Cement anchoring agent as well as use method and application thereof
By using a combination of water glass and aluminum sulfate early strength agent in the anchoring agent, the problems of slow setting speed and poor corrosion resistance of the anchoring agent are solved, and rapid setting, high early strength and good expansion are achieved, which is suitable for use in coal mines. anchoring applications and reduces cost and pollution.
Patent Information
- Application Number
- CN202410967725.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing anchoring agents have problems such as slow setting speed, low early strength, insufficient expansion rate and poor corrosion resistance when used in coal mines. In particular, resin anchoring agents have high cost and poor durability, while ordinary Portland cement anchoring agents are economical. Low but insufficient anchoring power.
A cement anchoring agent formula is used, including cement, water glass solution with a sodium modulus of 3.3, expansion agent UEA and aluminum sulfate early strength agent. After dry mixing and adding water, the water glass solution is added to form rapid setting, high early strength and good Swelling anchoring agent and solidifies in the anchor hole.
It achieves rapid condensation, early high strength and good expansibility of the anchoring agent, improves the anchoring force and corrosion resistance, meets the application requirements in mines and coal mines, while reducing economic costs, and the materials are easy to obtain, low emissions, and low pollute.
Smart Images

Figure CN118791269A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to a cement anchoring agent and a use method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Anchoring agent refers to a kind of cementing material used to fix the anchor body for reinforcement. It is often used in underground coal mine tunnels where metal anchors are used for support. Anchoring agents are divided into resin anchoring agents and ordinary silicate cement anchoring agents. Resin anchoring agents have high production costs, poor anchoring strength with rock formations, and poor durability of organic materials.
[0004] Ordinary Portland cement anchors have low economic costs, but they set slowly, have low initial strength, and insufficient expansion rates, which lead to insufficient anchoring force in the later stages. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a cement anchoring agent and a method for using and application thereof, which has the advantages of fast setting speed, high early strength, good expansion, good anchoring force and corrosion resistance.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] In a first aspect, a cement anchoring agent comprises the following components in parts by weight:
[0008] 100 parts of cement, 20-25 parts of water glass solution with a sodium modulus of 3.3, 3-9 parts of expansion agent UEA, 2.0-3.0 parts of aluminum sulfate early strength agent and water with a water-cement ratio of 0.3.
[0009] Optionally, the cement is ordinary Portland cement.
[0010] Optionally, the ordinary Portland cement is ordinary Portland cement of grade P.O42.5.
[0011] Optionally, the expansion agent UEA is an admixture with one or more of aluminum sulfate, aluminum oxide, and potassium aluminum sulfate as main components.
[0012] Optionally, in the aluminum sulfate early strength agent, the aluminum sulfate salt component accounts for more than 95%.
[0013] In a second aspect, the method for using the above-mentioned cement anchoring agent comprises the following steps:
[0014] S1. Dry mix cement, expansion agent UEA and aluminum sulfate early strength agent, and mix them evenly to form a mixed dry material;
[0015] S2. Add water to the mixed dry materials and mix them, then add the water glass solution and stir evenly to obtain a cement anchoring agent;
[0016] S3. Bag the cement anchor and put it into the anchor hole, waiting for it to solidify.
[0017] Optionally, in S3, the ambient temperature is 20°C.
[0018] A third aspect is the application of the above-mentioned cement anchor and / or the method for using the cement anchor in mines and coal mines.
[0019] The beneficial effects of the present invention are:
[0020] 1. The present invention selects water glass as an admixture to shorten the setting time. Water glass can effectively bond mineral tissues, accelerate the setting and hardening of silicate cement, and shorten the setting time. At the same time, silicate can effectively prevent the erosion of CI-, resist groundwater erosion, and improve corrosion resistance; the expansion agent UEA can form trisulfur type hydrated calcium sulfoaluminate (ettringite), and the formation of ettringite phase increases the volume of the solid phase, causing apparent volume expansion, and improving the initial anchoring force and gripping force of the anchor; the early strength agent is mainly composed of aluminum sulfate, and the effective component is greater than 95%. The early strength agent can accelerate the hydration of C3A and the formation of ettringite, thereby improving the early strength of the entire anchor body and giving full play to the bearing function of the surrounding rock; the combination of the three improves the setting speed and early strength of the anchoring agent and improves the anchoring performance.
[0021] 2. The present invention does not use high-cost raw materials, the raw materials are easy to obtain and the formula design is reasonable; and during the application process, it is conducive to the classified storage of various raw materials, which are prepared on the spot, with very little waste of materials, and has the advantages of low emissions and low pollution; it improves the anchoring performance while reducing the economic cost.
