Barrier bag

Through multi-layer functional film structure and longitudinal stretching technology, the problems of high aluminum content and environmental pollution in traditional packaging bags are solved, and high-performance and high-recycling barrier bags are realized, which meet environmental protection and performance requirements.

CN118790613AActive Publication Date: 2024-10-18JIAXING LUCKY MOON PACKAGING MATERIALS CO LTD

Patent Information

Application Number
CN202411276948.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-09-03
Filing Date
2024-09-12
Publication Date
2024-10-18
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

Traditional plastic packaging bags contain high levels of aluminum and are difficult to recycle, commonly used barrier ingredients contain chlorine which is harmful to the environment, and the printed film of polyethylene film does not match the rest of the material, resulting in many challenges in terms of recycling and performance of the packaging bags.

Method used

It adopts a multi-layer functional film structure, including multi-layer co-extruded sub-functional films, which are longitudinally stretched to form an oriented lamellar structure. The weight ratio of polyethylene is greater than or equal to 90%, and is passed through an aluminum plating layer and a heat-sealing film. Improve barrier properties and mechanical properties, reduce aluminum content.

Benefits of technology

It achieves high barrier properties, high strength, high stiffness, high gloss and high temperature resistance, while reducing the aluminum content, promoting the recycling of packaging bags, and meeting environmental protection and performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118790613A_ABST
    Figure CN118790613A_ABST
Patent Text Reader

Abstract

The invention discloses a single-material barrier bag which comprises multiple layers of functional films arranged in a stacked mode in the thickness direction, at least one layer of functional film comprises multiple layers of sub-functional films, the multiple layers of sub-functional films are combined into a whole through multi-layer co-extrusion, and the multiple layers of films are of a lamellar crystal structure arranged in an oriented mode through longitudinal stretching. The weight ratio of polyethylene in the barrier bag is larger than or equal to 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of plastic flexible packaging, in particular to a barrier bag. Background Art

[0002] Traditional aluminum-containing packaging bags mostly use aluminum foil layers and aluminum-plated layers to block oxygen and moisture. The aluminum-plated layer is made by vapor-depositing metal aluminum on the surface of the plastic film, with a thickness of about 300-400 angstroms. However, a high aluminum content is not conducive to the separation and recycling of materials in packaging bags, so reducing aluminum is of great significance for packaging bags. At present, the barrier components added to reduce the aluminum content usually contain chlorine, which is harmful to the environment and toxic, and does not meet environmental protection requirements. On the other hand, the aluminum-plated substrates are mainly polyester film (PET), cast polypropylene film (CPP), and biaxially oriented polypropylene film (BOPP), while the poor adhesion of aluminum plating on polyethylene film (PE) leads to poor fastness after aluminum and PE are compounded, and it cannot be directly applied to the aluminum plating process.

[0003] In addition, the printed film on the surface of the packaging bag is generally PET and oriented polypropylene film (OPP), which is different from the other PE materials in the packaging bag, which is also not conducive to the separation and recycling of the packaging bag. On the other hand, bags made of a single material PE are generally soft and cannot meet the appearance texture and strength requirements of the packaging bag. In addition, the packaging bag needs to be easy to tear when opened, and the contents should not leak easily, while ordinary polyethylene film has poor linear tearing properties.

[0004] Therefore, developing a single-material barrier bag with low aluminum content, high barrier, high light-shielding, high temperature resistance, high printing accuracy, texture, easy to tear horizontally, and recyclable is an urgent problem to be solved in this field. Summary of the invention

[0005] The present invention aims to solve one of the technical problems in the related art to a certain extent. To this end, the present invention provides a barrier bag.

[0006] In order to achieve the above-mentioned purpose, the present invention provides a barrier bag, comprising a multilayer functional film stacked along the thickness direction, at least one layer of the functional film comprises a multilayer sub-functional film, the multilayer sub-functional film is combined into one by multi-layer co-extrusion, the multilayer sub-functional film has an oriented lamellar structure by longitudinal stretching, and the polyethylene weight ratio of the barrier bag is greater than or equal to 90%.

[0007] Furthermore, the components of the sub-functional membrane include polyethylene and copolymers thereof having a molecular chain of at least one length and at least one degree of branching.

[0008] Furthermore, the components of the sub-functional film include at least one of low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, metallocene polyethylene, ethylene-vinyl alcohol polymer, and cycloolefin copolymer.

[0009] Furthermore, the number of layers of the sub-functional films of the functional film is an odd number, and the number of layers of the sub-functional films of the functional film does not exceed 11 layers.

[0010] Furthermore, the multi-layer functional film includes a first barrier film, a second aluminized film and a third heat-sealing film, wherein the first barrier film is located at the outermost layer, the heat-sealing film is located at the innermost layer, and the aluminized film also includes an aluminum layer, which is arranged at the outermost side of the aluminized film and is respectively bonded to the innermost sub-functional film of the first barrier film and the sub-functional film of the aluminized film.

[0011] Further, the first barrier film includes nine layers of sub-functional films; the components of the fifth layer of the first barrier film include ethylene-vinyl alcohol polymer, the components of the fourth and sixth layers of the first barrier film are the same and include polyolefin adhesive resin, the components of the first layer and the eighth layer of the first barrier film are the same and include linear low-density polyethylene, the components of the second, third and seventh layers of the first barrier film are the same and include low-density polyethylene and metallocene polyethylene, and the mass ratio of the low-density polyethylene to the metallocene polyethylene is between 4:1 and 9:1, and the components of the ninth layer of the first barrier film include low-density polyethylene and linear low-density polyethylene, and the mass ratio of the low-density polyethylene to the linear low-density polyethylene is between 2:3 and 1:1.

[0012] Furthermore, the thickness of the first barrier film is between 15um and 35um.

[0013] Furthermore, the first barrier film includes: nine layers of the sub-functional films; the components of the second to seventh sub-functional films of the first barrier film all include low-density polyethylene and metallocene polyethylene in a mass ratio between 4:1 and 9:1, the components of the first sub-functional film and the eighth sub-functional film of the first barrier film are the same and include linear low-density polyethylene, and the components of the ninth sub-functional film of the first barrier film include low-density polyethylene and linear low-density polyethylene and the mass ratio of the low-density polyethylene and the linear low-density polyethylene is between 2:3 and 1:1.

[0014] Furthermore, the aluminized film includes: nine layers of the sub-functional films and an aluminized layer; the first to ninth sub-functional films of the aluminized film have the same components and include high-density polyethylene, the thickness of the aluminized film is between 25um and 70um, and the thickness of the aluminized layer is between 2.9 angstroms and 3.5 angstroms.

