Preparation method of low-alkali accelerator taking modified aluminum ash as main raw material

Through the preparation of modified aluminum ash, the problems of poor adaptability of accelerating setting agents in shotcrete and insufficient utilization of secondary aluminum ash are solved. A low-alkali accelerating setting agent with superior performance and economy is prepared, achieving early reinforcement and safety of cement. , environmentally friendly applications.

CN118791245APending Publication Date: 2024-10-18JIANGSU CHINA RAILWAY ARIT NEW MATEIRALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410856322.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing liquid accelerating setting agents have problems in shotcrete projects such as poor adaptability, high dosage, temperature sensitivity and serious strength loss in the later period. Moreover, secondary aluminum ash has not been effectively utilized as a hazardous waste.

Method used

Modified aluminum ash is used as the main raw material, and a low-alkali accelerating agent is prepared through steps such as calcination, grinding, stirring, and dripping. The alkali content is controlled between 6% and 18%. It is combined with magnesium oxide, fluoride, etc. Forms an ultra-fine powder with a high aluminum oxide content that is used to promote the setting and hardening of concrete.

Benefits of technology

The prepared low-alkali accelerator has superior performance, low price, and strong adaptability. It can effectively promote the early strengthening and setting of cement, meet the green utilization and high-value needs of secondary aluminum ash, and has good economic and environmental benefits. benefit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004918171190000061
    Figure BDA0004918171190000061
  • Figure BDA0004918171190000071
    Figure BDA0004918171190000071
  • Figure BDA0004918171190000091
    Figure BDA0004918171190000091
Patent Text Reader

Abstract

The invention discloses a preparation method of a low-alkali accelerator taking modified aluminum ash as a main raw material. The preparation method comprises the following steps: compounding secondary aluminum ash and a modified raw material, calcining at high temperature, cooling and grinding to obtain the modified aluminum ash; preparing a sodium-containing compound solution; stirring the modified aluminum ash and water in a glass reaction container at normal temperature to prepare an aluminum ash solution, and dropwise adding a sodium-containing compound solution; adding a suspending agent into the solution, continuously stirring for 15-30 minutes, dropwise adding a thickening agent, keeping the temperature, stirring, and taking out of a pot to obtain a low-alkali accelerator; wherein the mass percent of each component is as follows: 30%-40% of the modified aluminum ash, 10%-20% of the iron-free aluminum sulfate, 5%-15% of the sodium-containing compound, 0.5%-1.5% of the suspending agent and 0.5%-1.5% of the thickening agent. The modified aluminum ash-based low-alkali accelerator prepared by the preparation method disclosed by the invention is relatively high in adaptability to cement, shows a good coagulation accelerating effect and an early-stage reinforcing effect with Portland cement, ordinary Portland cement and standard cement, and has relatively high use value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of low-alkali accelerating setting agent for shotcrete, and in particular to a preparation method of a low-alkali accelerating setting agent with modified aluminum ash as a main raw material. Background Art

[0002] Accelerator is a chemical admixture that can make cement or concrete set and harden quickly. It has become one of the essential components of shotcrete for tunnel engineering and underground engineering. At present, liquid accelerators at home and abroad are mainly divided into three categories according to the alkali content: alkali-free accelerator, low-alkali accelerator and alkaline accelerator. The advantages of economy make up for the shortcomings of alkali-free accelerator, such as poor adaptability, high dosage and temperature sensitivity, and alkaline accelerator, which has serious strength loss and poor stability in the later stage. It can not only ensure the safe application of accelerator in shotcrete engineering, but also has economic advantages.

