Preparation method of multi-material foaming insole and multi-material foaming sole
By adjusting the component proportions and additives during the midsole preparation process to form a network structure, the problem of deformation and cracking during the foaming process of the multi-material midsole is solved, and a multi-material foam midsole with balanced performance and stable shape is achieved. Meet the use needs of shoe soles.
Patent Information
- Application Number
- CN202410858826.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing midsoles are prone to deformation and joint cracking during the multi-material foaming process, resulting in uneven performance and inconvenient use.
A multi-material foam midsole preparation method is adopted, by mixing materials of different components at different temperatures to form girth strips and belly fillers, and during the foaming process, the mold is evacuated to form a network structure to ensure The shape stability of the material after foaming and the firmness of the joint.
It achieves no deformation and cracking of the multi-material midsole, improves the support and cushioning performance, meets the use requirements of the sole, and improves the material's resilience and anti-deformation capabilities by finely adjusting the component ratio and additives.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of midsole materials, and in particular to a preparation method of a multi-material foamed midsole and a multi-material foamed sole. Background Art
[0002] In order to improve the different performances of the shoe midsole corresponding to different positions of the human foot, different materials or midsole materials with different performances can be used in different parts of the shoe midsole. Existing midsoles are generally made of foaming materials, such as EVA, TPEE, etc. When the midsole is made of at least two foaming materials, the two materials need to be spliced before foaming. This splicing is generally connected with glue, and then foaming is performed. However, since different materials have different foaming ratios under the same temperature and environment, if foaming is performed simultaneously, the midsole after foaming will be deformed and cracks will appear at the joints of different materials. Summary of the invention
[0003] The purpose of the present invention is to overcome the above-mentioned defects or problems existing in the background technology, and to provide a method for preparing a multi-material foamed midsole and a multi-material foamed sole, which can improve the deformation of the multi-material midsole after foaming and the cracking of the joints.
[0004] To achieve the above object, the present invention adopts the following technical solutions:
[0005] A method for preparing a multi-material foamed midsole comprises the following steps: preparing a strip material: mixing the following components by weight at a temperature of 115±5°C for 10-15 minutes: 40-50 parts of a first ethylene vinyl acetate copolymer, 10-15 parts of a second ethylene vinyl acetate copolymer, 20-25 parts of a polyolefin elastomer, 10-20 parts of a hydrogenated styrene-butadiene block copolymer, 2-10 parts of ethylene propylene diene monomer rubber, 0.2-0.5 parts of an active agent, and 4-8 parts of a low-temperature foaming agent. Then add the following parts by weight of auxiliary agent 0.5-1 parts, crosslinking agent 0.5-1 parts, and mix at 120±5℃ for 10-15min; prepare the abdominal filling material: mix the following parts by weight at 115±5℃ for 10-15min: 20-30 parts of the first ethylene vinyl acetate copolymer, 25-30 parts of the second ethylene vinyl acetate copolymer, 15-20 parts of the polyolefin elastomer, 20-25 parts of the hydrogenated styrene-butadiene block copolymer, 2-5 parts of EPDM rubber, 9-10 parts of wear-resistant agent, 0.2-0.5 parts of active agent, 4-8 parts of low-temperature foaming agent; then add 0.5-1 parts of the following auxiliary agents and 0.5-1 parts of cross-linking agent in the following weight parts, and mix at 120±5℃ for 10-15min; prepare the midsole embryo: inject the mixed and molten strip material and the belly filling material into the embryo mold respectively, and surround the strip material around the belly filling material to form the strip part and the belly filling part respectively, so that the strip part and the belly filling part are connected The parts are bonded together, and then allowed to stand and cool to obtain a midsole embryo; foaming: the midsole embryo is placed in a foaming mold, the mold temperature is set to 172±3°C, and the mold is vacuumed. After 7-8 minutes, the foaming is completed, and the foamed product is taken out and allowed to stand and cool naturally at room temperature to obtain a foamed midsole; wherein the vinyl acetate (VA) content in the first ethylene-vinyl acetate copolymer is 26%, and the vinyl acetate (VA) content in the second ethylene-vinyl acetate copolymer is 33%.
[0006] Furthermore, the hydrogenated styrene-butadiene block copolymer adopts a star-shaped SEBS with a molecular weight of 300,000 to 350,000.
[0007] Furthermore, the grade of the polyolefin elastomer is POE8003.