[0015] Furthermore, the heat-sealing film comprises: nine layers of the sub-functional films; components of the first to eighth layers of the sub-functional films of the heat-sealing film comprise linear low-density polyethylene and cyclic olefin copolymer, and the mass ratio of the low-density polyethylene to the cyclic olefin copolymer is between 7:3 and 9:1; components of the ninth layer of the sub-functional film of the heat-sealing film comprise low-density polyethylene and linear low-density polyethylene, and the mass ratio of the low-density polyethylene to the linear low-density polyethylene is between 4:1 and 9:1; and the thickness of the heat-sealing film is between 30um and 60um.

[0016] The barrier bag of the present invention has the following beneficial effects: The barrier bag of the present invention has a multi-layer functional film, and the functional film includes a multi-layer sub-functional film. Compared with the barrier bag of ordinary single-layer functional film, the setting of the multi-layer sub-functional film provides more layers, and each layer of sub-functional film can have different properties. The multi-layer sub-functional film is co-extruded to obtain the functional film, and the different properties of the functional film are enhanced, so that the functional film has better comprehensive performance (higher barrier properties, higher mechanical properties such as strength, stiffness and toughness, better gloss, higher temperature resistance, etc.), which broadens the scope of application projects of barrier bags and solves challenging industrial problems. The components of the multi-layer sub-functional film can also be the same, thereby improving the compatibility between the functional film layers.

[0017] In addition, each layer of sub-functional film has an oriented lamellar structure through longitudinal stretching, and the composed functional film also has a higher orientation, which further improves the overall strength, stiffness, glossiness, barrier properties and heat resistance of the barrier bag.

[0018] On the other hand, the components of each layer of the functional film of the barrier bag of the present invention include polyethylene, and the weight ratio of polyethylene exceeds 90%. It is a barrier bag with a single material, and therefore can be recycled and reused at a lower cost and with higher efficiency.

[0019] In summary, the barrier bag of the present invention adopts the above-mentioned components and structures to replace aluminum foil and conventional thickness aluminum-plated layers to play the role of oxygen and moisture barrier, reduce the thickness of the aluminum-plated layer, greatly reduce the aluminum content, and is more conducive to recycling. In addition, various performances are further improved, and it has high barrier properties, high strength, high stiffness, high gloss, high temperature resistance and the like.

[0020] These features and advantages of the present invention will be disclosed in detail in the following specific embodiments and drawings. The best embodiments or means of the present invention will be described in detail in conjunction with the drawings, but they are not intended to limit the technical solutions of the present invention. In addition, there are multiple features, elements, and components that appear in each of the following texts and drawings, and different symbols or numbers are marked for convenience, but they all represent components with the same or similar structures or functions. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The present invention will be further described below in conjunction with the accompanying drawings: Figure 1 A schematic structural diagram of an implementation mode of a barrier bag provided by the present invention; Figure 2 is a structural schematic diagram of an embodiment of the first barrier film provided by the present invention; Figure 3 It is a structural schematic diagram of an implementation mode of the aluminum-plated film provided by the present invention; Figure 4 It is a structural schematic diagram of an implementation mode of the heat-sealing film provided by the present invention; Figure 5 is a schematic structural diagram of another embodiment of the first barrier film provided by the present invention; Figure 6 A schematic structural diagram of another embodiment of a barrier bag provided by the present invention; Figure 7 It is a flow chart of an implementation method of the barrier bag manufacturing method provided by the present invention.

[0022] Description of Reference Numerals 1: Barrier bag 11: First barrier film 12: Aluminized film 13: Heat sealing film 110: EVOH barrier layer 111: outer barrier layer 112: First composite layer 113: Second barrier layer 114: Adhesive layer 120: Aluminum coating 121: Aluminum substrate 130: easy-tear heat-sealing layer 131: first easy-tear layer DETAILED DESCRIPTION Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments in the implementation manner are intended to be used to explain the present invention and should not be construed as limiting the present invention.

[0023] References to "one embodiment" or "example" or "example" in this specification mean that a particular feature, structure, or characteristic described in conjunction with the embodiment itself may be included in at least one embodiment disclosed herein. The appearance of the phrase "in one embodiment" in various places in the specification does not necessarily refer to the same embodiment.

[0024] It should be pointed out that in the present invention, the "inner side" refers to the side of the packaging bag close to the packaged article, and the "outer side" refers to the side away from the packaged article.

[0025] According to the "Circular Economy Design Guidelines" of the European Flexible Packaging Circular Economy Organization (CEFLEX), the single material of flexible packaging mainly refers to a single polyolefin material, such as a single polypropylene (PP) or a single polyethylene (PE) material with a weight ratio exceeding 90%. Other barrier components such as silicon oxide, aluminum oxide, aluminum plating, ethylene-vinyl alcohol polymer, etc. are allowed to contain a maximum of 5% by weight.

[0026] The present invention provides a barrier bag, comprising a multilayer functional film stacked along the thickness direction, at least one layer of the functional film comprises a multilayer sub-functional film, the multilayer sub-functional film is combined into one by multi-layer co-extrusion, the multilayer sub-functional film has an oriented lamellar structure by longitudinal stretching, and the polyethylene weight ratio of the barrier bag is greater than or equal to 90%.

[0027] Compared with ordinary single-layer functional film barrier bags, the setting of multi-layer sub-functional films provides more layers, and each layer of sub-functional films has different properties. The multi-layer sub-functional films are co-extruded and combined into one functional film, which can enhance the different properties of the functional film, so that the functional film has better comprehensive performance (higher barrier properties, higher mechanical properties such as strength, stiffness and toughness, better gloss, higher temperature resistance, etc.), broadens the scope of application projects of barrier bags, and solves challenging industrial problems. The performance of multi-layer sub-functional films can also be the same, thereby improving the overall compatibility of the functional film and enhancing a certain specific function of the barrier bag.

[0028] The components of the multilayer sub-functional membrane include polyethylene and its copolymers having molecular chains of multiple lengths with multiple degrees of branching. Preferably, the components of the sub-functional membrane include at least one of low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, metallocene polyethylene, ethylene-vinyl alcohol polymer, and cycloolefin copolymer.

[0029] In addition, each layer of sub-functional film has an oriented lamellar structure through longitudinal stretching, and the composed functional film also has a higher orientation, which further improves the overall strength, stiffness, glossiness, barrier properties and heat resistance of the barrier bag. The components of each layer of functional film of the barrier bag of the present invention include polyethylene, and the weight ratio of polyethylene exceeds 90%. It is a barrier bag with a single material, and therefore can be recycled and reused at a lower cost and with higher efficiency.

