount of reaction control liquid added, which provides a quantitative indicator for the control of silver powder parameters.

[0019] 3. In the present invention, the silver powder prepared by the method has high surface roughness and high sintering activity. The silver powder has good thixotropic properties in the printing process. The silver powder with high sintering activity can ensure that it can still maintain good electrical properties under the condition of narrow line width, and can meet the requirements of silver powder in the fields of photovoltaic front silver paste and so on.

[0020] 4. In the present invention, in order to facilitate accurate material calculation and reduce the influence of impurities on synthesis control, the purity of silver nitrate used in each step is 99.5-99.9%, and the purity of reducing agent is 99.0%-99.9%. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 30.0 K is a scanning electron microscope image of the nano-nucleation sites in the synthetic control solution D prepared in Example 1.

[0022] Figure 2 This is a scanning electron microscope image of the 5.0K micro-nano silver powder prepared in Example 1.

[0023] Figure 3 This is a scanning electron microscope image of the micro-nano silver powder 10.0K prepared in Example 1. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0025] In the following examples, the purity of the silver nitrate used is 99.7%, and the purity of the ascorbic acid, hydrazine hydrate, and glucose used are 99.2%, 99.5%, and 99.6%, respectively.

[0026] In the present invention, in order to facilitate accurate material calculation and reduce the influence of impurities on synthesis control, the purity of the silver nitrate used should be preferably controlled within the range of 99.5-99.9%. The purity of the reducing agent should preferably be within the range of 99.0%-99.9%.

[0027] In the present invention, in step S1, the acidic reagent for adjusting the pH value is one or more of nitric acid, acetic acid, carbonic acid, and phenol. In the following implementation, an acidic reagent with a concentration of 10% acetic acid, 50% phenol, and 20% carbonic acid is used as an example for illustration.

[0028] In the present invention, in step S2, the alkaline reagent for adjusting the pH value is one or more of sodium hydroxide, potassium hydroxide, and ammonia water. In the following implementation, an alkaline reagent with a concentration of 10% sodium hydroxide, 15% potassium hydroxide, and 85% ammonia water is used as an example for illustration.

[0029] In step S3 of the following embodiment, the dispersant is polyvinyl pyrrolidone K30 as an example to further illustrate the scheme. The dispersant can be one or more of polyvinyl pyrrolidone, gelatin, hexadecyl trimethyl ammonium bromide, gum arabic, cellulose, polyethylene glycol and polyvinyl alcohol, and the dispersant added to the synthetic dispersant C1 and the control dispersant C2 is the same type of reagent.

[0030] In this scheme, a large number of experiments have shown that in step S4, the stirring rate of the synthetic control liquid D is 100-200r / min, the insulation temperature is 20-60°C, and the quality of the prepared product is relatively better. In addition, the synthetic control liquid D adopts a slow reaction method to form nano nucleation sites, and the particle size of the nucleation sites is preferably 30-80nm.

[0031] When the silver nitrate content in the oxidation solution A1 is constant, the size of the micro-nano powder can be controlled by controlling the amount of synthesis control solution D added.

[0032] In step S5 of the present invention, a peristaltic pump is used to transport the oxidizing solution A1 mixed with the synthetic control liquid D and the reducing solution B1 added with the synthetic dispersant C1 into the reactor. The flow rate of the peristaltic pump is 11-16 L / min, the insulation temperature of the reactor is 25-30° C., and the stirring rate is 300-1000 r / min. The quality of the obtained micro-nano silver powder is more stable and the product quality is better.

[0033] In the following embodiment, the diameter of the Y-tube and the peristaltic pump is set to 50 cm, and the discharge rate of the peristaltic pump is set to 20 L / min. In specific implementation, the diameter of the Y-tube and the peristaltic pump should be controlled to 5-80 cm, and the discharge rate of the peristaltic pump should be controlled to 10-30 L / min.