[0003] Secondary aluminum ash is the solid waste obtained after aluminum slag is extracted. Because it contains a large amount of aluminum oxide, it is listed in the "National Hazardous Waste List" and is HW321-026-48 hazardous waste. According to statistics, the production of 1 ton of primary aluminum produces about 35 kg of secondary aluminum ash, and the production of 1 ton of recycled aluminum produces about 100 kg of secondary aluminum ash. The composition of secondary aluminum ash is relatively complex and has obvious hazardous characteristics. It contains 3% to 9% of metal aluminum particles, 40% to 70% of aluminum oxide, 5% to 10% of oxides such as SiO2 and MgO, and 3% to 6% of fluorides such as Na3AlF6, NaF, and CaF2. Modified aluminum ash is to compound secondary aluminum ash with magnesium oxide, silicon dioxide and other substances for thermal excitation. The excited aluminum ash is the main source of aluminum in the accelerator and has a high utilization value. As a solid hazardous waste, secondary aluminum ash contains rich aluminum resources. It is made into an accelerator and applied in shotcrete to produce valuable products, which will have very important practical significance. Summary of the invention

[0004] 1. Technical problems to be solved:

[0005] In view of the above technical problems, the present invention provides a method for preparing a low-alkali accelerating setting agent using modified aluminum ash as the main raw material. 2. Technical solution:

[0006] A method for preparing a low-alkali quick-setting agent using modified aluminum ash as a main raw material, characterized in that it comprises the following steps:

[0007] Step 1: Compound the secondary aluminum ash with the modified raw material and place it in a high-temperature tubular sintering furnace for calcination. After cooling, grind it to form a black powdery ultrafine powder, which is the modified aluminum ash, and the aluminum oxide content is ≥20%;

[0008] Step 2: Mix the sodium-containing compound and water in equal proportions to prepare a sodium-containing compound solution with a concentration of 50%;

[0009] Step 3: placing the modified aluminum ash and water in a glass reaction container and stirring at room temperature to prepare an aluminum ash solution;

[0010] Step 4: Add the sodium compound solution prepared in step 2 dropwise to the aluminum ash solution in a stirred state;

[0011] Step 5: After the addition is completed, add the suspending agent to the solution and continue stirring for 15-30 minutes, then add the thickener, maintain the temperature at 80-90°C and stir for 1-3 hours before removing from the pan to obtain a low-alkali quick-setting agent; the alkali content of the low-alkali quick-setting agent is ≥6% and ≤18%;

[0012] In the above process, the mass percentage of each component in the total amount of raw materials is: modified aluminum ash 30% to 40%, iron-free aluminum sulfate 10% to 20%, sodium compound 5% to 15%, suspending agent 0.5% to 1.5%, thickener 0.5% to 1.5%, and the balance is water.

[0013] Furthermore, the modified raw material includes magnesium oxide and silicon dioxide, and the compounding process of step 1 is:

[0014] The secondary aluminum ash is placed in water and fully stirred. After stirring, it is allowed to stand for a period of time, the upper liquid is filtered off, and the lower aluminum ash is placed in a 105°C oven for drying. After drying and cooling, the pretreated secondary aluminum ash is obtained.

[0015] According to the following mass percentages, take the pretreated secondary aluminum ash: 78%-82%; magnesium oxide: 13%-16%; silicon dioxide: 3%-4%; lime: 2%-3%; place it in a mixer and mix it for 10-20 minutes, add 5%-6% of polypropylene alcohol as a binder, and after fully mixing, place it in a hydraulic molding machine and press it into a green body; the molding pressure during the pressing process is 25MPa, and the holding time is 2min; place the green body in a 100-110℃ oven and dry it for 24h, and sinter it in a high-temperature tubular sintering furnace after constant weight. After the reaction is completed, the cooled clinker is placed in a vibrating ultrafine grinding and mixing machine and ground to make its specific surface area reach 400m 2 / kg, you can get modified aluminum ash.

[0016] Furthermore, the iron-free aluminum sulfate is a white powdery ultrafine powder with a particle size of 0 to 2 mm, and its aluminum oxide accounts for ≥16%.

[0017] Furthermore, the sodium-containing compound is one or more of sodium hydroxide, sodium fluoride, and sodium aluminate mixed in any proportion.

