Integrally-formed composite sheet, preparation method thereof and composite hose
Through specific proportions of raw material components and drying, premixing, and melt blown film processes, the integrated molding of composite sheets is achieved, which solves the problems of complex preparation processes and introduction of harmful substances in traditional composite sheets, and improves barrier properties and mechanics. performance, simplifying the process and reducing costs.
Patent Information
- Application Number
- CN202410861148.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The preparation process of traditional composite sheets is complex, time-consuming and costly, and is prone to interlayer peeling and bubble problems, affecting performance and appearance quality, and the adhesives used may introduce harmful substances.
Using specific proportions of raw material components, such as low-density polyethylene, ethylene-vinyl alcohol copolymer, glyceryl monostearate, white carbon black, diethyl succinate, antioxidants and light stabilizers, through drying, Pre-mixed and melt-blown film processes enable one-piece molding, eliminating the need for adhesives.
The preparation process is simplified, the production cost and energy consumption are reduced, the barrier properties, mechanical properties and service life of the composite sheet are improved, the introduction of harmful substances is avoided, and the overall performance and appearance quality are significantly improved.
Smart Images

Figure BDA0004919200420000061 
Figure BDA0004919200420000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of packaging material production, and in particular to an integrally formed composite sheet material and a preparation method thereof, and a composite hose. Background Art
[0002] Plastic hoses are favored by daily chemical product manufacturers due to their portability and easy extrusion, and are widely used in the packaging of toiletries. Plastic hoses are generally made of plastic sheets, which are traditionally single-layer structures. However, in actual use, manufacturers have found that single-layer plastic sheets are difficult to meet the gas and liquid barrier performance requirements of toiletries. Therefore, currently, multiple layers of materials with different properties and types are usually combined together to form composite sheets.
[0003] Although composite sheets have better barrier properties than single-layer plastic sheets, traditional composite sheets usually adopt a multi-layer structure. During the preparation process, each layer of sheet needs to be made separately, and then they are bonded together with auxiliary materials such as adhesives to finally form a composite sheet. Due to the different properties of each layer of sheet, this preparation method is prone to problems such as interlayer peeling and bubbles, which will affect the overall performance and appearance quality of the composite sheet during subsequent use. At the same time, auxiliary materials such as adhesives used in the preparation process may introduce harmful substances, which is not good for health. In addition, the preparation process of this composite sheet is complicated, time-consuming, and energy-intensive, which increases production costs.
[0004] With the advancement of packaging technology and the improvement of environmental awareness, the demand for more efficient and environmentally friendly packaging materials is growing. Therefore, the development of an integrated composite sheet has important practical significance and application value. Summary of the invention
[0005] In order to reduce the production cost and production time of composite sheets, the present application provides an integrally formed composite sheet and its preparation method and composite hose. The present application realizes the integral forming of composite sheets by adopting raw material components of a specific ratio and a unique preparation method, which not only simplifies the preparation process and improves production efficiency, but also has barrier properties and mechanical properties comparable to traditional composite sheets, meeting the requirements of daily chemical products such as toiletries for packaging materials.
[0006] In the first aspect, the present application provides an integrally formed composite sheet material adopting the following technical solution: An integrally formed composite sheet, wherein the raw materials for preparing the composite sheet include the following components in parts by mass: 80-90 parts of low-density polyethylene, 5-10 parts of ethylene-vinyl alcohol copolymer, 2-3 parts of glyceryl monostearate, 2-4 parts of white carbon black, 1-3 parts of diethyl succinate, 1-2 parts of antioxidant, and 1-2 parts of light stabilizer.
[0007] In the above technical scheme, low-density polyethylene is used as the main substrate, which provides good mechanical properties and processing properties; ethylene-vinyl alcohol copolymer is used as a barrier layer, which has excellent barrier properties to gases and liquids; the synergistic effect of glyceryl monostearate, white carbon black and diethyl succinate effectively improves the heat resistance and weather resistance of the composite sheet, especially effectively enhances the compatibility between low-density polyethylene and ethylene-vinyl alcohol copolymer, and ethylene-vinyl alcohol copolymer can be more evenly dispersed in low-density polyethylene to form a stable composite structure inside the composite sheet, which significantly improves the barrier properties and mechanical properties of the composite sheet; the addition of antioxidants and light stabilizers helps to extend the service life of the composite sheet and maintain its good appearance and performance.