[0034] Example 1 A method for preparing micro-nano silver powder with controllable nucleation, which relates to the technical field of micro-nano silver powder preparation, comprises the following steps: (1) Weigh 500 g of silver nitrate and dissolve it in 2.94 L of deionized water, adjust the solution temperature to 30°C, add 10% acetic acid solution to adjust the pH value of the silver nitrate solution to 4.0, and obtain oxidation solution A1; take 10 g of silver nitrate and dissolve it in 29.5 mL of deionized water to obtain oxidation solution A2; (2) Weigh 259.1 g of ascorbic acid and dissolve it in 2.94 L of deionized water. Regulate the solution temperature to 30°C. Add 20% sodium hydroxide solution to adjust the pH value of the ascorbic acid solution to 4.5 to obtain a reduction solution B1. Weigh 5 g of ascorbic acid and dissolve it in 100 mL of deionized water to obtain a reduction solution B2. (3) Weigh 50 g of polyvinyl pyrrolidone K30 and dissolve it in 1000 ml of deionized water. Adjust the solution temperature to 30° C. to obtain a synthetic dispersant C1. (4) Weigh 50 g of polyvinyl pyrrolidone K30 and dissolve it in 250 mL of deionized water. Stir at 500 r / min for 40 min and adjust the solution temperature to 30 °C to obtain the controlled dispersant C2. (5) Add the reducing solution B2 to the control dispersant C2 and stir for 20 min to obtain a synthetic control liquid precursor. Add the oxidizing solution A2 to the synthetic control liquid precursor and stir for 5 h to obtain a synthetic control liquid D. Figure 1 , Figure 1 is a scanning electron microscope image of the nano-nucleation site in the prepared synthetic control solution D at 30.0 K; (6) Add the synthetic dispersant C1 into the reducing solution B1 and stir at 500 r / min for 10 min; (7) Take 100 g of synthetic control solution D and add it into oxidation solution A1, and stir at 500 r / min for 10 min; (8) The oxidation solution A1 and the reduction solution B1 were pumped into a Y-type tube reactor by a peristaltic pump at a speed of 20 L / min for collection. The stirring rate of the reactor was 1000 r / min. The solution was stirred for 10 min and allowed to stand for 10 min. The solution was centrifuged and washed until the conductivity of the solution was below 10 μs / cm. The solution was collected and dried. After being pulverized by a pulverizer for 10 min, it was sieved and collected with a 400-mesh screen to obtain micro-nano silver powder with high surface roughness. Figure 2 , 3 , are scanning electron microscope images of micro-nano silver powder 5.0K and 10.0K respectively.

[0035] According to the above specific method steps, the amount of polyvinyl pyrrolidone K30 added in step 3 is adjusted according to Table 1, and the other conditions are the same to prepare various micro-nano silver powders with high surface roughness. The performance parameters such as particle size distribution D10, particle size distribution D50, particle size distribution D90, tap density, specific surface area, etc. of each group of micro-nano silver powders are tested, and the results are shown in Table 1.

[0036] Table 1 As shown in Table 1, the amount of dispersant added in the synthetic dispersant C1 is controlled at 6-10% of the mass ratio of the silver nitrate in the oxidation solution A1 to obtain the size of the silver powder used in the positive electrode of the Topcon battery. When the amount added is 25g (accounting for 5% of the mass of the silver nitrate in A1), the powder size is larger, and when the amount added is 60g (accounting for 12% of the mass of the silver nitrate in A1), the powder size is smaller. The silver powders prepared in Groups 1 and 3 do not meet the current application requirements.

[0037] Example 2 A method for preparing micro-nano silver powder with controllable nucleation, which relates to the technical field of micro-nano silver powder preparation, comprises the following steps: (1) Weigh 500 g of silver nitrate and dissolve it in 3.92 L of deionized water, adjust the solution temperature to 35 °C, add 50% phenol solution to adjust the pH value of the silver nitrate solution to 3.5, and obtain oxidation solution A1; weigh 10 g of silver nitrate and dissolve it in 29.5 mL of deionized water to obtain oxidation solution A2; (2) Weigh 259.1 g of ascorbic acid and dissolve it in 3.92 L of deionized water. Regulate the solution temperature to 35 °C. Add 80% ammonia water to adjust the pH value of the ascorbic acid solution to 4.0 to obtain a reduction solution B1. Weigh 5 g of ascorbic acid and dissolve it in 100 mL of deionized water to obtain a reduction solution B2. (3) Weigh 50 g of polyvinyl pyrrolidone K30 and dissolve it in 1000 ml of deionized water. Adjust the solution temperature to 30° C. to obtain a synthetic dispersant C1. (4) Weigh 50 g of polyvinyl pyrrolidone K30 and dissolve it in 250 mL of deionized water. Stir at 500 r / min for 40 min and adjust the solution temperature to 30 °C to obtain the controlled dispersant C2. (5) Add the reducing solution B2 to the control dispersant C2 and stir for 20 minutes to obtain a synthetic control liquid precursor. Add the oxidizing solution A2 to the synthetic control liquid precursor and stir for 5 hours to obtain a synthetic control liquid D. (6) Add the synthetic dispersant C1 into the reducing solution B1 and stir at 500 r / min for 10 min; (7) Add 100 g of synthetic control solution D into the oxidation solution A1 and stir at 500 r / min for 10 min; (8) The oxidizing solution A1 and the reducing solution B1 were pumped into a Y-tube reactor using a peristaltic pump at a speed of 20 L / min for collection. The stirring rate of the reactor was 1000 r / min. The solution was stirred for 10 min and allowed to stand for 10 min. The solution was centrifuged and washed until the conductivity of the solution was below 10 μs / cm. The solution was collected and dried. After pulverization with a pulverizer for 10 min, it was sieved and collected with a 400-mesh sieve to obtain micro-nano silver powder with high surface roughness.