[0018] Furthermore, the suspending agent is one or more of hydrated magnesium silicate, attapulgite, and sepiolite mixed in any proportion.

[0019] Furthermore, the thickener is high molecular weight polyacrylamide or carboxymethyl cellulose.

[0020] Furthermore, the green body is a cylindrical green body, and the cylinder has a height of 1 cm and a diameter of 2.5 cm.

[0021] 3. Beneficial effects:

[0022] (1) The modified aluminum ash-based low-alkali accelerator prepared by the method has better performance and higher economic value. Compared with products with the same performance, the low-alkali accelerator is cheap, about 1 / 3 to 1 / 5 of the price of products with the same performance.

[0023] (2) The modified aluminum ash-based low-alkali quick-setting agent prepared by this method has strong adaptability to cement, and exhibits good accelerating effect and early strengthening effect on silicate cement, ordinary silicate cement and benchmark cement, and has high use value.

[0024] (3) The modified aluminum ash-based low-alkali quick-setting agent prepared by this method has secondary aluminum ash as its main raw material, which is hazardous waste. This invention can successfully synthesize low-alkali quick-setting agent from secondary aluminum ash, meeting the requirements of green production of secondary aluminum ash and high value-added products. In addition, this technology has high reliability, low operating cost, strong product market competitiveness, good overall economic efficiency and good environmental benefits. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail in the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] The secondary aluminum ash mentioned in the following embodiments of the present invention is provided by an aluminum plant in Shandong, and aluminum sulfate, sodium hydroxide, sodium fluoride, sodium aluminate, suspending agent and thickener are all purchased commercially.

[0027] In the specific embodiment, the high-efficiency performance evaluation of the generated modified aluminum ash-based low-alkali accelerator includes: the high-efficiency performance evaluation is mainly a comprehensive evaluation from the main performance, economy and operability of the aluminum ash-based low-alkali accelerator. The main performance of the modified aluminum ash-based low-alkali accelerator includes: stability, setting time, 1d compressive strength, and rebound rate; the economy mainly includes: the local availability of the raw materials of the modified aluminum ash-based low-alkali accelerator, the cost of the modified aluminum ash-based low-alkali accelerator and the dosage of the modified aluminum ash-based low-alkali accelerator in the shotcrete; the operability mainly includes the complexity of the synthesis process and the complexity of the on-site construction.

[0028] The method for evaluating the stability performance of the modified aluminum ash-based low-alkali quick-setting agent in the following examples and comparative examples is as follows: a certain amount of modified aluminum ash-based low-alkali quick-setting agent sample is placed in a measuring cylinder with a stopper, allowed to stand for a period of time at a certain temperature, and the volume of the supernatant or the volume of the bottom sediment is tested.

[0029] The preparation of modified aluminum ash-based low-alkali quick-setting agent in the following embodiments all includes two steps: 1. Preparation of modified aluminum ash; 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; Since the preparation of modified aluminum ash in each embodiment is common, the following step 1 will be performed first. And in order to avoid the impact of multiple variables on the performance of low-alkali quick-setting agent and affect the comparison between the specific embodiments and the comparative examples, in step 1 of the following embodiments, the modified aluminum ash ratios are all: secondary aluminum ash 80%, magnesium oxide 14%, silicon dioxide 3.5%, lime 2.5%, polypropylene alcohol 6%.