[0030] The barrier bag using the structure and components of the present invention can replace the aluminum foil or aluminum-plated layer in the prior art to play the role of oxygen and moisture barrier, greatly reducing the aluminum content, being more conducive to recycling, and further improving various performances, with high barrier properties, high strength, high stiffness, high gloss, high temperature resistance and the like.

[0031] The present invention does not impose any special limitation on the number of layers of the sub-functional film, as long as the number of layers of the sub-functional film of the functional film is an odd number and the number of layers of the sub-functional film of the functional film does not exceed 11. Preferably, the functional film of the present invention can be one or more combinations of one sub-functional film, three sub-functional film, five sub-functional film, seven sub-functional film, nine sub-functional film and eleven sub-functional film.

[0032] In some embodiments, the barrier bag is a three-layer functional film stacked from the outside to the inside, wherein the outer functional film includes five co-extruded sub-functional films, the middle functional film includes a functional film prepared by casting, and the inner functional film includes seven co-extruded sub-functional films, and the functional films all have an oriented lamellar structure through longitudinal stretching.

[0033] In some embodiments, the barrier bag is a two-layer functional film stacked from the outside to the inside, wherein the outer functional film includes three layers of co-extruded sub-functional film, and the inner functional film includes nine layers of co-extruded sub-functional film, and both functional films have an oriented lamellar structure through longitudinal stretching.

[0034] In some embodiments, the barrier bag is a three-layer functional film stacked from the outside to the inside, wherein the outer functional film includes nine co-extruded sub-functional films, the middle functional film includes nine co-extruded sub-functional films, and the inner functional film includes nine co-extruded sub-functional films, and the three functional films all have an oriented lamellar structure through longitudinal stretching.

[0035] In some embodiments, the multilayer sub-functional film in the functional film also has multiple thicknesses. For high-barrier multilayer co-extruded composite films, the film thickness and uniformity have a significant impact on the film quality. The thickness of the produced sub-functional film depends on the extrusion amount, the pulling speed, and the film width. The thickness of the sub-functional film is controlled by controlling the corresponding component extrusion amount, the pulling speed, and the width of the film. The thickness of the sub-functional film is not specifically limited to the thickness of the multilayer sub-functional film in the present invention, and it only needs to meet the thickness range of the conventional co-extruded film. The thickness can represent the degree of enhanced performance. For example, in order to improve the strength of the barrier bag, in the film after nine layers of co-extrusion and longitudinal stretching, a high-strength polyethylene component is added to the extruder in the preparation stage, its content is increased, and the same high-strength polyethylene component is added to the adjacent extruder. The above method can increase the thickness of the sub-functional film with high-strength function, so that the sub-functional film with greater thickness and high strength can improve the overall strength of the film to a greater extent. In order to improve other properties, the thickness of the corresponding sub-functional film can also be increased.

[0036] In some embodiments, Figure 1As shown, the multi-layer functional film of the barrier bag 1 includes a first barrier film 11, an aluminized film 12 and a heat-sealing film 13. The first barrier film 11 is located at the outermost layer, the heat-sealing film 13 is located at the innermost layer, the aluminized film 12 also includes an aluminized layer 120, and the aluminized layer 120 is arranged on the outermost side of the aluminized film 12 and is respectively bonded to the sub-functional film of the first barrier film and the sub-functional film of the aluminized film, and the outermost surface of the heat-sealing film 13 is bonded to the innermost surface of the aluminized film 12.

[0037] In the present invention, the addition of the aluminum coating layer 120 enables the barrier bag to have good barrier properties for blocking light, oxygen and water vapor, and the aluminum coating layer includes aluminum. However, the components and structure of the barrier bag of the present invention already have high barrier properties, and can completely replace the conventional aluminum coating layer in the art to play a barrier role. Therefore, the thickness of the aluminum coating layer provided in the present invention can be much smaller than the thickness of the conventional aluminum coating layer in the art. As an optional embodiment, the thickness of the aluminum coating layer of the present invention is between 2.9 angstroms and 3.5 angstroms.

[0038] In some embodiments, the sub-functional film of the aluminum-plated film is also called an aluminum-plated substrate, such as Figure 3 As shown, the present invention does not impose any special restrictions on the aluminum-plated substrate 121 of the aluminum-plated film 12, and it only needs to be a single material of polyethylene, and be able to fit with the aluminum-plated layer 120, and meet the standards specified in the application. The aluminum-plated layer 120 is arranged on the outermost surface of the aluminum-plated substrate 121, so the outermost surface of the aluminum-plated substrate 121 requires a higher aluminum adhesion. The higher aluminum adhesion requires that the aluminum-plated substrate 121 needs to be high-strength, hard and not easy to deform, so that the aluminum-plated layer 120 is plated on the surface of the aluminum-plated substrate 121 more completely during vacuum aluminum plating, and is not easy to fall off. This requires that the aluminum-plated substrate 121 of the aluminum-plated film needs a certain stiffness to meet the overall strength and hardness of the aluminum-plated film 12.

[0039] Preferably, the components of the aluminum-plated substrate 121 of the aluminum-plated film 12 include high-density polyethylene (HDPE). HDPE has the characteristics of low branching, very short molecular chains as branches, and tightly arranged molecular structure, and a degree of crystallization higher than 90%, so that the sub-functional film prepared by co-extrusion and longitudinal stretching of the components has good stiffness and water vapor barrier properties, and the stiff film surface is more conducive to aluminum plating. Furthermore, the surface of the aluminum-plated substrate 121 formed by co-extrusion blow molding and longitudinal stretching of multiple layers of HDPE can be corona treated to increase the surface roughness, so that the aluminum-plated layer 120 can be well attached to the surface of the aluminum-plated substrate 121 during subsequent aluminum plating, thereby increasing the adhesion of the aluminum plating on the surface of the aluminum-plated substrate 121, making the aluminum-plated layer 120 more firmly bonded to the aluminum-plated substrate 121, and compensating for the shortcoming of the weak bonding force of the aluminum plating of the PE film causing the barrier property to decrease.

[0040] The innermost sub-functional film of the first barrier film is laminated with the aluminum coating layer. Preferably, the two films are laminated with an adhesive. Furthermore, in order to increase the composite strength between the two films, Figure 1 and Figure 2 As shown, the surface of the first composite layer 112 of the first barrier film may be subjected to corona treatment to increase the surface roughness, thereby improving the adhesion of the first composite layer 112 to the aluminum-plated layer 120 and facilitating printing processing.