[0038] According to the above specific method steps, the amount of polyvinyl pyrrolidone K30 added in step 4 is adjusted according to Table 2, and the other conditions are the same to prepare various micro-nano silver powders with high surface roughness. The performance parameters such as particle size distribution D10, particle size distribution D50, particle size distribution D90, tap density, specific surface area, etc. of each group of micro-nano silver powders are tested, and the results are shown in Table 2.

[0039] Table 2 The above results show that when the amount of dispersant added in dispersant C2 is controlled at 500-800% of the mass ratio of silver nitrate in oxidizing solution A2, the prepared micro-nano silver powder can meet the size requirements of silver powder for the positive electrode of Topcon battery.

[0040] When the addition amount is 10 g (accounting for 100% of the mass of silver nitrate A1), the dispersing effect of the control dispersant C2 is insufficient, resulting in too fast reaction of the oxidizing solution A2 and the reducing solution B2 in the synthetic control solution D, and insufficient aggregation of the silver source to form nano-dots.

[0041] When the addition amount is 90g (accounting for 900% of the mass of silver nitrate A1), the dispersing effect of the control dispersant C2 is too strong, which makes it difficult for the oxidation solution A2 and the reduction solution B2 in the synthetic control solution D to react, and nano-dots cannot be effectively generated to control the subsequent reaction. It can be seen that the silver powders obtained in groups 4 and 6 do not meet the application requirements of the positive electrode of the Topcon battery.

[0042] Example 3 A method for preparing micro-nano silver powder with controllable nucleation, which relates to the technical field of micro-nano silver powder preparation, comprises the following steps: (1) Weigh 5000 g of silver nitrate and dissolve it in 29.43 L of deionized water, adjust the solution temperature to 35°C, add 20% carbonate solution to adjust the pH value of the silver nitrate solution to 3.0, and obtain oxidizing solution A1; weigh 50 g of silver nitrate and dissolve it in 200 mL of deionized water to obtain oxidizing solution A2; (2) Weigh 2591 g of ascorbic acid and dissolve it in 29.43 L of deionized water, adjust the solution temperature to 35 °C, add 20% potassium hydroxide solution to adjust the pH value of the ascorbic acid solution to 5.0, and obtain a reduction solution B1; weigh 60 g of ascorbic acid and dissolve it in 300 mL of deionized water to obtain a reduction solution B2; (3) Weigh 490 g of polyvinyl pyrrolidone K30 and dissolve it in 10 L of deionized water. Adjust the solution temperature to 35 °C to obtain a synthetic dispersant C1. (4) Weigh 400 g of polyvinyl pyrrolidone K30 and dissolve it in 4 L of deionized water. Stir at 500 r / min for 40 min and adjust the solution temperature to 35 °C to obtain controlled dispersant C2. (5) Add the reducing solution B2 to the control dispersant C2 and stir for 30 minutes to obtain a synthetic control liquid precursor. Add the oxidizing solution A2 to the synthetic control liquid precursor and stir for 10 hours to obtain a synthetic control liquid D. (6) Add the synthetic dispersant C1 into the reducing solution B1 and stir at 500 r / min for 10 min; (7) Add 1000 g of synthetic control solution D into oxidation solution A and stir at 500 r / min for 10 min; (8) The oxidizing solution A and the reducing solution B1 were pumped into a Y-tube reactor using a peristaltic pump at a speed of 20 L / min and collected. The stirring rate of the reactor was 1000 r / min. The solution was stirred for 10 min and allowed to stand for 10 min. The solution was centrifuged and washed until the conductivity of the solution was below 10 μs / cm. The solution was collected and dried. After pulverization in a pulverizer for 10 min, it was sieved and collected using a 400-mesh sieve to obtain micro-nano silver powder with high surface roughness.

[0043] Example 4 The only difference between this embodiment and embodiment 1 is that the pH value of the oxidizing solution A1 is adjusted to 4.2, and the pH value of the reducing solution B1 is adjusted to 5.0, and micro-nano silver powder is prepared.

[0044] Example 5 The only difference between this embodiment and embodiment 1 is that the solutions are prepared at a temperature of 45° C. to prepare the micro-nano silver powder.