[0030] 1. Prepare modified aluminum ash; first take 1500g of secondary aluminum ash and place it in water for full stirring. After stirring, let it stand for a while, filter out the upper liquid, and place the lower aluminum ash in a 105℃ oven for drying. The product after drying and cooling is the secondary aluminum ash; take 1000g of secondary aluminum ash, 180g of magnesium oxide, 45g of silicon dioxide, and 30g of lime, mix them and place them in a mixer for 15-20min, add 30g of polypropylene alcohol as a binder, mix them well and place them in a hydraulic forming machine, and press them into cylindrical green bodies. Place the green cylinder in a 105℃ oven and dry it for 24h. After constant weight, sinter it in a high-temperature tubular sintering furnace. After the reaction is completed, take out the clinker after cooling. Place the cooled clinker in a vibrating ultrafine grinding mixer and grind it for 10min. Its specific surface area is measured to be 425m 2 / kg, and modified aluminum ash is obtained. Specific embodiment 1:

[0032] 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; components and proportions of its raw materials:

[0033] Components Proportion Modified aluminum ash 40% Aluminum sulfate 10% Sodium hydroxide solution (45%) 15% Attapulgite 0.6% Polyacrylamide 0.4% water 34%

[0034] The preparation steps are:

[0035] 2.1 Place the modified aluminum ash and water in a glass reaction container for a preliminary reaction to form an aluminum ash solution. A small amount of gas will be generated during this process.

[0036] 2.2 Use a drop pump to slowly drop the sodium hydroxide solution into the glass container. The reaction process is quite intense and a large amount of gas will be generated (which can be collected). During the dropwise addition, turn on the heat preservation and stirring, set the temperature to 85°C, and stir at medium speed throughout the process.

[0037] 2.3 After the addition is completed, add attapulgite, adjust the speed to high-speed stirring, and stir for 30 minutes, then add polyacrylamide.

[0038] 2.4 After all the materials are put in, keep warm and stir for 2 hours at 85℃, then close the water bath and cool to room temperature to obtain the aluminum ash-based low-alkali quick-setting agent. Specific embodiment 2:

[0040] 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; components and proportions of raw materials:

[0041] Components Proportion Modified aluminum ash 40% Aluminum sulfate 10% Sodium fluoride solution (45%) 15% Attapulgite 0.6% Polyacrylamide 0.4% water 34%

[0042] The preparation steps are:

[0043] 2.1 Place the modified aluminum ash and water in a glass reaction container for a preliminary reaction to form an aluminum ash solution. A small amount of gas will be generated during this process.

[0044] 2.2 Use a dropping pump to slowly drop the sodium fluoride solution into the glass container. The reaction process is quite intense and a large amount of gas will be generated (which can be collected). During the dropping process, turn on the heat preservation and stirring, set the temperature to 85℃, and stir at medium speed throughout the process.

[0045] 2.3 After the addition is completed, add attapulgite, adjust the speed to high-speed stirring, and stir for 30 minutes, then add polyacrylamide.

[0046] 2.4 After all the materials are put in, keep warm and stir for 2 hours at 85℃, then close the water bath and cool to room temperature to obtain the aluminum ash-based low-alkali quick-setting agent.

[0047] Example 3

[0048] 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; components and proportions of raw materials:

[0049] Components Proportion Modified aluminum ash 40% Aluminum sulfate 10% Sodium aluminate solution (45%) 15% Attapulgite 0.6% Polyacrylamide 0.4% water 34%

[0050] The preparation steps are:

[0051] 2.1 Place the modified aluminum ash and water in a glass reaction container for a preliminary reaction to form an aluminum ash solution. A small amount of gas will be generated during this process.

[0052] 2.2 Use a dropping pump to slowly drop the sodium aluminate solution into the glass container. The reaction process is quite intense and a large amount of gas will be generated (which can be collected). During the dropping process, turn on the heat preservation and stirring, set the temperature to 85℃, and stir at medium speed throughout the process.

[0053] 2.3 After the addition is completed, add attapulgite, adjust the speed to high-speed stirring, and stir for 30 minutes, then add polyacrylamide.

[0054] 2.4 After all the materials are put in, keep warm and stir for 2 hours at 85℃, then close the water bath and cool to room temperature to obtain the aluminum ash-based low-alkali quick-setting agent.

