Preparation method of cerium dioxide with uniform particle size
By introducing organic dilution solvents and macromolecular group control agents during the cerium salt roasting process, the problem of large size and agglomeration of cerium dioxide nanoparticles is solved, uniform dispersion and efficient preparation of nanoscale cerium oxide is achieved, and production costs and processes are reduced. Complexity.
Patent Information
- Application Number
- CN202411091716.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-18
AI Technical Summary
Cerium dioxide nanoparticles prepared by traditional methods are large in size and easy to agglomerate, resulting in high wafer defect rates and poor dispersion in advanced processes. The production process requires complex conditions such as high temperature, high pressure, and catalysts, which increases cost and difficulty.
During the cerium salt roasting process, organic diluting solvents and macromolecular group control agents are introduced to reduce the particle size and prevent agglomeration through the nucleation mechanism of nanometer cerium oxide. Roasting is performed under constant temperature and mild conditions, reducing the reaction temperature and the number of steps.
Nanoscale cerium oxide particles with uniform particle size and good dispersion are obtained, which reduces production costs and reaction times, simplifies the process, and improves production efficiency.
Smart Images

Figure CN118791035A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth oxide material preparation, and particularly relates to a method for preparing cerium dioxide with uniform particle size. Background Art
[0002] Nano CeO2 is a widely used rare earth oxide with small particle size, high specific surface area and surface energy. It is often used in automobile exhaust treatment, solid fuel cells, catalysis, biology, grinding and other fields. With the increasing development of integrated circuits, the demand for IC chips is increasing, and the demand for integrated circuit materials is also increasing. For integrated circuit materials, Europe, the United States and Japan are in the world's leading position, and China's integrated circuit materials are still in a relatively backward state. Among integrated circuit materials, chemical mechanical polishing (CMP) related materials are one of the most critical materials, especially in advanced processes. CMP has an increasingly high status. Nano cerium oxide is a grinding particle for chemical mechanical polishing of integrated circuit dielectric materials, because cerium oxide has the characteristics of controllable heterogeneity and high selectivity.
[0003] Compared with traditional nano-silicon oxide particles, nano-cerium oxide particles not only have the characteristics of low silicon nitride removal rate, but also have the characteristics of high conversion of trivalent cerium ions and tetravalent cerium ions. In addition, the hardness of cerium oxide is lower than that of silicon oxide, which can effectively reduce the defects remaining on the wafer. These characteristics are very important for advanced processes and can effectively improve the yield rate of advanced wafer processes.
[0004] In the traditional method of preparing cerium dioxide, for example, a method for preparing cerium dioxide nanoparticles by high-temperature calcination is disclosed in a Chinese patent application with publication number CN110577233A, which uses cerium nitrate and dimethyl oxalate as a cerium source and a complexing agent, respectively, and aqueous solutions of cerium nitrate and dimethyl oxalate are prepared, mixed and stirred, and carbon black is added to prevent agglomeration. The reaction is carried out at 60°C for 20 hours, and after filtering, washing, and drying, the cerium dioxide nanoparticles are calcined at 700°C for 2 hours. However, the size of CeO2 particles synthesized by conventional preparation methods is generally greater than 150nm and is easy to agglomerate. These characteristics will lead to an increase in the defect rate on wafers of advanced processes. Therefore, the demand for reducing the size and agglomeration of nano cerium oxide particles has always been a difficult problem to solve. Moreover, the CeO2 particles prepared by conventional methods have poor dispersibility, and the production process requires high temperature and high pressure, catalysts and other conditions, the process is relatively complex, and the reaction cycle is long, which increases the difficulty and cost of production. Therefore, seeking a CeO2 preparation method with good dispersibility and simple process is still facing challenges. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for preparing cerium dioxide with uniform particle size. Starting from the nucleation mechanism of nano-cerium oxide, an organic diluent solvent and a macromolecular cluster control agent are introduced into the cerium salt roasting process, which can effectively solve the problem that the nano-cerium oxide particle size is large and easy to agglomerate, thereby obtaining nano-scale cerium oxide particles with smaller nano size, good dispersibility and concentrated particle size distribution; and it can solve the problems of high production conditions of CeO2, relatively complex process, long reaction cycle, and easy agglomeration in high temperature environment.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing cerium dioxide with uniform particle size comprises the following steps:
[0008] Step 1: heating cerium nitrate hexahydrate, a mixture of ethylene glycol and glycerol polyols and undecyl imidazoline at a constant temperature until they melt, and maintaining the temperature for a period of time;
[0009] Step 2: The above sample is calcined. During the calcination process, the temperature reaches the required temperature at a constant heating rate and is maintained for a period of time to obtain cerium dioxide powder with uniform particle size.