[0045] Example 6 The only difference between this embodiment and embodiment 1 is that in the reducing solution B2, the amount of ascorbic acid added is 2.5 g, and micro-nano silver powder is prepared.

[0046] Example 7 The only difference between this embodiment and embodiment 1 is that the amount of the synthetic control solution D added to the oxidation solution A1 is 200 g, and micro-nano silver powder is prepared.

[0047] The micro-nano silver powders of the above-mentioned Examples 1-7 were tested, and the powder test parameters thereof are shown in Table 3.

[0048] Table 3 It can be seen from Examples 1 and 2 that: when faced with different concentrations of oxidizing solution, reducing solution, dispersing solution, ambient temperature, and pH value, the powder parameters prepared by using the same amount of nucleation control liquid are similar. It can be seen from Example 3 that when the amount of silver powder prepared increases, the amount of synthetic control liquid added can be increased proportionally, and the parameters of the synthesized powder have no significant changes compared with Examples 1 and 2, indicating that this method can achieve stable and large-scale preparation of micro-nano silver powder. In combination with Examples 1-3, the method of introducing controllable nucleation points, i.e., the addition of synthetic control liquid D, can prepare micro-nano silver powder with high surface roughness, and the distribution of its powder D50 is 1.92-2.01μm, and the tap density is 6.7-6.8g / cm 3 , with a specific surface area of ​​0.5-0.6m 2 / g, it meets the current Topcon solar cell front electrode's requirements for high surface roughness of micro-nano silver powder.

[0049] It can be found from Examples 4 and 5 that after adopting the method of introducing external crystal nuclei into powder growth, when the amount of synthesis control liquid added remains unchanged, the size parameters and specific surface area of ​​the powder do not change significantly when the conditions for controlling the reaction rate such as the pH value of the oxidation solution and the reduction solution and the reaction temperature are changed. This shows that the introduction of external nucleation points in the synthesis control liquid can inhibit unstable homogeneous nucleation during the reaction process and promote heterogeneous nucleation. The method of the present invention can simplify the condition control steps of micro-nano silver powder in the preparation process, and the stability of batch production of silver powder is significantly improved.

[0050] From Example 6, it can be learned that by reducing the amount of reducing agent B2 added in the synthesis control solution, the concentration of nano nucleation sites in the synthesis control solution can be reduced. When the silver nitrate silver source is constant, the particle size of the prepared micron powder is increased.

[0051] It can be seen from Example 7 that by increasing the amount of synthesis control liquid added, the nucleation sites introduced during the synthesis process are increased and the particle size of the generated powder is reduced.

[0052] It can be seen from the above examples that the synthetic control liquid is a key factor in the preparation of the powder of the present invention. The precise control of the preparation conditions and dosage of the synthetic control liquid can achieve the purpose of quantitatively controlling the parameters of the micron powder.

[0053] In the field of preparation of micro-nano silver powder with high surface roughness, the existing technologies all need to strictly control the reaction rate of silver nitrate solution and reducing solution, including but not limited to the need to strictly control the process conditions such as reactant temperature, pH value, concentration, etc., in order to finally obtain micro-nano silver powder that meets the requirements. It can be seen that the process requirements and operation requirements are extremely high, and it is not convenient for mass production. At the same time, the parameters such as the particle size of the prepared product fluctuate greatly. In the present invention, a method for preparing micro-nano silver powder with controllable nucleation is proposed. In the process of reaction synthesis between silver nitrate solution and reducing solution, nano nucleation sites (synthesis control liquid) are introduced externally to inhibit uncontrollable homogeneous nucleation in the reaction process between silver nitrate solution and reducing solution, promote controllable heterogeneous nucleation, and make the final powder parameters controlled by the synthesis control liquid, which can simplify the process control steps in the preparation process of silver powder, achieve the purpose of stable and controllable preparation of micro-nano silver powder, and is suitable for batch and industrial production.

[0054] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.