[0055] Example 4

[0056] 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; components and proportions of raw materials:

[0057]

[0058]

[0059] The preparation steps are:

[0060] 2.1 Place the modified aluminum ash and water in a glass reaction container for a preliminary reaction to form an aluminum ash solution. A small amount of gas will be generated during this process.

[0061] 2.2 Use a drop pump to slowly drop the sodium hydroxide solution into the glass container. The reaction process is quite intense and a large amount of gas will be generated (which can be collected). During the dropwise addition, turn on the heat preservation and stirring, set the temperature to 85°C, and stir at medium speed throughout the process.

[0062] 2.3 After the dropwise addition is completed, hydrated magnesium silicate is added, and the speed is immediately adjusted to high-speed stirring for 30 minutes, and then polyacrylamide is added.

[0063] 2.4 After all the materials are put in, keep warm and stir for 2 hours at 85℃, then close the water bath and cool to room temperature to obtain the aluminum ash-based low-alkali quick-setting agent.

[0064] Embodiment 5:

[0065] 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; raw material components and their proportions:

[0066] Components Proportion Modified aluminum ash 30% Aluminum sulfate 20% Sodium hydroxide solution (45%) 15% Meerschaum 1% Polyacrylamide 1% water 33%

[0067] The preparation steps are:

[0068] 2.1 Place the modified aluminum ash and water in a glass reaction container for a preliminary reaction to form an aluminum ash solution. A small amount of gas will be generated during this process.

[0069] 2.2 Use a drop pump to slowly drop the sodium hydroxide solution into the glass container. The reaction process is quite intense and a large amount of gas will be generated (which can be collected). During the dropwise addition, turn on the heat preservation and stirring, set the temperature to 85°C, and stir at medium speed throughout the process.

[0070] 2.3 After the addition is completed, add sepiolite, adjust the speed to high-speed stirring, the stirring time is 30 minutes, and then add polyacrylamide.

[0071] 2.4 After all the materials are put in, keep warm and stir for 2 hours at 85℃, then close the water bath and cool to room temperature to obtain the aluminum ash-based low-alkali quick-setting agent.

[0072] Example 6

[0073] 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; components and proportions of raw materials:

[0074] Components Proportion Modified aluminum ash 30% Aluminum sulfate 20% Sodium hydroxide solution (45%) 15% Hydrated magnesium silicate 1% Carboxymethyl cellulose 1% water 33%

[0075] The preparation steps are:

[0076] 2.1 Place the modified aluminum ash and water in a glass reaction container for a preliminary reaction to form an aluminum ash solution. A small amount of gas will be generated during this process.

[0077] 2.2 Use a drop pump to slowly drop the sodium hydroxide solution into the glass container. The reaction process is quite intense and a large amount of gas will be generated (which can be collected). During the dropwise addition, turn on the heat preservation and stirring, set the temperature to 85°C, and stir at medium speed throughout the process.

[0078] 2.3 After the addition is completed, add hydrated magnesium silicate, adjust the speed to high-speed stirring, stir for 30 minutes, and then add carboxymethyl cellulose.

[0079] 2.4 After all the materials are put in, keep warm and stir for 2 hours at 85℃, then close the water bath and cool to room temperature to obtain the aluminum ash-based low-alkali quick-setting agent.

[0080] Embodiment 7:

[0081] 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; components and proportions of raw materials:

[0082] Components Proportion Modified aluminum ash 35% Aluminum sulfate 25% Sodium hydroxide solution (45%) 5% Attapulgite 1% Carboxymethyl cellulose 1% water 33%

[0083] The preparation steps are:

[0084] 2.1 Place the modified aluminum ash and water in a glass reaction container for a preliminary reaction to form an aluminum ash solution. A small amount of gas will be generated during this process.

[0085] 2.2 Use a drop pump to slowly drop the sodium hydroxide solution into the glass container. The reaction process is quite intense and a large amount of gas will be generated (which can be collected). During the dropwise addition, turn on the heat preservation and stirring, set the temperature to 85°C, and stir at medium speed throughout the process.