[0010] As a preferred solution for the preparation of cerium dioxide with uniform particle size, the mass ratio of the added cerium nitrate hexahydrate, the mixture of ethylene glycol and glycerol (1:1), and the undecyl imidazoline is 2:5:6.
[0011] As a preferred solution for the preparation of cerium dioxide with uniform particle size, the constant temperature of heating to melting is 60° C. and the holding time is 5 to 10 minutes.
[0012] As a preferred solution for the preparation of cerium dioxide with uniform particle size, the calcination conditions are air atmosphere, a constant heating rate of 2-10°C / min, a holding temperature of 300-500°C, and a holding time of 1-3h.
[0013] The beneficial effects of the present invention are:
[0014] Starting from the nucleation mechanism of nano-cerium oxide, the introduction of organic diluents and macromolecular group control agents in the cerium salt roasting process can effectively solve the problem of large particle size and easy agglomeration of nano-cerium oxide, thereby obtaining nano-scale cerium oxide particles with smaller nano-size, good dispersibility and concentrated particle size distribution; and compared with the traditional reaction to generate cerium dioxide, which requires high temperature, high pressure, catalyst and other reaction conditions, in the present invention, the reaction conditions are relatively mild, and the reaction can be carried out under the conditions of 60°C and one atmosphere, and no more expensive rare metals added as catalysts in traditional reactions are required, thereby greatly reducing the production cost compared with traditional reactions. ; In the roasting step, the traditional roasting step requires a temperature of at least 700°C, while the present invention only requires 300-500°C, further reducing the reaction cost; and the traditional process engineering price is complex, the reaction cycle is long, and the process usually requires three steps or more, and various precision instruments are required in the middle. Due to the large number of steps required for the reaction, the reaction time will also be longer than 12 hours. In the present invention, due to the use of a two-step reaction, the reaction can be effectively controlled within 4 hours, greatly reducing the reaction time, so that on the basis of low raw material cost and simple synthesis process, the production efficiency is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, and all of them belong to the protection scope of the present invention, among which:
[0016] Figure 1 It is the structural formula of the raw material required in the method for preparing cerium dioxide with uniform particle size provided by the present invention;
[0017] Figure 2 yes Figure 1 The structural formula of the product obtained by mixing various raw materials and heating and melting them in the method for preparing cerium dioxide with uniform particle size shown;
[0018] Figure 3 yes Figure 2 The method for preparing cerium dioxide with uniform particle size shown above generates a product that demonstrates its uniformity;
[0019] Figure 4 yes Figure 1 XDR image of cerium dioxide powder produced in the preparation method of cerium dioxide with uniform particle size shown;
[0020] Figure 5 yes Figure 1A scanning electron microscope image of cerium dioxide powder produced in the method for preparing cerium dioxide with uniform particle size shown;
[0021] Figure 6 yes Figure 1 The diameter distribution of cerium dioxide powder produced under different feed ratios in the preparation method of cerium dioxide with uniform particle size shown;
[0022] Figure 7 yes Figure 6 Scanning electron microscope images of cerium dioxide powders produced under different feed ratios in the preparation method of cerium dioxide with uniform particle size shown;
[0023] Figure 8 yes Figure 1 The particle size distribution diagram of the cerium dioxide powder produced by the preparation method of cerium dioxide with uniform particle size is shown. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] In the description of the present invention, the term "plurality" refers to two or more than two, unless otherwise clearly defined. The term "and / or" used herein includes any and all combinations of one or more related listed items. The terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; "connection" can also be a direct connection or an indirect connection through a medium. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances.