[0041] The present invention does not specifically limit the components of the first barrier film, but only needs to satisfy the requirement that the components are a single polyethylene material, can be attached to the surface of the aluminum-plated layer, and meet the standards specified in the application. Preferably, the components of the first barrier film include low-density polyethylene (LDPE), metallocene polyethylene (MPE) and linear low-density polyethylene (LLDPE).

[0042] In some embodiments, the sub-functional film of the first barrier film can also be used as a printing layer for printing patterns. The present invention does not impose any special restrictions on the specific position of the printing layer. It only needs to be able to print patterns and the printed patterns meet the specified application standards. Preferably, the innermost sub-functional film of the first barrier film is used for printing patterns. The present invention does not impose any special restrictions on the components of the printing layer. Preferably, the components of the printing layer include at least one of low-density polyethylene, metallocene polyethylene and linear low-density polyethylene.

[0043] Traditional PE films are easily stretched and deformed during high-speed printing, resulting in poor printing effects and low printing precision. Due to the problem of film elongation, the printing speed needs to be reduced by at least 30% to 40%. The first barrier film of the present invention is formed by co-extrusion of multiple sub-functional films and longitudinal stretching (MDO), and has the characteristics of high strength, high stiffness, not easy to deform, and high temperature resistance. The structure and components of the printing layer in the first barrier film provide the film with rigidity to withstand the elongation during high-speed printing, so good printing effects can be obtained without reducing the printing speed, thereby improving printing efficiency.

[0044] In addition, the LLDPE component added to the first barrier film has a linear main chain with short and uniform branches, and these short branches can slide against each other when stretched. Therefore, the film obtained by co-extrusion and longitudinal stretching of the LLDPE component is very flexible and has excellent thermal stability and dimensional stability. During the printing process, it has high impact strength and high rigidity to prevent the film from excessive elongation and deformation during printing, thereby having better printing accuracy and printing effect, and high rigidity can provide a part of the hardness texture for the barrier bag. At the same time, the above film has excellent chemical resistance in a wide temperature range and can be printed with printing inks of different components; heat resistance, melting point and softening point are also among the best categories in plastic films, making the film surface more resistant to high temperatures and non-sticky to hot knives. In addition, the film of the above components also has high ink adhesion, thereby achieving an ideal printing effect. The printing process is preferably, but not limited to, gravure printing, flexographic printing and offset printing.

[0045] Low-density polyethylene (LDPE) has a large number of short and long chain branches. The hardness and strength of the film obtained by co-extrusion and longitudinal stretching of LDPE components are reduced, but the plasticity is good. As a sub-functional film, it can provide higher plasticity for the functional film as a whole. High transparency can also provide higher gloss for the functional film as a whole. It has a lower melting point and good fluidity, so it has a lower heat sealing temperature and heat sealing bonding strength than other PE materials. Compared with traditional polyethylene, metallocene polyethylene (MPE) has a larger molecular weight and denser distribution than traditional polyethylene, so it has better impact strength and greater elongation at break, but at the same time, MPE has good transparency and low haze.

[0046] The first barrier film with the above components is longitudinally stretched after multi-layer co-extrusion, and has higher gloss and transparency, making it more beautiful. After longitudinal stretching, the tensile strength of the first barrier film in the transverse and longitudinal directions is greatly improved, thereby increasing the overall strength of the barrier bag, while also having certain barrier properties.

[0047] In other embodiments, the components of the first barrier film also include ethylene-vinyl alcohol polymer (EVOH). The addition of EVOH can further improve the oxygen and moisture barrier properties of the film. The film obtained by co-extrusion and longitudinal stretching of the EVOH component can significantly improve the overall oxygen and moisture barrier properties of the barrier bag, thereby replacing the thicker aluminum coating in the field to play the role of oxygen and moisture barrier, further reducing the aluminum content of the barrier bag, and the aluminum coating of the barrier bag can be thinner to achieve the effect of reducing aluminum, which is more conducive to the separation and recycling of the barrier bag. At the same time, EVOH is harmless to the environment and is conducive to the development of a circular economy. In some embodiments, the thickness of the aluminum coating is between 2.9 angstroms and 3.5 angstroms. Compared with the traditional aluminum coating thickness of 300A to 400A, the barrier bag of the present invention greatly reduces the thickness of the aluminum coating.

[0048] like Figure 1 and Figure 2 As shown, the present invention does not impose any special restrictions on the location of the EVOH barrier layer 110, as long as it can play a barrier role, fit with other sub-functional films and will not cause the first barrier film to curl. As an optional embodiment, in order to improve the combination of the EVOH barrier layer 110 with other sub-functional films and avoid the curling of the first barrier film, the EVOH barrier layer 110 is arranged in the middle of the first barrier film 11, and is connected to the adjacent sub-barrier layers 113 on both sides through the adhesive layer 114. Preferably, the adhesive layer 114 is selected from polyethylene adhesive resin, and the EVOH barrier layer 110 is used as the middle layer. The adhesive layers 114 on the adjacent two sides are symmetrical structures with the same components, the same proportions, the same thickness and symmetrical positions. The sub-barrier layers 113 on the adjacent two sides are structures with the same components, the same proportions and the same thickness. The outer barrier layers 111 on the adjacent two sides are structures with the same components, the same proportions and the same thickness, so that the EVOH barrier layer can be subjected to the same force on both sides, solving the curling problem of the first barrier film.

[0049] The present invention does not specifically limit the components of the heat-sealing film, but only needs to satisfy the requirement that the components are a single polyethylene material, have a certain heat-sealing effect and a transverse tearing effect, and meet the standards specified in the application. Preferably, the components of the heat-sealing film include linear low-density polyethylene (LLDPE), cyclic olefins, and low-density polyethylene (LDPE).

[0050] It is difficult to tear polyethylene packaging bags into straight lines, that is, the tear orientation is poor. Figure 1 and Figure 4 As shown, the present invention prepares the first tearable layer 131 by co-extrusion and longitudinal stretching of LLDPE and cycloolefin components. The longitudinal stretching makes the structure of the first tearable layer 131 have great orientation in the longitudinal direction. When the multi-layer functional film is compounded to obtain a barrier bag, the bag making method is horizontal bag making, and the tearing direction is consistent with the film material direction, both in the longitudinal direction, so it can be easily torn along the shear direction under the effect of tearing. At the same time, LLDPE is a short and evenly branched linear main chain, so that the barrier bag has no obvious tensile resistance caused by obvious lateral complex branching, so it forms the characteristic of transverse tearing. The first tearable layer 131 is co-extruded and longitudinally stretched. The cycloolefin component that is easy to tear is added to the bottom film, that is, a tearing failure point is introduced into the first tearable layer 131. Under the action of external force, the tearing failure point is torn first, and then other non-tearable parts are driven, and then the tearing effect is expanded to the entire barrier bag, so that the barrier bag has transverse tearing property and enhances the convenience of use.