[0008] Furthermore, the active agent is stearic acid.
[0009] Furthermore, the anti-wear agent is an organic silicon anti-wear agent.
[0010] Furthermore, the auxiliary agent is zinc carbonate.
[0011] Furthermore, the cross-linking agent is dicumyl peroxide.
[0012] Furthermore, the low-temperature foaming agent is white azodicarbonamide.
[0013] In addition, the present invention also provides a multi-material foamed sole, characterized in that the multi-material foamed sole is obtained by using the foamed midsole obtained by the preparation method of the multi-material foamed midsole as described in any one of technical solutions 1 to 8 as a raw material and undergoing a compression molding process; in the compression molding process, the mold heating time is 8-9 minutes, the mold heating temperature is 160±5°C, and the cooling time is 7-8 minutes.
[0014] It can be seen from the above description of the present invention that, compared with the prior art, the present invention has the following beneficial effects:
[0015] The present invention provides a method for preparing a multi-material foamed midsole and a multi-material foamed sole. The multi-material foamed midsole prepared by the method has substantially no deformation after foaming, and no cracking at the joint of the strip material and the filling material, although the foaming ratios of the strip material and the filling material are different. Meanwhile, the strip part formed by the strip material has better supporting performance, and the filling material formed by the filling material has better shock-absorbing performance, thereby meeting the use requirements of the sole.
[0016] In the present invention, the main components of the strip material and the filling material are ethylene vinyl acetate copolymer, polyolefin elastomer and hydrogenated styrene-butadiene block copolymer. However, since the strip material and the filling material are used in different positions in the midsole embryo, there is a big difference in the formula proportions of the two. By finely adjusting the mass proportions of the corresponding components, the strip material enhances the support performance on the basis of good rebound, and the filling material further enhances the rebound and shock-absorbing performance. At the same time, although there is a difference in foaming ratio when the strip material and the filling material are foamed synchronously at different mass proportions, the two shrink to the same extent in the cooling process after foaming because they use basically the same components, and the deformation of the midsole after foaming is caused by shrinkage. The shrinkage degree is inconsistent during the process; and polyolefin elastomer is added to the surrounding strip material and the belly filling material, which can help the surrounding strip and the belly filling maintain good shape stability during the shrinkage process; in addition, if the midsole is deformed after foaming, it will also cause cracks at the positions where the different materials were originally connected by glue, and the surrounding strip and the belly filling in the present invention are already bonded together during injection, and during foaming, they will be physically cross-linked at the bonding positions of the surrounding strip and the belly filling to form a spatial network structure, so that during the cooling process after foaming, even if there is a slight deformation of the surrounding strip and the belly filling, the connection between the two is very firm, and there will be no uneven edges of the two materials at the joint.
[0017] In the present invention, two ethylene vinyl acetate copolymers with different VA contents are used in the components, among which EVA with a VA content of 26% can provide basic hardness and wear resistance, so that the final material has a better shock-absorbing effect, and EVA with a VA content of 33% can bring better softness and elasticity to the material, so that the final material has better rebound performance; the amounts of the two ethylene vinyl acetate copolymers in the surrounding strip material and the belly filling material are different, thereby bringing different physical properties to the surrounding strip part and the belly filling part.
[0018] In addition, hydrogenated styrene-butadiene block copolymer is specially added, and preferably star-shaped SEBS with a molecular weight of 300,000 to 350,000 is added. Adding a certain amount of star-shaped SEBS can improve the deformation resistance of the surrounding strips and filling materials, and the surrounding strips and filling materials can better maintain their own shapes during the shrinkage process after foaming. In addition, SEBS itself has good mechanical properties and can be combined with ethylene vinyl acetate copolymer and polyolefin elastomer to improve the resilience of the final material, and at the same time, it can also improve the surface finish of the product.
[0019] The use of a low-temperature foaming agent can reduce the impact of the color of the foaming agent on the final material, and foaming at a low temperature can reduce the overall foaming ratio, thereby reducing the difference in foaming ratios between the surrounding material and the filling material, and further improving the deformation of the midsole after foaming. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are preferred embodiments of the present invention and should not be regarded as excluding other embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] In the claims and description of the present invention, if the terms "include", "have" and their variations are used, they are intended to mean "including but not limited to".