[0022] 3. The product of the present invention has a fast setting speed, high early strength, and good anchoring force after adding water. It is tested using MT219-2002 "cement anchor roll anchoring agent" and can meet the technical requirements of the full anchor. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0024] Figure 1 is a flow chart of the method of use in a specific embodiment of the present invention;
[0025] Figure 21 and 2 are sensitivity analysis results of various factors of the anchoring agent in the specific implementation mode of the present invention; (A) is the analysis result of the initial setting time, (B) is the analysis result of the final setting time, (C) is the analysis result of the 3d expansion rate, (D) is the analysis result of the 7d expansion rate, (E) is the analysis result of the 1h compressive strength, and (F) is the analysis result of the 24h compressive strength. DETAILED DESCRIPTION
[0026] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0027] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0028] A cement anchoring agent comprises the following components in parts by weight:
[0029] 100 parts of cement, 20-30 parts of water glass solution with a sodium modulus of 3.3, 5-10 parts of expansion agent UEA, 2-3 parts of aluminum sulfate early strength agent and water with a water-cement ratio of 0.3.
[0030] Optionally, the cement is ordinary Portland cement.
[0031] Optionally, the ordinary Portland cement is ordinary Portland cement of grade P.O42.5.
[0032] The function of water glass solution is to shorten the setting time. Water glass can effectively bond mineral tissue, accelerate the setting and hardening of silicate cement, and shorten the setting time. At the same time, silicate can effectively prevent CI - It can resist the erosion of groundwater, improve the corrosion resistance, improve the durability, and effectively ensure the later anchoring strength;
[0033] The sodium modulus is used to indicate the sodium silicate content in the sodium silicate solution, which means the molar ratio of silicate ions to sodium ions in the solution. The viscosity of the water glass solution with a sodium modulus of 3.3 is relatively high, and it is neutral water glass.
[0034] Optionally, the expansion agent UEA is an admixture with one or more of aluminum sulfate, aluminum oxide, and potassium aluminum sulfate as main components, which can increase the expansion rate of the anchor; it forms trisulfide hydrated calcium sulfoaluminate (calcium sulfoaluminate) by self-hydration or participating in the hydration of cement minerals or reacting with cement hydration products; the formation of the calcium sulfoaluminate phase greatly increases the volume of the solid phase, so adding a small amount can effectively adjust the expansion rate, causing apparent volume expansion, and improving the initial anchoring force and grip strength of the anchor.
[0035] Optionally, in the aluminum sulfate early strength agent, the aluminum sulfate salt component accounts for more than 95%. The early strength of the anchoring agent determines the anchoring effect of the anchoring system. The early strength agent can accelerate the hydration of C3A and the formation of ettringite, thereby improving the early strength of the entire anchor body and giving full play to the bearing function of the surrounding rock.
[0036] The method for using the cement anchoring agent comprises the following steps:
[0037] S1. Dry mix cement, expansion agent UEA and aluminum sulfate early strength agent, and mix them evenly to form a mixed dry material;
[0038] S2. Add water glass solution with a sodium modulus of 3.3 to the mixed dry materials and stir evenly to obtain a cement anchoring agent;
[0039] S3. Put the cement anchor into the anchor hole after bagging, add water at a water-cement ratio of 0.3, and wait for it to solidify.
[0040] Optionally, in S3, the ambient temperature is 20°C.
[0041] The application of the above-mentioned cement anchor and / or the method for using the cement anchor in mines and coal mines includes: anchoring of metal bolts in coal mine tunnels.
[0042] Example 1
[0043] A cement anchoring agent comprises the following components in parts by weight: 100 parts of P.O42.5 grade ordinary Portland cement;
[0044] 10 to 30 parts of water glass solution with a sodium modulus of 3.3;
[0045] Expanding agent UEA, 1-12 parts;
[0046] 1 to 3 parts of aluminum sulfate early strength agent;
[0047] The water-to-cement ratio is 0.3-0.5.
[0048] The method for using the cement anchoring agent comprises the following steps:
[0049] S1. Dry mix cement, expansion agent UEA and aluminum sulfate early strength agent, and mix them evenly to form a mixed dry material;
[0050] S2. Add water to the mixed dry materials and mix them, then add the water glass solution and stir evenly to obtain a cement anchoring agent;
[0051] S3. Bag the cement anchor and put it into the anchor hole, waiting for it to solidify.
[0052] Optionally, in S3, the ambient temperature is 20°C.