[0026] It should be noted that when an element is referred to as being "assembled on", "installed on", "fixed on" or "disposed on" another element, it can be directly connected to the other component or there can be a central element. When an element is considered to be "connected to" another element, it can be directly connected to the other element or there can be a central element. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0027] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0028] Nano CeO2 is a widely used rare earth oxide with small particle size, high specific surface area and surface energy. It is often used in automobile exhaust treatment, solid fuel cells, catalysis, biology, grinding and other fields. With the increasing development of integrated circuits, the demand for IC chips is increasing, and the demand for integrated circuit materials is also increasing. For integrated circuit materials, Europe, the United States and Japan are in the world's leading position, and China's integrated circuit materials are still in a relatively backward state. Among integrated circuit materials, chemical mechanical polishing (CMP) related materials are one of the most critical materials, especially in advanced processes. CMP has an increasingly high status. Nano cerium oxide is a grinding particle for chemical mechanical polishing of integrated circuit dielectric materials, because cerium oxide has the characteristics of controllable heterogeneity and high selectivity.
[0029] Compared with traditional nano-silicon oxide particles, nano-cerium oxide particles not only have the characteristics of low silicon nitride removal rate, but also have the characteristics of high conversion of trivalent cerium ions and tetravalent cerium ions. In addition, the hardness of cerium oxide is lower than that of silicon oxide, which can effectively reduce the defects remaining on the wafer. These characteristics are very important for advanced processes and can effectively improve the yield rate of advanced wafer processes.
[0030] In the traditional method of preparing cerium dioxide, for example, a method for preparing cerium dioxide nanoparticles by high-temperature calcination is disclosed in a Chinese patent application with publication number CN110577233A, which uses cerium nitrate and dimethyl oxalate as a cerium source and a complexing agent, respectively, and aqueous solutions of cerium nitrate and dimethyl oxalate are prepared, mixed and stirred, and carbon black is added to prevent agglomeration. The reaction is carried out at 60°C for 20 hours, and after filtering, washing, and drying, the cerium dioxide nanoparticles are calcined at 700°C for 2 hours. However, the size of CeO2 particles synthesized by conventional preparation methods is generally greater than 150nm and is easy to agglomerate. These characteristics will lead to an increase in the defect rate on wafers of advanced processes. Therefore, the demand for reducing the size and agglomeration of nano cerium oxide particles has always been a difficult problem to solve. Moreover, the CeO2 particles prepared by conventional methods have poor dispersibility, and the production process requires high temperature and high pressure, catalysts and other conditions, the process is relatively complex, and the reaction cycle is long, which increases the difficulty and cost of production. Therefore, seeking a CeO2 preparation method with good dispersibility and simple process is still facing challenges.
[0031] In the present invention, if Figure 1As shown, the materials required for the reaction are as follows: A is the raw material of cerium oxide, which is cerium nitrate hexahydrate; B and C are solvents, which are propylene glycol and ethylene glycol, which have the functions of dilution and dispersion; D is a cationic surfactant, which is undecyl imidazoline, which has the function of encapsulating A and providing space.