[0051] The heat-sealing film further includes an easy-tear heat-sealing layer 130. The component of the easy-tear heat-sealing layer 130 is preferably, but not limited to, LDPE. LDPE has a low melting point, so the easy-tear heat-sealing layer 130 made of LDPE has a low melting point and heat-sealing temperature in the barrier bag of the present invention. In the process of heat-sealing the barrier bag, the easy-tear heat-sealing layer 130 is preferentially melted to form a molten body with fluidity and viscosity, and the molten body is pressed with the easy-tear heat-sealing layer 130 of the adjacent barrier bag to form a sealed barrier bag. The component of the easy-tear heat-sealing layer 130 may also include LLDPE.

[0052] The present invention does not impose any special restrictions on the positions of the first easy-tear layer 131 and the easy-tear heat-sealing layer 130, and it is only necessary that the easy-tear heat-sealing layer 130 is on the outside of the heat-sealing film 13 and is combined with the easy-tear heat-sealing layer 130 of other heat-sealing films 13 by heat sealing. Preferably, the easy-tear heat-sealing layer 130 is arranged on the innermost side of the heat-sealing film 13, and the first easy-tear layer 131 is arranged on the outside of the heat-sealing film 13 and is attached to the aluminized film 12.

[0053] The heat-sealing film of the present invention also has the advantages of excellent environmental stress crack resistance, low sealing temperature, high heat-sealing strength and high stiffness.

[0054] The present invention does not specifically limit the number of sub-functional film layers included in the functional film, as long as the corresponding functions are met. Preferably, the first barrier film, the aluminized film and the heat-sealing film each include nine layers of sub-functional films, and the nine layers of sub-functional films include the first layer to the ninth layer stacked from the outside to the inside.

[0055] The present invention does not impose any special restrictions on the number of layers and composition ratio of the first barrier film. Preferably, Figure 2 As shown, the first barrier film includes nine layers of sub-functional films. Specifically, the first barrier film includes: a first layer; a second layer; a third layer; a fourth layer; a fifth layer; a sixth layer; a seventh layer; an eighth layer; a ninth layer; The fifth layer is an EVOH barrier layer 110, the components of which include ethylene-vinyl alcohol polymer. Preferably, the fifth layer includes 100 wt% of ethylene-vinyl alcohol polymer. The fourth layer and the sixth layer are adhesive layers 114, which have the same composition and include polyolefin adhesive resin. The adhesive layer 114 is used to bond the EVOH barrier layer 110 to the adjacent sub-functional film to improve the bonding force and prevent the film from curling due to poor interlayer compatibility. The first layer and the eighth layer are outer barrier layers 111, having the same composition and comprising linear low-density polyethylene, preferably comprising 100 wt% linear low-density polyethylene; The second layer, the third layer and the seventh layer are secondary barrier layers 113, which have the same composition and include low-density polyethylene and metallocene polyethylene, and the mass ratio of LDPE to MPE is between 4:1 and 9:1; The ninth layer is the first composite layer 112, and its components include low-density polyethylene and linear low-density polyethylene, and the mass ratio of the low-density polyethylene to the linear low-density polyethylene is between 2:3 and 1:1.

[0056] Preferably, the oxygen permeability of the first barrier film is 0.9 cm 3 / m 2 day to 2.0cm 3 / m 2 ·Day, moisture permeability is 3.0g / m 2 ·Daily up to 5.0g / m 2 ·day, the thickness of the first barrier film is between 15um and 35um.

[0057] In other embodiments, Figure 5 As shown, the first barrier film includes nine layers of sub-functional films. Specifically, the first barrier film includes: a first layer; a second layer; a third layer; a fourth layer; a fifth layer; a sixth layer; a seventh layer; an eighth layer; a ninth layer; The second to seventh layers are secondary barrier layers 113, and the components thereof include low-density polyethylene and metallocene polyethylene in a mass ratio of 4:1 to 9:1; The first layer and the eighth layer are outer barrier layers 111, having the same composition and comprising linear low-density polyethylene, preferably comprising 100 wt% linear low-density polyethylene; The ninth layer is the first composite layer 112, and its components include low-density polyethylene and linear low-density polyethylene, and the mass ratio of the low-density polyethylene to the linear low-density polyethylene is between 2:3 and 1:1.

[0058] In some embodiments, Figure 4 As shown, the heat-sealing film includes nine layers of sub-functional films, specifically, the heat-sealing film includes: the first layer; the second layer; the third layer; the fourth layer; the fifth layer; the sixth layer; the seventh layer; the eighth layer; the ninth layer; wherein the components of the first to eighth layers include linear low-density polyethylene and cyclic olefin copolymer, and the mass ratio of the linear low-density polyethylene to the cyclic olefin copolymer is between 7:3 and 9:1, and the components of the ninth layer include low-density polyethylene and linear low-density polyethylene, and the mass ratio of the low-density polyethylene to the linear low-density polyethylene is between 4:1 and 9:1. The thickness of the heat-sealing film is between 30um and 60um.

[0059] In some embodiments, Figure 3As shown, the aluminized film includes nine layers of sub-functional films and an aluminized layer. Specifically, the aluminized film 12 includes an aluminized substrate 121 and an aluminized layer 120. The aluminized substrate 121 includes: a first layer; a second layer; a third layer; a fourth layer; a fifth layer; a sixth layer; a seventh layer; an eighth layer; and a ninth layer. The first to ninth layers have the same components and include high-density polyethylene, preferably 100 wt% high-density polyethylene. The overall oxygen permeability of the aluminized film is 8.0 cm 3 / m 2 day to 15.0cm 3 / m 2 ·Day, moisture permeability is 1.0g / m 2 ·Daily up to 2.0 g / m 2 · day, the overall thickness of the aluminum coating is between 25um and 70um, and the thickness of the aluminum coating is between 2.9 angstroms and 3.5 angstroms.