[0022] The present invention provides a method for preparing a multi-material foam midsole and a multi-material foam sole, wherein the method for preparing the multi-material foam midsole comprises the following steps:
[0023] Step 1, prepare the strip material: mix the following components by weight at a temperature of 115±5°C for 10-15min: 40-50 parts of the first ethylene vinyl acetate copolymer, 10-15 parts of the second ethylene vinyl acetate copolymer, 20-25 parts of the polyolefin elastomer, 10-20 parts of the hydrogenated styrene-butadiene block copolymer, 2-10 parts of EPDM rubber, 0.2-0.5 parts of the active agent, and 4-8 parts of the low-temperature foaming agent; then add the following auxiliary agents by weight 0.5-1 parts and cross-linking agent 0.5-1 parts, and mix at a temperature of 120±5°C for 10-15min;
[0024] Step 2, prepare the abdominal filling material: mix the following components by weight at a temperature of 115±5°C for 10-15min: 20-30 parts of the first ethylene vinyl acetate copolymer, 25-30 parts of the second ethylene vinyl acetate copolymer, 15-20 parts of the polyolefin elastomer, 20-25 parts of the hydrogenated styrene-butadiene block copolymer, 2-5 parts of EPDM rubber, 9-10 parts of the wear-resistant agent, 0.2-0.5 parts of the active agent, and 4-8 parts of the low-temperature foaming agent; then add the following auxiliary agents by weight 0.5-1 parts and cross-linking agent 0.5-1 parts, and mix at a temperature of 120±5°C for 10-15min;
[0025] Step 3, preparing a midsole embryo: injecting the mixed and molten surrounding strip material and the filling material into the embryo mold respectively, and surrounding the surrounding strip material around the filling material to form a surrounding strip portion and a filling portion respectively, so that the junction of the surrounding strip portion and the filling portion is bonded, and then standing and cooling to obtain a midsole embryo;
[0026] Step 4: Foaming: Place the midsole embryo into a foaming mold, set the mold temperature to 172±3°C, and evacuate the mold. After 7-8 minutes, the foaming is completed. Take out the foamed product and let it stand and cool naturally at room temperature to obtain a foamed midsole.
[0027] The vinyl acetate (VA) content in the first ethylene-vinyl acetate copolymer is 26%, and the vinyl acetate (VA) content in the second ethylene-vinyl acetate copolymer is 33%.
[0028] The hydrogenated styrene-butadiene block copolymer uses star-shaped SEBS with a molecular weight of 300,000 to 350,000, and the brand is Baling Petrochemical 604T. The anti-wear agent uses an organic silicon anti-wear agent, specifically a silicone coupling agent. The active agent uses stearic acid. The auxiliary agent uses zinc carbonate. The cross-linking agent uses diisopropylbenzene peroxide. The low-temperature foaming agent uses white azodicarbonamide.
[0029] After the midsole embryo is prepared, it is foamed. During the foaming process, as the temperature of the embryo increases from the surface to the inside, the embryo is in a molten state as a whole. The decomposition temperature of the low-temperature foaming agent is about 135°C. It decomposes rapidly in the mold with a gas emission of 120mL / g. The decomposed gas is mainly nitrogen, and the rest is carbon monoxide, carbon dioxide and a small amount of ammonia. Under the action of the foaming agent, the surrounding strips and the filling belly of the embryo gradually expand, and different components are cross-linked to form a network structure until the foaming time is over. The mold is opened to obtain the foamed product.
[0030] The present invention provides a method for preparing a multi-material foamed midsole and a multi-material foamed sole. The multi-material foamed midsole prepared by the method has substantially no deformation after foaming, and no cracking at the joint of the strip material and the filling material, although the foaming ratios of the strip material and the filling material are different. Meanwhile, the strip part formed by the strip material has better supporting performance, and the filling material formed by the filling material has better shock-absorbing performance, thereby meeting the use requirements of the sole.