[0086] 2.3 After the dropwise addition is completed, attapulgite is added, and the speed is immediately adjusted to high-speed stirring for 30 minutes, followed by the addition of carboxymethyl cellulose.

[0087] 2.4 After all the materials are put in, keep warm and stir for 2 hours at 85℃, then close the water bath and cool to room temperature to obtain the modified aluminum ash-based low-alkali quick-setting agent.

[0088] Embodiment 8:

[0089] 2. Preparation of modified aluminum ash-based low-alkali quick-setting agent; components and proportions of raw materials:

[0090]

[0091]

[0092] The preparation steps are:

[0093] 2.1 Place the modified aluminum ash and water in a glass reaction container for a preliminary reaction to form an aluminum ash solution. A small amount of gas will be generated during this process.

[0094] 2.2 Use a drop pump to slowly drop the sodium hydroxide solution into the glass container. The reaction process is quite intense and a large amount of gas will be generated (which can be collected). During the dropwise addition, turn on the heat preservation and stirring, set the temperature to 85°C, and stir at medium speed throughout the process.

[0095] 2.3 After the addition is completed, add sepiolite, adjust the speed to high-speed stirring, stir for 30 minutes, and then add carboxymethyl cellulose.

[0096] 2.4 After all the materials are put in, keep warm and stir for 2 hours at 85℃, then close the water bath and cool to room temperature to obtain the modified aluminum ash-based low-alkali quick-setting agent.

[0097] Comparative Example 1

[0098] The low-alkali quick-setting agent prepared with reference to Example 1 in patent CN116874221A comprises the following steps:

[0099] (1) Take an appropriate amount of water and mix sodium hydroxide and aluminum hydroxide in a mass ratio of 1:2.5 to prepare a sodium aluminate solution;

[0100] (2) Add an appropriate amount of water to the sodium aluminate solution, stir evenly, then add aluminum sulfate to the above system at once, start stirring and heating, set the reaction temperature to 60°C and keep the reaction for 0.5h;

[0101] (3) After the aluminum sulfate reaction is complete, a regulator is added dropwise to the above system within 10 minutes to adjust the pH value to neutral;

[0102] (4) using a stirring device to mix sodium carbonate and hydrophilic silica gel in a mass ratio of 2:1 to obtain a modifier, and then adding the modifier to sodium fluorosilicate and mixing to obtain modified sodium fluorosilicate; the specific surface area of ​​the silica gel is 600 m2 / g;

[0103] (5) adding the modified sodium fluorosilicate to the neutral solution of (3) and keeping the temperature at 60°C for 1 hour;

[0104] (6) Turn off the heating, add organic alcohol amine, and stir for 0.5 h to obtain the low-alkali quick-setting agent.

[0105] The weight percentage of the prepared low-alkali quick-setting agent is:

[0106]

[0107]

[0108] Comparative Example 2

[0109] Referring to the early strength liquid low-alkali quick-setting agent prepared in the embodiment of patent CN117964275A, the method comprises the following steps:

[0110] (1) reacting sodium hydroxide and aluminum hydroxide at a sodium-aluminum ratio of 1:1.18 to obtain a 50% sodium aluminate solution, and adding an alcohol substance to the reaction for preliminary alcoholization;

[0111] (2) alcoholizing aluminum hydroxide with a pH value of 2 and alkaline alcohol to obtain a weakly acidic aluminum salt solution with a pH value of 4 to 6;

[0112] (3) Add the weakly acidic aluminum salt solution obtained in step (2) dropwise into a 65° C. sodium aluminate liquid under a high-speed emulsifier to make its pH value reach 11, thereby obtaining a translucent alcoholized alkaline aluminum sol.