[0060] As a preference, Figure 1 and Figure 6 As shown, the first barrier film, aluminized film and heat-sealing film having nine layers of sub-functional films and corresponding components are compounded to form a bag to obtain a barrier bag. Figure 1 It is a high barrier bag with EVOH component. Figure 6 The barrier bag without EVOH component is a barrier bag with EVOH component added, and the barrier bag with EVOH component added has higher oxygen and moisture barrier properties than the barrier bag without EVOH added. The overall structure enables the barrier bag to have high barrier properties with oxygen and moisture barrier less than or equal to 0.5, high light blocking property, high temperature resistance and higher strength. Different components can be added according to the actual use scenario to meet different performance requirements.

[0061] The first barrier film and the aluminized film are compounded by an adhesive, and the aluminized film and the heat-sealing film are compounded by an adhesive. The present invention does not specifically limit the components of the adhesive, and the adhesive is not limited to commercially available glues such as polyurethane composite glue and polyethylene adhesive resin. The adhesive used in the present invention may further contain tackifying resins, plasticizers, drying delay agents, defoamers, thickeners, waxes, preservatives, colorants, etc. as needed. Preferably, the compounding method is solvent-free compounding, and the compounding method without solvent is more environmentally friendly. In addition, in order to improve the composite strength, the functional film is corona treated on the surface of the composite to make the surface rougher and improve the composite strength. Preferably, the corona value is between 38 dynes and 42 dynes. The functional film subjected to corona treatment includes: the surface of the innermost sub-functional film of the first barrier film and the surface of the outermost sub-functional film of the heat-sealing film.

[0062] The present invention does not specifically limit the application of barrier bags. Customized barrier bags can be made according to actual performance requirements. Functional films with different performances can be made by adjusting the component ratio, the number of layers, structure, position, thickness and other parameters of the multi-layer sub-functional film. Functional films with different performances are combined into barrier bags with different functions, so as to be applied in different scenarios. As some optional embodiments, the barrier bag of the present invention can be a facial mask bag, a food packaging bag, a coffee bag, a milk powder packaging bag, a medicine packaging bag, a retortable bag, a shopping bag, etc.

[0063] like Figure 7 As shown, as an embodiment of the method for making a barrier bag of the present invention, the specific steps include: In step S100, EVOH, LDPE, MPE and LLDPE in a first set ratio are added to a multilayer co-extruder, blown into a plastic film, and then longitudinally stretched to obtain a first barrier film; In step S200, after adding the second set ratio of HDPE into a multi-layer co-extruder, blow-molding to form a plastic film, the film is longitudinally stretched to obtain an aluminum-plated substrate; In step S300, the aluminum-plated substrate is aluminum-plated to obtain an aluminum-plated film; In step S400, after adding LLDPE, cycloolefin and LDPE in a third set ratio into a multilayer co-extruder, blow-molding to form a plastic film, the film is longitudinally stretched to obtain a heat-sealed film; In step S500, the first barrier film, the aluminized film and the heat-sealing film are compounded to obtain the above-mentioned barrier bag.

[0064] The barrier bag produced by the above-mentioned manufacturing method is the barrier bag provided in the first aspect of the present disclosure.

[0065] The film produced by multi-layer co-extrusion has multiple layers of sub-functional films, and the formula can be more flexible and varied. The component combination of each layer of sub-functional film makes each layer of sub-functional film have different properties, thereby enhancing the different properties of the overall functional film, making the functional film have better comprehensive performance (higher barrier properties, higher mechanical properties such as strength, stiffness and toughness, better gloss, higher temperature resistance, etc.), broadening the scope of application engineering of barrier bags and solving challenging industrial problems.

[0066] In addition, the film formed by multi-layer co-extrusion is also stretched longitudinally to increase the film's orientation in the longitudinal direction, thereby improving the film's stiffness, optics, and barrier properties. The MDO stretching equipment is completed by multiple rolls through four stages: preheating, stretching, annealing, and cooling.

[0067] The weight ratio of polyethylene, a raw material component, used in the present invention exceeds 90%. By adopting the production method of the present invention, this barrier bag made of a single material can replace thick aluminum to play the role of oxygen and moisture barrier, greatly reducing the aluminum content, and is more conducive to recycling. Compared with conventional polyethylene packaging bags, various performances are further improved, and the bag has high barrier properties, high strength, high stiffness, high gloss, high temperature resistance and the like.

[0068] In step S100, preferably, the longitudinal stretching multiple of the first barrier film is between 5 and 5.5. The present invention does not specifically limit other methods for making the first barrier film. For example, in order to increase the composite strength between the first barrier film and the adjacent functional film, the surface of the first barrier film may be subjected to corona treatment to increase the surface roughness. For another example, a pattern may be printed on the inner surface of the first barrier film in order to print a logo.

[0069] In step S200, preferably, the longitudinal stretching multiple of the aluminum-plated substrate is between 1 and 1.5. The present invention does not specifically limit other methods for making the aluminum-plated substrate. For example, the surface of the aluminum-plated substrate can also be subjected to corona treatment to increase the surface roughness so that the aluminum layer can fit well on the surface during subsequent aluminum plating, thereby increasing the adhesion of the aluminum plating on the surface of the aluminum-plated substrate and making the aluminum-plated layer more firmly bonded to the surface of the aluminum-plated substrate, thereby compensating for the shortcoming of reduced barrier properties caused by weak bonding strength of the aluminum plating of the PE film.

[0070] In step S300, the present invention does not specifically limit the aluminum plating method, and it is only necessary to set the aluminum plating layer on the surface of the aluminum plating substrate in step S200 and adhere to the surface of the aluminum plating substrate. For example, a vacuum sputtering aluminum plating method can be used.

[0071] In step S400, preferably, the longitudinal stretching ratio of the heat-sealing film is between 1 and 1.5 times.

[0072] In step S500, the first barrier film, the aluminized film and the heat-sealing film are compounded, including: compounding the first barrier film, the aluminized film and the heat-sealing film with an adhesive. The present invention does not specifically limit the compounding method. For example, a dry compounding method can be used to apply an adhesive (glue) on a plastic film, and then evaporate the excess solvent through a drying oven, and then use a hot pressing roller to press it together with another plastic film or an aluminized layer. For another example, a wet compounding method can be used to apply an adhesive (glue) on a plastic film or an aluminized layer, press it with other plastic films or aluminized layers, and then dry it through a drying oven. For another example, a solvent-free compounding method can be used to press a plastic film with a pre-coated hot melt adhesive layer with another layer of plastic film through a hot roller.

[0073] The present invention will be further described below with reference to the embodiments.