[0031] In the present invention, the main components of the strip material and the filling material are ethylene vinyl acetate copolymer, polyolefin elastomer and hydrogenated styrene-butadiene block copolymer. However, since the strip material and the filling material are used in different positions in the midsole embryo, there is a big difference in the formula proportions of the two. By finely adjusting the mass proportions of the corresponding components, the strip material enhances the support performance on the basis of good rebound, and the filling material further enhances the rebound and shock-absorbing performance. At the same time, although there is a difference in foaming ratio when the strip material and the filling material are foamed synchronously at different mass proportions, the two shrink to the same extent in the cooling process after foaming because they use basically the same components, and the deformation of the midsole after foaming is caused by shrinkage. The shrinkage degree is inconsistent during the process; and polyolefin elastomer is added to the surrounding strip material and the belly filling material, which can help the surrounding strip and the belly filling maintain good shape stability during the shrinkage process; in addition, if the midsole is deformed after foaming, it will also cause cracks at the positions where the different materials were originally connected by glue, and the surrounding strip and the belly filling in the present invention are already bonded together during injection, and during foaming, they will be physically cross-linked at the bonding positions of the surrounding strip and the belly filling to form a spatial network structure, so that during the cooling process after foaming, even if there is a slight deformation of the surrounding strip and the belly filling, the connection between the two is very firm, and there will be no uneven edges of the two materials at the joint.
[0032] In the present invention, two ethylene vinyl acetate copolymers with different VA contents are used in the components, among which EVA with a VA content of 26% can provide basic hardness and wear resistance, so that the final material has a better shock-absorbing effect, and EVA with a VA content of 33% can bring better softness and elasticity to the material, so that the final material has better rebound performance; the amounts of the two ethylene vinyl acetate copolymers in the surrounding strip material and the belly filling material are different, thereby bringing different physical properties to the surrounding strip part and the belly filling part.
[0033] In addition, hydrogenated styrene-butadiene block copolymer is specially added, and preferably star-shaped SEBS with a molecular weight of 300,000 to 350,000 is added. Adding a certain amount of star-shaped SEBS can improve the deformation resistance of the surrounding strips and filling materials, and the surrounding strips and filling materials can better maintain their own shapes during the shrinkage process after foaming. In addition, SEBS itself has good mechanical properties and can be combined with ethylene vinyl acetate copolymer and polyolefin elastomer to improve the resilience of the final material, and at the same time, it can also improve the surface finish of the product.
[0034] The use of a low-temperature foaming agent can reduce the impact of the color of the foaming agent on the final material, and foaming at a low temperature can reduce the overall foaming ratio, thereby reducing the difference in foaming ratios between the surrounding material and the filling material, and further improving the deformation of the midsole after foaming.
[0035] In addition, the present invention also provides a multi-material foamed sole, which uses the foamed midsole obtained by the preparation method of the multi-material foamed midsole provided by the above technical solution as a raw material, and undergoes a compression molding process to obtain the multi-material foamed sole; in the compression molding process, the mold heating time is 8-9 minutes, the mold heating temperature is 160±5°C, and the cooling time is 7-8 minutes. Specifically, after the prepared foamed midsole is placed in the mold, the mold is closed and heated, and after the hot pressing process is completed according to the predetermined heating temperature and heating time, the mold is opened, and the hot pressed product is cooled in the mold for 7-8 minutes, and then taken out and left to cool naturally at room temperature for 24 hours to obtain the above-mentioned multi-material foamed sole.
[0036] In order to further illustrate the performance of the multi-material foamed midsole provided by the present invention, the following examples and comparative examples are provided.
[0037] Example 1
[0038] Weigh the components according to the following mass parts:
[0039] Strip material: first ethylene vinyl acetate copolymer: 42 parts; second ethylene vinyl acetate copolymer: 12 parts; polyolefin elastomer: 24 parts; hydrogenated styrene-butadiene block copolymer: 18 parts; EPDM rubber: 4 parts; active agent: 0.44 parts; auxiliary agent: 0.8 parts; cross-linking agent: 0.56 parts; low-temperature foaming agent: 4.5 parts.
[0040] Belly filling material: first ethylene vinyl acetate copolymer: 25 parts; second ethylene vinyl acetate copolymer: 30 parts; polyolefin elastomer: 20 parts; hydrogenated styrene-butadiene block copolymer: 22 parts; EPDM rubber: 3 parts; wear-resistant agent: 9.23 parts; active agent: 0.46 parts; auxiliary agent: 0.9 parts; cross-linking agent: 0.63 parts; low-temperature foaming agent: 6.2 parts.
[0041] The vinyl acetate content in the first ethylene vinyl acetate copolymer is 26%, and the vinyl acetate content in the second ethylene vinyl acetate copolymer is 33%. The hydrogenated styrene-butadiene block copolymer uses star-shaped SEBS with a molecular weight of 300,000 to 350,000, and the brand is Baling Petrochemical 604T. The anti-wear agent uses an organic silicon anti-wear agent, specifically a silicone coupling agent. The activator uses stearic acid. The auxiliary agent uses zinc carbonate. The high cross-linking agent uses diisopropylbenzene peroxide. The low-temperature foaming agent uses white azodicarbonamide.