[0113] The surface modifier is prepared by:

[0114] (1) adding 40-50% of isopentenyl polyoxyethylene, 0.2-1% of polyethylene glycol monomethyl ether esterified macromonomer and 20-40% of water to a reactor equipped with a stirrer, raising the temperature in the reactor to 35° C., and stirring the solution therein until it becomes colorless and transparent;

[0115] (2) adding three solutions A, B, and C to the reaction kettle simultaneously, wherein solution A is a mixture of 3-4% g of acrylic acid and 2-5% of water, solution B is a mixture of 0.01-0.1% of ascorbic acid, 0.1-2% of thioglycolic acid, and 5-8% of water, and solution C is a mixture of 1-6% of hydrogen peroxide, 1.15-1.20% of sodium gluconate, and 5-8% of water;

[0116] (3) Add 0.5-0.8% solid sodium hydroxide into the reaction kettle and stir until dissolved to obtain a colorless and transparent surface modifier.

[0117] The modified calcium silicate crystals are prepared by:

[0118] (1) adding water and a surface modifier into a reaction kettle at room temperature;

[0119] (2) Use a high-speed emulsifier to stir for 15 minutes;

[0120] (3) adding modified sodium silicate nonahydrate solution and calcium nitrate solution to the reaction kettle simultaneously, the dropping time is 40 minutes;

[0121] (4) After the dropwise addition is completed, the mixture is stirred at high speed for 30 minutes to obtain modified calcium silicate crystals.

[0122] Under the stirring of a high-speed emulsifier, a certain amount of modified calcium silicate crystal solution is added dropwise to the heat-insulated alcoholized alkaline aluminum sol, and the early-strength liquid low-alkali quick-setting agent is obtained after reacting for 3 to 4 hours.

[0123] Comparative Example 3:

[0124] Referring to the low-alkali quick-setting agent prepared in the embodiment of patent CN114477831A, the method comprises the following steps:

[0125] (1) To prepare 1 kg of the low-alkali quick-setting agent, the following raw materials are required:

[0126] Components quality Sodium aluminate solution 100 Aluminum sulfate (Group A: Group B = 1:1.5) 600 Magnesium sulfate 40 Hydrofluoric acid 40 Phosphoric acid 30 Triethanolamine 100 Acetic acid 10 water 80

[0127] (2) Place a 1000 ml four-necked flask in a water bath, add sodium aluminate and water, set the water bath temperature to 50 °C and start stirring at a stirring speed of 350 rpm;

[0128] (3) Slowly add aluminum sulfate from group A into the four-necked flask and stir for about 10 minutes;

[0129] (4) Slowly add triethanolamine into the four-necked flask, preferably the adding time is controlled within 3 to 5 minutes, and then react for about 15 minutes;

[0130] (5) Slowly add aluminum sulfate from group B into the four-necked flask and stir for about 30 minutes;

[0131] (6) Add magnesium sulfate into the four-necked flask and adjust the stirring speed to 300 rpm;

[0132] (7) Slowly add 40% hydrofluoric acid to the four-necked flask, control the addition time to about 3 min to 5 min, and react for about 30 min;

[0133] (8) Add phosphoric acid into a four-necked flask and stir for about 20 minutes;

[0134] (9) Add acetic acid into a four-necked flask and stir for about 1 hour to obtain a transparent liquid, which is the low-doping and low-alkali quick-setting agent. The table shows the performance test results of the quick-setting agents of the embodiment and the comparative example.

[0135]

[0136]

[0137] As can be seen from the table, compared with other common low-alkali quick-setting agents, the modified aluminum ash-based low-alkali quick-setting agent (Example 4) of the present invention has better setting time and strength. This is because the modified aluminum ash contains more aluminum oxide components, and a large amount of calcium aluminate is generated in the early stage of hydration in a low-alkali environment, which promotes the hydration of tricalcium silicate, shortens the setting time of cement slurry and improves the early compressive strength of mortar.

[0138] Although the present invention has been disclosed as above in terms of preferred embodiments, they are not intended to limit the present invention. Anyone skilled in the art can make various changes or modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection defined by the claims of this application.