[0074] Example Example 1 The first barrier film is prepared, and the specific steps include: The feeding machine grabs the raw materials of corresponding components according to the set ratio and adds them into the co-extruder. The components and set ratios used in each layer are as follows: the first layer: 100% linear low-density polyethylene; the second layer: 80% low-density polyethylene and 20% metallocene polyethylene; the third layer: 80% low-density polyethylene and 20% metallocene polyethylene; the fourth layer: 100% polyolefin adhesive resin; the fifth layer: 100% vinyl alcohol-ethylene copolymer; the sixth layer: 100% polyolefin adhesive resin; the seventh layer: 80 low-density polyethylene and 20% metallocene polyethylene; the eighth layer: 100% linear low-density polyethylene; the ninth layer: 40% low-density polyethylene and 60% linear low-density polyethylene; The extruder melts and plasticizes the raw materials in the above proportions in sequence and then feeds them into a die head for extrusion blow molding to form a film, thereby obtaining a primary barrier film with a nine-layer co-extrusion structure; The primary barrier film is longitudinally stretched at a stretching ratio of 5 to obtain a first barrier film, wherein the thickness ratio of the first barrier film from the first layer to the ninth layer is 2:1:2:1:2:2:3:2:4; The aluminum-plated film is prepared, and the specific steps include: The aluminized film is prepared by the same method as the first barrier film, except that the raw material and the ratio of 100% high-density polyethylene are added to the nine-layer co-extruder, and the extruder melts and plasticizes the raw materials in the above ratio in sequence and then feeds them into the die head for extrusion and blow molding to obtain the first aluminized substrate; The first aluminum-plated substrate is longitudinally stretched, and the stretching ratio is set to 1 to obtain an aluminum-plated substrate, wherein the thickness ratio of the aluminum-plated substrate from the first layer to the ninth layer is 2:1:2:1:2:2:3:2:4; Vacuum-plating an aluminum substrate to obtain an aluminum-plated film; The heat-sealing film is prepared, and the specific steps include: The heat-sealing film is prepared by the same method as the first barrier film, except that the raw materials and proportions used in each layer are as follows: the first to eighth layers are all 70% linear low-density polyethylene and 30% cycloolefin; the ninth layer: 80% low-density polyethylene and 20% linear low-density polyethylene, and the extruder melts and plasticizes the raw materials in the above proportions in sequence and then feeds them into the die head for extrusion blow molding to form a film, thereby obtaining a first heat-sealing film with a nine-layer co-extrusion structure; The first heat-sealing film is longitudinally stretched at a stretching ratio of 1 to obtain a heat-sealing film, wherein the thickness ratio of the heat-sealing film from the first layer to the ninth layer is 2:1:2:1:2:2:3:2:4; The first barrier film, the aluminized film and the heat-sealing film are compounded with glue to form a barrier bag 1 without solvent.

[0075] Example 2 A barrier bag 2 was prepared by using the same materials and preparation method as in Example 1, except that the first barrier film was stretched to 5.5 times and the aluminized film was stretched to 1.5 times, to obtain a barrier bag 2.

[0076] Example 3 A barrier bag was prepared using the same materials and preparation method as in Example 1, except that the raw materials and proportions of the extruders for the fourth, fifth and sixth layers of the first barrier film were 80% low-density polyethylene and 20% metallocene polyethylene, to obtain barrier bag 3.

[0077] Example 4 A barrier bag 4 was prepared by using the same materials and preparation method as in Example 3, except that the first barrier film was stretched to 5.5 times and the aluminized film was stretched to 1.5 times, to obtain a barrier bag 4.

[0078] Comparative Example 1 The components and structure of the present invention are not adopted, and it is a common barrier bag popular in the market. The specific structure includes: KOPP / / NY / / CPE, which is a three-layer composite, wherein KOPP is a coating film of polyvinylidene chloride coated on a biaxially oriented polypropylene film as a substrate, NY is a nylon filter membrane, and CPE is a chlorinated polyethylene film. The barrier bag is a commonly used commercially circulated material structure.

[0079] Test Case A set of test items were performed on the barrier bags of the embodiments and the barrier bags of the comparative examples. The specific test items are shown in Table 1. The specific results of the embodiments and the comparative examples are shown in Table 1.

[0080] The EVOH material of the present invention is used in Examples 1 and 2, which can further improve the oxygen and moisture barrier properties of the barrier bag and also improve the longitudinal tensile strength of the film. However, Examples 3 and 4 and the comparative example do not use the EVOH material of the present invention, so the corresponding oxygen and moisture barrier properties are both lower than those of Examples 1 and 2.

[0081] Example 1 uses a printed film stretched 5 times in the longitudinal direction, adds 100% vinyl alcohol-ethylene copolymer to the middle layer of the printed film, and uses an aluminized film stretched 1 times in the longitudinal direction. The performance of the prepared barrier bag meets the standard requirements, and the oxygen permeability is 1.5cc / m 2 *day, moisture permeability is 1.6 g / m 2 *day, heat seal strength (top seal) is 3.7kgf / 15mm, heat seal strength (bottom seal) is 3.5kgf / 15mm, tensile strength MD direction is 4.6 kgf / 15mm, TD direction is 3.4 kgf / 15mm, thickness is 108um, weight is 104g / m 2, the rest of the test performances are within the qualified range.

[0082] Compared with Example 1, Example 2 increases the stretching multiples of the first barrier film and the aluminized film. The stretching multiples of the first barrier film are increased from 5 times to 5.5 times, and the stretching multiples of the aluminized film are increased from 1 times to 1.5 times. The heat sealing strength and tensile strength of the prepared barrier bag are significantly improved compared with Example 1, and the oxygen permeability is 0.8 cc / m 2 *day, moisture permeability is 0.9 g / m 2 *day, heat seal strength (top seal) is 4.6kgf / 15mm, heat seal strength (bottom seal) is 4.9kgf / 15mm, tensile strength MD direction is 6.5kgf / 15mm, TD direction is 5.2 kgf / 15mm, thickness is 108um, weight is 104g / m 2 , the rest of the test performances are within the qualified range.

[0083] Example 3 does not add vinyl alcohol-ethylene copolymer. The stretching ratio is the same as that of Example 1. The oxygen barrier performance is significantly reduced, the moisture barrier performance is slightly reduced, the heat sealing strength and tensile strength are slightly reduced, and the oxygen permeability is 3.4 cc / m 2 *day, moisture permeability is 1.5 g / m 2 *day, heat seal strength (top seal) is 4.2kgf / 15mm, heat seal strength (bottom seal) is 4kgf / 15mm, tensile strength MD direction is 4.5 kgf / 15mm, TD direction is 3.9 kgf / 15mm, thickness is 143um, weight is 134g / m 2 , the rest of the test performances are within the qualified range.