[0042] Using the above components as raw materials, the multi-material midsole embryo is prepared according to the following steps:
[0043] Step 1: Prepare the strip material: weigh the other components of the strip material except the auxiliary agent and the cross-linking agent according to the mass fraction, and mix them at 115°C for 10 minutes; then add the auxiliary agent and the cross-linking agent, and mix them at 120°C for 10 minutes;
[0044] Step 2: Prepare the abdominal filling material: weigh the other components of the abdominal filling material except the auxiliary agent and the cross-linking agent according to the mass fraction, and mix them at 115°C for 10 minutes; then add the auxiliary agent and the cross-linking agent, and mix them at 120°C for 10 minutes;
[0045] Step 3: preparing a midsole embryo: injecting the mixed and molten strip material and the belly filling material into the embryo mold respectively, and surrounding the belly filling material with the strip material to form a strip portion and a belly filling portion respectively, so that the strip material and the belly filling material are bonded at the joint, and then standing and cooling to obtain a midsole embryo;
[0046] Step 4: Foaming: Place the midsole embryo into a foaming mold, set the mold temperature to 172°C, and evacuate the mold. After 7.5 minutes, the foaming is completed. Take out the foamed product and let it stand at room temperature to cool naturally to obtain a foamed midsole.
[0047] Example 2
[0048] Weigh the components according to the following mass parts:
[0049] Strip material: first ethylene vinyl acetate copolymer: 45 parts; second ethylene vinyl acetate copolymer: 10 parts; polyolefin elastomer: 23 parts; hydrogenated styrene-butadiene block copolymer: 17 parts; EPDM rubber: 5 parts; active agent: 0.42 parts; auxiliary agent: 0.75 parts; cross-linking agent: 0.6 parts; low-temperature foaming agent: 5 parts.
[0050] Belly filling material: first ethylene vinyl acetate copolymer: 26 parts; second ethylene vinyl acetate copolymer: 29 parts; polyolefin elastomer: 18 parts; hydrogenated styrene-butadiene block copolymer: 21 parts; EPDM rubber: 4 parts; wear-resistant agent: 9.5 parts; active agent: 0.48 parts; auxiliary agent: 0.85 parts; cross-linking agent: 0.65 parts; low-temperature foaming agent: 6.5 parts.
[0051] The vinyl acetate content in the first ethylene vinyl acetate copolymer is 26%, and the vinyl acetate content in the second ethylene vinyl acetate copolymer is 33%. The hydrogenated styrene-butadiene block copolymer uses star-shaped SEBS with a molecular weight of 300,000 to 350,000, and the brand is Baling Petrochemical 604T. The anti-wear agent uses an organic silicon anti-wear agent, specifically a silicone coupling agent. The activator uses stearic acid. The auxiliary agent uses zinc carbonate. The high cross-linking agent uses diisopropylbenzene peroxide. The low-temperature foaming agent uses white azodicarbonamide.
[0052] Using the above components as raw materials, the multi-material midsole embryo is prepared according to the following steps:
[0053] Step 1: Prepare the strip material: weigh the other components of the strip material except the auxiliary agent and the cross-linking agent according to the mass fraction, and mix them at 115°C for 15 minutes; then add the auxiliary agent and the cross-linking agent, and mix them at 120°C for 15 minutes;
[0054] Step 2: Prepare the abdominal filling material: weigh the other components of the abdominal filling material except the auxiliary agent and the cross-linking agent according to the mass fraction, and mix them at 115°C for 15 minutes; then add the auxiliary agent and the cross-linking agent, and mix them at 120°C for 15 minutes;
[0055] Step 3: preparing a midsole embryo: injecting the mixed and molten strip material and the belly filling material into the embryo mold respectively, and surrounding the belly filling material with the strip material to form a strip portion and a belly filling portion respectively, so that the strip material and the belly filling material are bonded at the joint, and then standing and cooling to obtain a midsole embryo;
[0056] Step 4: Foaming: Place the midsole embryo into a foaming mold, set the mold temperature to 172°C, and evacuate the mold. After 7.5 minutes, the foaming is completed. Take out the foamed product and let it stand at room temperature to cool naturally to obtain a foamed midsole.