[0055] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing micro-nano silver powder with controllable nucleation, characterized in that: The steps include: S1, dissolving silver nitrate in deionized water, maintaining the solution temperature at 25-50°C, adding an acidic reagent and adjusting the pH value of the solution to 3.0-6.0, to obtain an oxidation solution A1, wherein the concentration of silver nitrate in the oxidation solution A1 is 0.1-3.0 mol / L; separately taking 1-10% of the mass of silver nitrate in the A1 solution and dissolving it in deionized water, to obtain an oxidation solution A2, wherein the concentration of silver nitrate in the oxidation solution A2 is 0.1-3.0 mol / L; S2, dissolving a reducing agent in deionized water, maintaining the solution temperature at 25-50°C, adding an alkaline agent and adjusting the pH value of the solution to 2.0-6.0, to obtain a reducing solution B1, wherein the reducing agent concentration in the reducing solution B1 is 0.1-1.0 mol / L; dissolving another reducing agent of 1-10% of the reducing agent mass in the B1 solution in deionized water, to obtain a reducing solution B2; wherein the reducing agent concentration in the reducing solution B2 is 0.1-1.0 mol / L; S3, taking 6-10% of the mass of silver nitrate in the oxidation solution A1 in step S1 and dissolving it in deionized water to obtain a synthetic dispersant C1, wherein the amount of deionized water added is 20-50 times the mass of the dispersant; taking 500-800% of the mass of silver acid in the oxidation solution A2 in step S1 and dissolving it in deionized water to obtain a synthetic dispersant C2, wherein the amount of deionized water added is 5-20 times the mass of the dispersant; S4, adding the reducing solution B2 to the control dispersant C2, stirring for 20-40 minutes to obtain a synthetic control liquid precursor, adding the oxidizing solution A2 to the synthetic control liquid precursor, stirring for 5-25 hours, to obtain a synthetic control liquid D; S5. Add synthetic control liquid D containing 20-200% of the mass of silver nitrate in oxidizing solution A1 to oxidizing solution A1, add synthetic dispersant C1 to reducing solution B1, stir for 3-5 minutes respectively, transport oxidizing solution A1 mixed with synthetic control liquid D and reducing solution B1 with synthetic dispersant C1 to reactor respectively, stir for 25-40 minutes, let stand for 10-30 minutes to obtain micro-nano silver powder solution, wash with centrifuge until the conductivity of micro-nano silver powder solution is less than 10μs / cm, dry, and pulverize to obtain micro-nano silver powder with high surface roughness.

2. A method for preparing micro-nano silver powder with controllable nucleation according to step 1, characterized in that: The purity of the silver nitrate used in each step is 99.5-99.9%, and the purity of the reducing agent is 99.0%-99.9%, to ensure accurate control of the amount of material added and the pH value.

3. A method for preparing micro-nano silver powder with controllable nucleation according to step 1, characterized in that: In step S1, the acidic reagent for adjusting the pH value is one or more of nitric acid, acetic acid, carbonic acid, and phenol.

4. A method for preparing micro-nano silver powder with controllable nucleation according to step 1, characterized in that: In step S2, the reducing agent is one or more of ascorbic acid, hydrazine hydrate, glucose, acetone and formaldehyde.

5. The method for preparing a micro-nano silver powder with controllable nucleation according to step 1 is characterized in that: In step S2, the alkaline reagent for adjusting the pH value is one or more of sodium hydroxide, potassium hydroxide, and ammonia water.

6. A method for preparing micro-nano silver powder with controllable nucleation according to step 1, characterized in that: In step S3, the dispersant is one or more of polyvinyl pyrrolidone, gelatin, hexadecyltrimethylammonium bromide, gum arabic, cellulose, polyethylene glycol and polyvinyl alcohol, and the dispersants added to the synthetic dispersant C1 and the control dispersant C2 are the same type of reagents.

7. The method for preparing a micro-nano silver powder with controllable nucleation according to step 1 is characterized in that: In step S4, the stirring rate of the synthesis control liquid D is 100-200 r / min, and the insulation temperature is 20-60°C.

8. The method for preparing a micro-nano silver powder with controllable nucleation according to step 1 is characterized in that: In step S4, the synthesis control liquid D forms nano nucleation sites by slow reaction, and the particle size of the nucleation sites is 30-80 nm. When the silver nitrate content in the oxidation solution A1 is constant, the size of the micro-nano powder can be controlled by controlling the amount of synthesis control liquid D added.

9. The method for preparing a micro-nano silver powder with controllable nucleation according to step 1 is characterized in that: In step S5, a peristaltic pump is used to transport the oxidizing solution A1 mixed with the synthetic control liquid D and the reducing solution B1 added with the synthetic dispersant C1 into the reactor. The flow rate of the peristaltic pump is 11-16L / min, the insulation temperature of the reactor is 25-30°C, and the stirring rate is 300-1000r / min.

10. The method for preparing micro-nano silver powder with controllable nucleation according to step 9 is characterized in that: The diameter of the Y-tube and the peristaltic pump is 5-80 cm, and the discharge rate of the peristaltic pump is 10-30 L / min.

Citation Information

Cited By

  • High-dispersity micro-nano silver powder as well as preparation method and application thereof

    CN119657937A

  • A highly dispersible micro-nano silver powder and its preparation method and application

    CN119657937B