[0008] Preferably, the mass ratio of glyceryl monostearate, white carbon black and diethyl succinate is 2:(2-3):(1-2).
[0009] In the above technical scheme, this application further optimizes the mass ratio of glyceryl monostearate, white carbon black and diethyl succinate based on the key roles played by glyceryl monostearate, white carbon black and diethyl succinate in the composite sheet and the synergistic effect between them, and further improves the performance of the composite sheet. Glyceryl monostearate, as a plasticizer, can improve the flexibility and processing performance of the composite sheet; white carbon black, as a filler, not only improves the mechanical strength of the composite sheet, but also enhances its heat resistance and weather resistance; diethyl succinate plays a role in volume expansion and toughening, which helps to improve the compatibility and tear resistance of the composite sheet. Through a large number of experiments, the present application found that when the mass ratio of glyceryl monostearate, white carbon black and diethyl succinate is controlled at 2:(2-3):(1-2), the synergistic effect among glyceryl monostearate, white carbon black and diethyl succinate can be further enhanced, the compatibility of each component in the composite sheet can be improved, and the performance of the composite sheet can be further optimized, so that it has both excellent barrier properties and good mechanical properties.
[0010] Preferably, the antioxidant is antioxidant 1010 and antioxidant 168.
[0011] In the above technical solution, the present application selects a combination of antioxidant 1010 and antioxidant 168 as the antioxidant of the composite sheet, which can effectively improve the antioxidant performance of the composite sheet and meet the high requirements for the performance of the composite sheet in practical applications.
[0012] Preferably, the light stabilizer is UV-531.
[0013] In the above technical solution, the present application can effectively improve the light aging resistance of the composite sheet by selecting UV-531 as the light stabilizer of the composite sheet. UV-531 has excellent ability to absorb ultraviolet rays, which can significantly reduce the destructive effect of ultraviolet rays on the composite sheet, thereby extending the service life of the composite sheet. In addition, UV-531 also has good compatibility and processing performance, and can be fully mixed with other components of the composite sheet to ensure the stable performance of the composite sheet.
[0014] Preferably, the raw materials for preparing the integrally formed composite sheet further include 1-2 parts of amino silicone oil.
[0015] In the above technical solution, by adding amino silicone oil, the flexibility of the composite sheet can be further improved, its touch can be improved, and the user experience can be enhanced. As an excellent softener, amino silicone oil can penetrate into the molecular chain of the composite sheet, reduce the friction between molecules, and make the composite sheet softer and smoother. At the same time, amino silicone oil also has a certain lubricating effect, which can reduce the friction and wear of the composite sheet during processing and use, and extend its service life. In addition, glyceryl monostearate, white carbon black and diethyl succinate can make the amino silicone oil evenly dispersed in the composite sheet, maintaining the stable performance of the composite sheet.
[0016] Preferably, the ethylene molar content of the ethylene-vinyl alcohol copolymer is 32%.
[0017] In the above technical solution, the present application further improves the barrier properties of the composite sheet by selecting an ethylene-vinyl alcohol copolymer with an ethylene molar content of 32% as a component of the composite sheet. The ethylene molar content of the ethylene-vinyl alcohol copolymer has an important influence on its barrier properties. The ethylene-vinyl alcohol copolymer with an ethylene molar content of 32% has excellent barrier properties and can effectively protect the quality of packaged items. At the same time, this ethylene-vinyl alcohol copolymer also has good processing performance and compatibility, and can be fully mixed with other components of the composite sheet to achieve one-piece molding of the composite sheet.
[0018] In a second aspect, the present application provides a method for preparing an integrally formed composite sheet using the following technical solution: A method for preparing an integrally formed composite sheet comprises the following steps: Step 1: drying the formulated amount of ethylene-vinyl alcohol copolymer; Step 2: premixing the remaining raw materials in the formula with the ethylene-vinyl alcohol copolymer treated in step 1 at a high speed to obtain a premix; Step 3: After the premix is melted, it is subjected to a film blowing process to obtain an integrally formed composite sheet.