[0053] The above components are optimized by orthogonal test. The design levels / factors of the orthogonal test are shown in Table 1, wherein the amount of water glass, the amount of early strength agent and the amount of expansion agent are all based on 100 parts of P.O42.5 grade ordinary Portland cement as 100% by weight.
[0054] Table 1
[0055]
[0056]
[0057] The sequence number and ratio of each factor of the orthogonal experiment are shown in Table 2, wherein the amount of water glass, the amount of early strength agent and the amount of expansion agent are based on 100 parts of P.O42.5 grade ordinary Portland cement by weight as 100%.
[0058] Table 2
[0059]
[0060] The test results of the orthogonal test are shown in Table 3.
[0061] Table 3
[0062]
[0063] According to the orthogonal test results, the initial setting time, final setting time, 3d expansion rate, 7d expansion rate, 1h uniaxial compressive strength, and 24h uniaxial compressive strength of the anchor are analyzed by range analysis. The order of importance of each influencing factor in the orthogonal test scheme can be sorted through range analysis, and then the significance of each factor on the index can be determined, and the law and trend of each output index changing with the factor can be obtained by analysis. The theoretical formula of range analysis is shown as follows:
[0064] R=max(K j )-min(K j ),
[0065] Among them, y i For the test results,
[0066] The final range calculation results are shown in Table 4. And draw a sensitivity analysis chart, such as Figure 2 shown.
[0067] Table 4
[0068]
[0069] like Figure 2 As shown, with the minimum initial setting time and final setting time, maximum expansion rate (including 3d expansion rate and 7d expansion rate) and compressive strength (including 1h compressive strength and 24h compressive strength) as the goal orientation, the optimal conditions of the four indicators are comprehensively balanced to find the conditions that take into account the main factors of each indicator.
[0070] like Figure 2 (A) Initial setting time analysis results and Figure 2 The final setting time analysis results of (B) show that in terms of the effect of setting speed, the water-binder ratio ( Figure 2 The influence of water-cement ratio (expressed as water-cement ratio in the text, the two have the same meaning) is the greatest. As the water-cement ratio gradually increases, the setting time is prolonged. Secondly, the influence of water glass content is relatively obvious. As the water glass content increases, the setting time decreases. The effects of early strength agent and expansion agent on the initial setting time are relatively small.
[0071] like Figure 2 (C) 3D expansion rate analysis results and Figure 2 The 7d expansion rate analysis results of (D) show that in terms of the influence of expansion rate, the expansion agent dosage has the greatest effect. When its content exceeds 9%, the effect slows down, indicating that there is a limit value; the water-cement ratio has the second greatest influence.
[0072] like Figure 2 (E) 1h compressive strength analysis results and Figure 2 The 24h compressive strength analysis results of (F) show that in terms of compressive strength, the early strength agent has the greatest effect, and the increase of water-binder ratio and expansion agent will cause the compressive strength to gradually decrease.
[0073] Through analysis, the optimal level of factor A is K1, the optimal level of factor B is K3, the optimal level of factor C is K4, and the optimal level of factor D is K4, so the optimal combination is AK1BK3CK4DK4, that is, the water-cement ratio is 0.3, the water glass content is 25%, the early strength agent content is 2.5%, and the expansion agent content is 9%.
[0074] MT219-2002 "Cement Anchor Roll Anchor" stipulates that the full anchor method: initial setting time is 4 to 7 minutes, final setting time is less than 10 minutes; compressive strength is 15Mpa (1h), 25Mpa (24h).
[0075] Analysis of the orthogonal test results shows that the cement anchor comprising the following components in parts by weight meets the requirements of MT219-2002 "Cement Anchor Roll Anchor" for full anchor anchors.
[0076] Specifically:
[0077] 100 parts of P.O42.5 grade ordinary Portland cement;
[0078] 20-30 parts of water glass solution with a sodium modulus of 3.3;
[0079] Expanding agent UEA, 3-9 parts;
[0080] Aluminum sulfate early strength agent 2.0-3.0 parts;
[0081] The water-to-cement ratio is 0.3.
[0082] The initial setting time is 6-7 minutes, the final setting time is 8-10 minutes; the compressive strength is 15.06-19.77Mpa (1h), 25.03-33.98Mpa (24h); the 3d expansion rate is 0.1-0.56%, and the 7d expansion rate is 0.28-0.74%. It meets the requirements of MT219-2002 "Cement Anchor Roll Anchor" for full anchor anchors.