[0032] like Figure 2 As shown in the figure, when A, B, C and D are mixed in proportion and melted at elevated temperature, the molecules and ions in the mixture will automatically form OH bonds. Figure 2 The encapsulation structure is formed in the middle, and the molecular van der Waals force between D and A is greater than the molecular van der Waals force between B and A and between C and A. Therefore, A and D will be encapsulated to form a large molecular cluster, and B and C will automatically be interspersed in the A and D macromolecular clusters due to the relationship of OH bonds. In addition, in the small molecule solution of B and C, the macromolecular clusters of A and D will have excellent dispersibility. Due to the existence of the A and D macromolecular clusters, during the high-temperature roasting process, as the elements such as C, O, and N gradually vaporize, cerium oxide particles are finally left. It is the structure of the A and D macromolecular clusters that effectively prevents the agglomeration of cerium oxide particles, so this method can obtain non-agglomerated and uniformly distributed cerium oxide nanoparticles.
[0033] The embodiment of the present invention provides a method for preparing cerium dioxide with uniform particle size, which comprises: step 1: heating cerium nitrate hexahydrate, a mixture of ethylene glycol and glycerol polyols, and undecyl imidazoline at a constant temperature until they melt, and maintaining the temperature for a period of time;
[0034] Step 2: The above sample is calcined. During the calcination process, the temperature reaches the required temperature at a constant heating rate and is maintained for a period of time to obtain cerium dioxide powder with uniform particle size.
[0035] In the present invention, the above scheme is adopted, starting from the nucleation mechanism of nano-cerium oxide, and introducing an organic diluent solvent and a macromolecular group control agent in the cerium salt roasting process, which can effectively solve the problem of large particle size and easy agglomeration of nano-cerium oxide, thereby obtaining nano-scale cerium oxide particles with smaller nano-size, good dispersibility and concentrated particle size distribution; and compared with the traditional reaction to generate cerium dioxide, which requires high temperature, high pressure, catalyst and other reaction conditions, in the present invention, the reaction conditions are relatively mild, and the reaction can be carried out under the conditions of 60°C and one atmosphere, and no more expensive rare metals added as catalysts in the traditional reaction are required, thereby greatly improving the efficiency of the reaction compared with the traditional reaction. Reduce production costs; in the roasting step, the traditional roasting step requires a temperature of at least 700°C, while the present invention only requires 300-500°C, further reducing the reaction cost; and the traditional process engineering price is complex, the reaction cycle is long, and the process usually requires three steps or more, and various precision instruments are required in the middle. Due to the large number of steps required for the reaction, the reaction time will also be longer than 12 hours. In the present invention, due to the use of a two-step reaction, the reaction can be effectively controlled within 4 hours, greatly reducing the reaction time, so that on the basis of low raw material cost and simple synthesis process, the production efficiency is greatly improved.
[0036] Specifically, the mass ratio of the added cerium nitrate hexahydrate, the mixture of ethylene glycol and glycerol (1:1), and the undecyl imidazoline is 2:5:6.
[0037] Specifically, the constant temperature of heating to melting is 60° C., and the holding time is 5 to 10 minutes.
[0038] Specifically, the calcination conditions are air atmosphere, a constant heating rate of 2 to 10° C. / min, a holding temperature of 300 to 500° C., and a holding time of 1 to 3 hours.
[0039] The present invention is further described in detail below in conjunction with specific embodiments:
[0040] In the first step, 2 g of cerium nitrate hexahydrate, 10 g of a mixture of propylene glycol and ethylene glycol (1:1) and 12 g of undecyl imidazoline were weighed and placed in a quartz boat.
[0041] The second step is to move to a 60°C heating table, stir and heat until melted, and maintain for 5 to 10 minutes.
[0042] In the third step, after the sample is cooled, it is moved to a muffle furnace and heated to 300°C at a heating rate of 5°C / min, maintained for 120 min, and calcined to obtain a light yellow solid powder, which is CeO2.
[0043] Specifically, the cerium oxide produced by the above method has good uniformity because Figure 2The periphery of the macromolecules is a long-chain alkane structure, which helps to arrange these macromolecules in an orderly manner, such as Figure 3 As shown, during the calcination of the cerium salt, the ethylene glycol and propylene glycol added in the present invention can provide sufficient flow space for these macromolecular clusters, which is also conducive to the orderly arrangement of these macromolecular clusters, so that uniformly dispersed cerium oxide nanoparticles can be obtained.