[0057] Example 3
[0058] Weigh the components according to the following mass parts:
[0059] Strip material: first ethylene vinyl acetate copolymer: 43 parts; second ethylene vinyl acetate copolymer: 11 parts; polyolefin elastomer: 22 parts; hydrogenated styrene-butadiene block copolymer: 16 parts; EPDM rubber: 4 parts; active agent: 0.4 parts; auxiliary agent: 0.78 parts; cross-linking agent: 0.58 parts; low-temperature foaming agent: 4.8 parts.
[0060] Belly filling material: first ethylene vinyl acetate copolymer: 24 parts; second ethylene vinyl acetate copolymer: 28 parts; polyolefin elastomer: 19 parts; hydrogenated styrene-butadiene block copolymer: 23 parts; EPDM rubber: 3 parts; wear-resistant agent: 9.8 parts; active agent: 0.45 parts; auxiliary agent: 0.88 parts; cross-linking agent: 0.62 parts; low-temperature foaming agent: 6.3 parts.
[0061] The vinyl acetate content in the first ethylene vinyl acetate copolymer is 26%, and the vinyl acetate content in the second ethylene vinyl acetate copolymer is 33%. The hydrogenated styrene-butadiene block copolymer uses star-shaped SEBS with a molecular weight of 300,000 to 350,000, and the brand is Baling Petrochemical 604T. The anti-wear agent uses an organic silicon anti-wear agent, specifically a silicone coupling agent. The activator uses stearic acid. The auxiliary agent uses zinc carbonate. The high cross-linking agent uses diisopropylbenzene peroxide. The low-temperature foaming agent uses white azodicarbonamide.
[0062] Using the above components as raw materials, the multi-material midsole embryo is prepared according to the following steps:
[0063] Step 1: Prepare the strip material: weigh the other components of the strip material except the auxiliary agent and the cross-linking agent according to the mass fraction, and mix them at 115°C for 15 minutes; then add the auxiliary agent and the cross-linking agent, and mix them at 120°C for 15 minutes;
[0064] Step 2: Prepare the abdominal filling material: weigh the other components of the abdominal filling material except the auxiliary agent and the cross-linking agent according to the mass fraction, and mix them at 115°C for 15 minutes; then add the auxiliary agent and the cross-linking agent, and mix them at 120°C for 15 minutes;
[0065] Step 3: preparing a midsole embryo: injecting the mixed and molten strip material and the belly filling material into the embryo mold respectively, and surrounding the belly filling material with the strip material to form a strip portion and a belly filling portion respectively, so that the strip material and the belly filling material are bonded at the joint, and then standing and cooling to obtain a midsole embryo;
[0066] Step 4: Foaming: Place the midsole embryo into a foaming mold, set the mold temperature to 172°C, and evacuate the mold. After 7.5 minutes, the foaming is completed. Take out the foamed product and let it stand at room temperature to cool naturally to obtain a foamed midsole.
[0067] Comparative Example 1
[0068] Based on Example 1, the difference is that in the formula components, neither the surrounding strip material nor the belly filling material includes a polyolefin elastomer component.
[0069] Comparative Example 2
[0070] Based on Example 1, the difference is that in the formula components, the first ethylene vinyl acetate in the strip material is replaced by thermoplastic polyester elastomer TPEE.
[0071] Comparative Example 3
[0072] Based on Example 1, the difference is that in the formula components, neither the surrounding strip material nor the belly filling material includes the component of hydrogenated styrene-butadiene block copolymer.
[0073] The foamed midsoles prepared in the above-mentioned embodiments 1, 2, 3 and comparative examples 1, 2, 3 were inspected by visual and tactile means. The foamed midsoles prepared in embodiments 1, 2, 3 were basically free of deformation, and the boundary between the strip and the filling belly was clear and without cracks; the foamed midsoles prepared in comparative example 1 had a certain degree of deformation, and cracks appeared at the junction of the strip and the filling belly; the foamed midsoles prepared in comparative example 2 had a greater degree of deformation than comparative example 1, and a larger degree of cracks appeared at the junction of the strip and the filling belly; the foamed midsoles prepared in comparative example 3 had a certain degree of deformation, and a certain degree of cracks appeared at the junction of the strip and the filling belly. After inspection, it can be seen that compared with embodiments 1, 2, 3, comparative examples 1, 2, 3 all had different degrees of deformation and cracking, which shows that the preparation method of the multi-material foamed midsole provided by the present invention can improve the deformation and cracking of the junction of the midsole with multiple materials after synchronous foaming.