[0019] Preferably, the drying temperature of step 1 is 80-90°C, the drying time is 7-9h, and the melting temperature of step 3 is 190-210°C.
[0020] In the above technical scheme, the present application successfully prepares an integrally formed composite sheet through specific drying, premixing and melt blowing steps. First, the ethylene-vinyl alcohol copolymer is dried to effectively remove the moisture therein, avoid the generation of bubbles and other problems during the subsequent processing, and improve the quality and stability of the composite sheet. High-speed premixing can fully mix the components and provide uniform raw materials for subsequent melting and film blowing processes. Melting the premix at a temperature of 190-210°C can ensure the full melting and mixing of the components to form a uniform molten system, and the molten system can be prepared into an integrally formed composite sheet through a film blowing process. The entire preparation process is simple and efficient, without the use of auxiliary materials such as adhesives, which reduces production costs and energy consumption, improves production efficiency, and meets environmental protection and health requirements.
[0021] In a third aspect, the present application provides a composite hose using the following technical solution: A composite hose is prepared by using the composite sheet material as described in the first aspect.
[0022] In the above technical solution, the present application provides a composite hose, which is prepared by using the one-piece composite sheet of the present application. Due to the excellent performance and one-piece molding characteristics of the composite sheet, the prepared composite hose has excellent barrier properties, mechanical properties and appearance quality. At the same time, the preparation process of the composite hose is simple and fast, which reduces production costs and time costs and improves production efficiency. Therefore, the composite hose of the present application has broad application prospects and market potential in the field of packaging, and can be widely used in the packaging of food, medicine, cosmetics and other fields.
[0023] In summary, the present application includes at least one of the following beneficial technical effects: 1. The present application adds glyceryl monostearate, white carbon black and diethyl succinate to low-density polyethylene and ethylene-vinyl alcohol copolymer, and the three cooperate with each other to effectively enhance the compatibility between low-density polyethylene and ethylene-vinyl alcohol copolymer, improve the dispersibility of ethylene-vinyl alcohol copolymer in low-density polyethylene, and significantly improve the barrier properties of the composite sheet.
[0024] 2. This application further improves the antioxidant and light aging resistance of the composite sheet by selecting a combination of antioxidant 1010 and antioxidant 168 as an antioxidant and UV-531 as a light stabilizer. This enables the composite sheet to maintain good performance stability during long-term use and prolongs the service life of the packaged items.
[0025] 3. The present application further adds amino silicone oil to the composite sheet to further improve the flexibility of the composite sheet, improve its touch, and enhance the user experience. At the same time, the present application further found in the research that glyceryl monostearate, white carbon black and diethyl succinate can make the amino silicone oil evenly dispersed in the composite sheet, maintaining the stability of the performance of the composite sheet.
[0026] 4. This application successfully prepares an integrally formed composite sheet by optimizing the components and preparation process of the composite sheet. The composite sheet not only retains the excellent performance of each component, but also overcomes the problems of interlayer peeling and bubbles that are prone to occur in traditional multi-layer composite sheets, and significantly improves the overall performance and appearance quality of the composite sheet. At the same time, since no auxiliary materials such as adhesives are required during the preparation process, the possible introduction of harmful substances is avoided, and the environmental protection and health performance of the composite sheet is guaranteed. This integrally formed composite sheet not only has excellent performance, but also has a simple and environmentally friendly preparation process, and has important application value and market prospects. DETAILED DESCRIPTION
[0027] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0028] Example 1 An integrally formed composite sheet is prepared from raw materials including 90 kg of low-density polyethylene, 5 kg of ethylene-vinyl alcohol copolymer, 3 kg of glyceryl monostearate, 4 kg of white carbon black, 3 kg of diethyl succinate, 1 kg of antioxidant, and 1 kg of light stabilizer.
[0029] The low-density polyethylene was LDPE 2420H purchased from CNOOC and Shell Petrochemical Co., Ltd.
[0030] The ethylene-vinyl alcohol copolymer is EVOH T102 purchased from Kuraray Co., Ltd. of Japan, and has an ethylene molar content of 32%.