Claims

1. A method for preparing a low-alkali quick-setting agent using modified aluminum ash as the main raw material, characterized by: The following steps are involved: Step 1: The secondary aluminum ash is mixed with the modified raw material and then placed in a high-temperature tubular sintering furnace for calcination. After cooling, it is ground into powder. The resulting black powder is the modified aluminum ash, and its aluminum oxide content is ≥20%. Step 2: Stir the sodium-containing compound and water in equal proportions to prepare a sodium-containing compound solution with a concentration of 50%; Step 3: Place the modified aluminum ash and water in a glass reaction container and stir at room temperature to prepare an aluminum ash solution; Step 4: Add the sodium compound solution prepared in step 2 dropwise to the stirred aluminum ash solution; Step 5: After the addition is completed, add the suspending agent to the solution and continue stirring for 15-30 minutes, then add the thickener dropwise, maintain the temperature at 80-90℃ and stir for 1-3 hours before removing from the pot to obtain the low-alkali accelerator; the alkali content of the low-alkali accelerator is ≥6% and ≤18%; In the above process, the mass percentage of each component in the total amount of raw materials is: modified aluminum ash 30% to 40%, iron-free aluminum sulfate 10% to 20%, sodium compound 5% to 15%, suspending agent 0.5% to 1.5%, thickener 0.5% to 1.5%, and the balance is water. The method for preparing a low-alkali accelerator using modified aluminum ash as the main raw material according to claim 1 is characterized in that: the modified raw material includes magnesium oxide and silicon dioxide, and the compounding process of step 1 is: The secondary aluminum ash is placed in water and stirred thoroughly. After stirring, it is allowed to stand for a period of time. The upper liquid is filtered off, and the lower aluminum ash is placed in a 105°C oven for drying. After drying and cooling, the pretreated secondary aluminum ash is obtained. According to the following mass percentages, take the pretreated secondary aluminum ash: 78% to 82%; magnesium oxide: 13% to 16%; silicon dioxide: 3% to 4%; lime: 2% to 3%; place it in a mixer and mix it for 10-20 minutes, add 5% to 6% of polypropylene alcohol as a binder, and after fully mixing, place it in a hydraulic molding machine and press it into a green body; the molding pressure during the pressing process is 25MPa, and the holding time is 2min; the green body is placed in a 100-110℃ oven to dry for 24h, and sintered in a high-temperature tubular sintering furnace after constant weight. After the reaction is completed, the cooled clinker is placed in a vibrating ultrafine grinding and mixing machine and ground to make its specific surface area reach 400m 2 / kg, you can get modified aluminum ash.

2. The method for preparing a low-alkali accelerating setting agent with modified aluminum ash as the main raw material according to claim 1, characterized in that: The iron-free aluminum sulfate is a white powdery ultrafine powder with a particle size of 0 to 2 mm, and its aluminum oxide content is ≥16%.

3. The method for preparing a low-alkali quick-setting agent with modified aluminum ash as the main raw material according to claim 1, characterized in that: The sodium-containing compound is one or more of sodium hydroxide, sodium fluoride, and sodium metaaluminate mixed in any proportion.

4. The method for preparing a low-alkali accelerating setting agent with modified aluminum ash as the main raw material according to claim 1, characterized in that: The suspending agent is one or more of hydrated magnesium silicate, attapulgite and sepiolite mixed in any proportion.

5. The method for preparing a low-alkali quick-setting agent with modified aluminum ash as the main raw material according to claim 1, characterized in that: The thickener is high molecular weight polyacrylamide or carboxymethyl cellulose.

6. The method for preparing a low-alkali quick-setting agent with modified aluminum ash as the main raw material according to claim 2, characterized in that: The green compact is a cylindrical green compact, and the cylinder has a height of 1 cm and a diameter of 2.5 cm.