[0083] Example 2
[0084] A cement anchoring agent, using the best combination AK1BK3CK4DK4 obtained in Example 1, that is, composed of the following components in parts by weight:
[0085] 100 parts of P.O42.5 grade ordinary Portland cement;
[0086] 25 parts of water glass solution with a sodium modulus of 3.3;
[0087] Expanding agent UEA, 9 parts;
[0088] 2.5 parts of aluminum sulfate early strength agent;
[0089] Water-cement ratio, 0.3.
[0090] The method of using the anchoring agent is:
[0091] S1. Dry mix cement, expansion agent UEA and aluminum sulfate early strength agent, and mix them evenly to form a mixed dry material;
[0092] S2. Add water glass solution with a sodium modulus of 3.3 to the mixed dry materials and stir evenly to obtain a cement anchoring agent;
[0093] S3. Bag the cement anchor and put it into the anchor hole. Add water at a water-cement ratio of 0.3 and wait for it to solidify at an ambient temperature of 20°C.
[0094] The anchoring agent of this embodiment is tested by the same testing method as that of embodiment 1. The high-strength quick-setting anchoring agent has an initial setting time of 6 to 7 minutes and a final setting time of 8 to 9 minutes; compressive strength: 16.4Mpa (1h), 28.2Mpa (24h); 3d expansion rate 0.32%, 7d expansion rate 0.54%; it meets the requirements of MT219-2002 "cement anchor roll anchoring agent" for full anchoring agents. It can be used in mines and coal mines.
[0095] Grip force test
[0096] The anchoring agent in Example 2 was used in the mechanical model of soft rock blocks. Samples were taken from the engineering site and processed into cubes with a size of 15 cm × 15 cm × 15 cm. A circular hole with a diameter of 12 mm was punched in the center of the cube. A steel bar with a length of 15 cm and φ6 mm was selected as an anchor rod. The anchoring agent was poured into the rock sample according to the usage method, and then the anchor rod was inserted. After curing for 24 hours, the anchor rod was pulled out, and the pull-out force at which the anchor structure failed during the pulling process was tested.
[0097] After testing, the average pull-out force was 10.8kN and the type of failure was cracking of the anchor body, proving that the new anchoring agent has superior anchoring performance.
[0098] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A cement anchoring agent, characterized in that: The composition comprises the following components in parts by weight: 100 parts of cement, 20-25 parts of water glass solution with a sodium modulus of 3.3, 3-9 parts of expansion agent UEA, 2.0-3.0 parts of aluminum sulfate early strength agent and water with a water-cement ratio of 0.
3.
2. The cement anchoring agent according to claim 1, characterized in that The cement is ordinary Portland cement.
3. The cement anchoring agent according to claim 2, characterized in that: The ordinary Portland cement is ordinary Portland cement of P.O42.5 grade.
4. The cement anchoring agent according to claim 1, characterized in that: The expansion agent UEA is an admixture with one or more of aluminum sulfate, aluminum oxide, and potassium aluminum sulfate as main components.
5. The cement anchoring agent according to claim 1, characterized in that: In the aluminum sulfate early strength agent, the aluminum sulfate salt component accounts for more than 95%.
6. The cement anchoring agent according to any one of claims 1 to 5, characterized in that: The composition comprises the following components in parts by weight: 100 parts of P.O42.5 grade ordinary Portland cement, 25 parts of water glass solution with a sodium modulus of 3.3, 9 parts of expansion agent UEA, 2.5 parts of aluminum sulfate early strength agent and water with a water-cement ratio of 0.
3.
7. A method for using the cement anchoring agent according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Dry mix cement, expansion agent UEA and aluminum sulfate early strength agent, and mix them evenly to form a mixed dry material; S2. Add water to the mixed dry materials and mix them, then add the water glass solution and stir evenly to obtain a cement anchoring agent; S3. Bag the cement anchor and put it into the anchor hole, waiting for it to solidify.
8. The method for using the cement anchoring agent according to claim 7, characterized in that: In S3, the ambient temperature is 20°C.
9. Use of the cement anchoring agent according to any one of claims 1 to 6 and / or the method for using the cement anchoring agent according to any one of claims 7 to 9 in mines and coal mines.
10. The use according to claim 9, characterized in that Used for anchoring metal bolts in coal mine tunnels.
Citation Information
Patent Citations
Anchoring mortar and application method thereof
CN105218011A
Cement-based high-performance anchoring agent
CN109053100A
Anti-bleeding grouting material for splitting compaction grouting and preparation method of anti-bleeding grouting material
CN115385596A
Cement composition for bolt anchoring and bolt anchoring method
WO2020008794A1