[0074] The description of the above specification and embodiments is used to explain the protection scope of the present invention, but does not constitute a limitation on the protection scope of the present invention. Through the enlightenment of the present invention or the above embodiments, ordinary technicians in this field can obtain modifications, equivalent substitutions or other improvements to the embodiments of the present invention or part of the technical features thereof through logical analysis, reasoning or limited experiments, which should be included in the protection scope of the present invention.
Claims
1. A method for preparing a multi-material foam midsole, characterized in that: The following steps are involved: Preparation of strip material: knead the following components by weight at 115±5°C for 10-15min: 40-50 parts of the first ethylene vinyl acetate copolymer, 10-15 parts of the second ethylene vinyl acetate copolymer, 20-25 parts of the polyolefin elastomer, 10-20 parts of the hydrogenated styrene-butadiene block copolymer, 2-10 parts of EPDM rubber, 0.2-0.5 parts of the active agent, and 4-8 parts of the low-temperature foaming agent; then add the following auxiliary agents by weight, 0.5-1 parts, and cross-linking agent, and knead at 120±5°C for 10-15min; Preparation of abdominal filling material: kneading the following components by weight at 115±5°C for 10-15min: 20-30 parts of a first ethylene-vinyl acetate copolymer, 25-30 parts of a second ethylene-vinyl acetate copolymer, 15-20 parts of a polyolefin elastomer, 20-25 parts of a hydrogenated styrene-butadiene block copolymer, 2-5 parts of ethylene-propylene rubber, 9-10 parts of an anti-wear agent, 0.2-0.5 parts of an active agent, and 4-8 parts of a low-temperature foaming agent; then adding the following auxiliary agents by weight, 0.5-1 parts, and a cross-linking agent, and kneading at 120±5°C for 10-15min; Preparing a midsole embryo: injecting the mixed and molten strip material and the belly filling material into an embryo mold respectively, and surrounding the belly filling material with the strip material to form a strip portion and a belly filling respectively, so that the junction of the strip portion and the belly filling is bonded, and then cooling the midsole embryo; Foaming: placing the midsole embryo into a foaming mold, setting the mold temperature to 172±3°C, and evacuating the mold. After 7-8 minutes, the foaming is completed, taking out the foamed product and letting it stand and cool naturally at room temperature to obtain a foamed midsole; wherein the vinyl acetate (VA) content in the first ethylene-vinyl acetate copolymer is 26%, and the vinyl acetate (VA) content in the second ethylene-vinyl acetate copolymer is 33%.
2. The method for preparing a multi-material foamed midsole according to claim 1, characterized in that: The hydrogenated styrene-butadiene block copolymer adopts star-shaped SEBS with a molecular weight of 300,000 to 350,000.
3. The method for preparing a multi-material foamed midsole according to claim 2, characterized in that: The polyolefin elastomer grade is POE8003.
4. The method for preparing a multi-material foamed midsole according to claim 1, characterized in that: The active agent is stearic acid.
5. The method for preparing a multi-material foamed midsole according to claim 1, characterized in that: The anti-wear agent is an organic silicon anti-wear agent.
6. The method for preparing a multi-material foam midsole according to claim 1, characterized in that: The auxiliary agent is zinc carbonate.
7. The method for preparing a multi-material foamed midsole according to claim 1, characterized in that: The cross-linking agent is dicumyl peroxide.
8. The method for preparing a multi-material foamed midsole according to claim 1, characterized in that: The low-temperature foaming agent is white azodicarbonamide.
9. A multi-material foam sole, characterized in that: The multi-material foamed sole is obtained by using the foamed midsole obtained by the preparation method of the multi-material foamed midsole as described in any one of claims 1 to 8 as a raw material through a compression molding process; in the compression molding process, the mold heating time is 8-9 minutes, the mold heating temperature is 160±5°C, and the cooling time is 7-8 minutes.
Citation Information
Patent Citations
Manufacturing method of multi-color and multi-functional EVA sports and leisure sole
CN106750871A
High-comfort cushioning foaming insole material, preparation method thereof and sports shoes
CN111286110A
Soft and elastic composite foaming material with good touch feeling, preparation method thereof and shoe sole
CN116218126A
Method for manufacturing a semi-finished product, in particular a shoe sole and semi-finished product obtained
EP3949783A1
Lightweight outsole
KR1020140008872A