[0044] The yellow solid powder obtained by calcination is subjected to X-ray powder diffraction analysis, scanning electron microscopy analysis, and particle size distribution analysis; Figure 4 As shown in FIG. 1 , from the XDR diagram obtained by X-ray powder diffraction analysis, it can be concluded that the above scheme can prepare pure CeO2 powder; Figure 5 As shown in FIG. 1 , the photographs analyzed by scanning electron microscope test show that the sample prepared by the above scheme is almost monodispersed nano-CeO2 particles; Figure 8 As shown, the graph from the particle size distribution test analysis shows that the CeO2 powder prepared by the above method has a uniform particle size distribution and the diameter of the CeO2 powder particles is appropriate.
[0045] like Figure 6 As shown in the figure, in order to demonstrate the implementation cases of different feed ratios of B / C / D, it is proved that the distribution of cerium oxide particles is greatly affected by D, but the influence of B / C is not significant, which is consistent with Figure 2 and Figure 3 The derived nanoparticle nucleation theory is consistent. The ratio in the figure represents the molar ratio of A: (B+C): D, with equal amounts of B and C. From the particle size distribution graph, it can be seen that when the ratio is 1:2: (4-8), the particle size distribution is better than that of competitors, and when it exceeds this range, the particle size distribution is worse than that of competitors. In addition, when the ratio of B and C is 0, the particle size distribution is worse than that of competitors. When the ratio of B and C is 2 or 10, the particle size distribution is better than that of competitors. The particle size distribution is best when the ratio of A to D is about 1:6, which is consistent with Figure 2 The derivation of the cerium salt coordination theory is consistent. When the ratio of A to D is lower than 1:6, the particle size distribution is significantly worse than that of the competing products. This is because the amount of D is insufficient to form all the cerium salts. Figure 2 The large molecular clusters in the particles deteriorate the particle size distribution.
[0046] like Figure 7 As shown, these four SEM test analysis photos are SEM images of nano-cerium oxide prepared by different methods. The upper left picture shows cerium oxide particles obtained by direct calcination of cerium salt, which have large particle size and serious agglomeration. The upper right picture shows cerium oxide particles obtained by calcination of cerium salt plus sodium dodecyl sulfate. The lower left picture shows cerium oxide particles obtained by calcination of cerium salt plus ethylene glycol and sodium dodecyl sulfate. The lower right picture shows cerium oxide particles obtained by calcination of cerium salt plus ethylene glycol, glycerol and undecyl imidazoline in the present invention. Figure 6It can be seen that the cerium oxide particles in the lower right figure not only have a smaller particle size but also have the best dispersibility.
[0047] The present invention is described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the scope of protection of the present invention.
Claims
1. A method for preparing cerium dioxide with uniform particle size, characterized in that: The following steps are involved: Step 1: heating cerium nitrate hexahydrate, a mixture of ethylene glycol and glycerol polyols and undecyl imidazoline at a constant temperature until they melt, and maintaining the temperature for a period of time; Step 2: The above sample is calcined. During the calcination process, the temperature reaches the required temperature at a constant heating rate and is maintained for a period of time to obtain cerium dioxide powder with uniform particle size.
2. The method for preparing cerium dioxide with uniform particle size according to claim 1, characterized in that: The mass ratio of the added cerium nitrate hexahydrate, the mixture of ethylene glycol and glycerol (1:1), and the undecyl imidazoline is 2:5:
6.
3. The method for preparing cerium dioxide with uniform particle size according to claim 1, characterized in that: Heat to a constant melting temperature of 60°C and maintain it for 5 to 10 minutes.
4. The method for preparing cerium dioxide with uniform particle size as claimed in claim 1, wherein the calcination conditions are air atmosphere, the constant heating rate is 2-10°C / min, the holding temperature is 300-500°C, and the holding time is 1-3h.