[0084] Example 4 does not add vinyl alcohol-ethylene copolymer. The stretching ratio is the same as that of Example 2. The oxygen barrier performance is significantly reduced, the tensile strength is reduced, the heat sealing strength is increased, the oxygen barrier performance is significantly reduced, the moisture barrier performance is slightly reduced, the heat sealing strength and tensile strength are slightly reduced, and the oxygen permeability is 3.1 cc / m 2 *day, moisture permeability is 0.9 g / m 2 *day, heat seal strength (top seal) is 3.8 kgf / 15mm, heat seal strength (bottom seal) is 3.1 kgf / 15mm, tensile strength MD direction is 5.3 kgf / 15mm, TD direction is 4.7 kgf / 15mm, thickness is 143um, weight is 134g / m 2 , the rest of the test performances are within the qualified range.

[0085] The comparative example did not use the barrier bag structure and components of the present invention, and its performance was inferior to that of the barrier bag of the present invention, with an oxygen permeability of 8.5 cc / m 2 *day, moisture permeability: 2.3 g / m2 *day, heat seal strength (top seal) is 3.2 kgf / 15mm, heat seal strength (bottom seal) is 3.2 kgf / 15mm, tensile strength MD direction is 3.6 kgf / 15mm, TD direction is 2.3 kgf / 15mm, thickness is 68um, weight is 68g / m 2 , the rest of the test performances are within the qualified range.

[0086] Table 1

[0087] In summary, the barrier bag using the structure and components of the present invention has higher oxygen and moisture barrier properties, higher tensile strength and heat sealing strength than the control example. The increase in the longitudinal stretching multiple will further improve the oxygen and moisture barrier properties, tensile strength and heat sealing strength of the barrier bag of the present invention. In addition, the barrier bag of the present invention with the EVOH component added has higher oxygen and moisture barrier properties than the barrier bag of the present invention without EVOH added. Different components can be added according to the actual use scenario to meet different performance requirements.

[0088] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the drawings and the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.

[0089] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A barrier bag, characterized in that: It comprises a multilayer functional film stacked along the thickness direction, at least one layer of the functional film comprises a multilayer sub-functional film, the multilayer sub-functional film is combined into one by multi-layer co-extrusion, the multilayer functional film has an oriented lamellar structure by longitudinal stretching, and the polyethylene weight ratio of the barrier bag is greater than or equal to 90%.

2. The barrier bag according to claim 1, characterized in that: The components of the sub-functional membrane include polyethylene and copolymers thereof having at least one molecular chain length with at least one degree of branching.

3. The barrier bag according to claim 2, characterized in that: The components of the sub-functional film include at least one of low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, metallocene polyethylene, ethylene-vinyl alcohol polymer, and cyclic olefin copolymer.

4. The barrier bag according to claim 3, characterized in that: The number of layers of the sub-functional films of the functional film is an odd number, and the number of layers of the sub-functional films of the functional film does not exceed 11 layers.

5. The barrier bag according to claim 4, characterized in that: The multi-layer functional film includes a first barrier film, an aluminized film and a heat-sealing film, wherein the first barrier film is located at the outermost layer, the heat-sealing film is located at the innermost layer, and the aluminized film also includes an aluminized layer, which is arranged at the outermost side of the aluminized film and is respectively bonded to the sub-functional film of the first barrier film and the sub-functional film of the aluminized film.

6. The barrier bag according to claim 5, characterized in that: The aluminized film includes: nine layers of the sub-functional films and an aluminized layer; the first to ninth sub-functional films of the aluminized film have the same components and include high-density polyethylene, the thickness of the aluminized film is between 25um and 70um, and the thickness of the aluminized layer is between 2.9 angstroms and 3.5 angstroms.

7. The barrier bag according to claim 5, characterized in that: The first barrier film includes nine layers of sub-functional films; the fifth layer of the first barrier film includes ethylene-vinyl alcohol polymer, the fourth and sixth layers of the first barrier film have the same components and include polyolefin adhesive resin, the first and eighth layers of the first barrier film have the same components and include linear low-density polyethylene, the second, third and seventh layers of the first barrier film have the same components and include low-density polyethylene and metallocene polyethylene, and the mass ratio of the low-density polyethylene to the metallocene polyethylene is between 4:1 and 9:1, and the ninth layer of the first barrier film includes low-density polyethylene and linear low-density polyethylene, and the mass ratio of the low-density polyethylene to the linear low-density polyethylene is between 2:3 and 1:

1.

8. The barrier bag according to claim 7, characterized in that: The thickness of the first barrier film is between 15um and 35um.

9. The barrier bag according to claim 5, characterized in that: The first barrier film includes: nine layers of the sub-functional films; the components of the second to seventh sub-functional films of the first barrier film all include low-density polyethylene and metallocene polyethylene in a mass ratio between 4:1 and 9:1, the components of the first sub-functional film and the eighth sub-functional film of the first barrier film are the same and include linear low-density polyethylene, and the components of the ninth sub-functional film of the first barrier film include low-density polyethylene and linear low-density polyethylene and the mass ratio of the low-density polyethylene and the linear low-density polyethylene is between 2:3 and 1:

1.

10. The barrier bag according to any one of claims 5 to 9, characterized in that: The heat-sealing film comprises: nine layers of the sub-functional films; components of the first to eighth layers of the sub-functional films of the heat-sealing film comprise linear low-density polyethylene and cyclic olefin copolymer, and the mass ratio of the low-density polyethylene to the cyclic olefin copolymer is between 7:3 and 9:1; components of the ninth layer of the sub-functional film of the heat-sealing film comprise low-density polyethylene and linear low-density polyethylene, and the mass ratio of the low-density polyethylene to the linear low-density polyethylene is between 4:1 and 9:1; and the thickness of the heat-sealing film is between 30um and 60um.

Citation Information

Patent Citations

  • Propylene-based polymer multi-layer composite film, and preparation method, use and product thereof

    CN103847198A

  • Propylene polymer-ethylene polymer multilayer composite membrane containing composite bonding layers as well as preparation method, application and products thereof

    CN104149443A

  • Aluminum plating film, microwave composite film, and preparation methods of aluminum plating film and microwave composite film

    CN107839328A

  • All-plastic composite toothpaste tube sheet suitable for being recycled and production method of all-plastic composite toothpaste tube sheet

    CN114055889A

  • Environment-friendly packaging composite film, preparation method thereof and application of environment-friendly packaging composite film in yeast packaging