[0031] Among them, glyceryl monostearate was purchased from Liaocheng Ruijie Chemical Co., Ltd., referred to as monoglyceride GMS.
[0032] Among them, the silica was OCI fumed silica K200 purchased from Dongyang, South Korea.
[0033] Among them, diethyl succinate was purchased from Shanghai Guyan Industrial Co., Ltd., CAS No.: 123-25-1.
[0034] The antioxidant is compounded by antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.
[0035] Among them, antioxidant 1010 and antioxidant 168 are from BASF of Germany.
[0036] Among them, the light stabilizer is UV-531.
[0037] Among them, UV-531 is the ultraviolet absorber UV-531 purchased from Nanjing Milan New Materials Co., Ltd.
[0038] The method for preparing the integrally formed composite sheet comprises the following steps: Step 1: Dry the ethylene-vinyl alcohol copolymer at 80°C for 9 hours.
[0039] Step 2: Premixing low-density polyethylene, glyceryl monostearate, white carbon black, diethyl succinate, antioxidant, light stabilizer and the ethylene-vinyl alcohol copolymer treated in step 1 at high speed to obtain a premix.
[0040] Step 3: After the premix is melted at 210° C., a film blowing process is performed to obtain an integrally formed composite sheet with a thickness of 200 μm.
[0041] Example 2 An integrally formed composite sheet, which is different from Example 1 in that the raw materials include 80kg of low-density polyethylene, 10kg of ethylene-vinyl alcohol copolymer, 2kg of glyceryl monostearate, 2kg of white carbon black, 2kg of diethyl succinate, 2kg of antioxidant, and 2kg of light stabilizer.
[0042] The method for preparing the integrally formed composite sheet comprises the following steps: Step 1: Dry the ethylene-vinyl alcohol copolymer at 90°C for 7h.
[0043] Step 2: Premixing low-density polyethylene, glyceryl monostearate, white carbon black, diethyl succinate, antioxidant, light stabilizer and the ethylene-vinyl alcohol copolymer treated in step 1 at high speed to obtain a premix.
[0044] Step 3: After the premix is melted at 190° C., a film blowing process is performed to obtain an integrally formed composite sheet with a thickness of 200 μm.
[0045] Example 3 An integrally formed composite sheet, which is different from Example 1 in that the raw materials for preparation include 85kg of low-density polyethylene, 8kg of ethylene-vinyl alcohol copolymer, 2kg of glyceryl monostearate, 3kg of white carbon black, 1kg of diethyl succinate, 1.5kg of antioxidant, and 1.5kg of light stabilizer.
[0046] The method for preparing the integrally formed composite sheet comprises the following steps: Step 1: Dry the ethylene-vinyl alcohol copolymer at 85°C for 8h.
[0047] Step 2: Premixing low-density polyethylene, glyceryl monostearate, white carbon black, diethyl succinate, antioxidant, light stabilizer and the ethylene-vinyl alcohol copolymer treated in step 1 at high speed to obtain a premix.
[0048] Step 3: After the premix is melted at 200° C., a film blowing process is performed to obtain an integrally formed composite sheet with a thickness of 200 μm.
[0049] Example 4 An integrally formed composite sheet, which is different from Example 1 in that the preparation raw materials also include 1 kg of amino silicone oil.
[0050] Among them, amino silicone oil (ASO) was purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd.
[0051] The method for preparing the integrally formed composite sheet comprises the following steps: Step 1: Dry the ethylene-vinyl alcohol copolymer at 80°C for 9 hours.
[0052] Step 2: Premix low-density polyethylene, glyceryl monostearate, white carbon black, diethyl succinate, antioxidant, light stabilizer, amino silicone oil and the ethylene-vinyl alcohol copolymer treated in step 1 at high speed to obtain a premix.
[0053] Step 3: After the premix is melted at 210° C., a film blowing process is performed to obtain an integrally formed composite sheet with a thickness of 200 μm.
[0054] Example 5 An integrally formed composite sheet, which is different from Example 4 in that the amount of amino silicone oil added is 2 kg.
[0055] Comparative Example 1 An integrally formed composite sheet, which is different from Example 1 in that it does not contain glyceryl monostearate.
[0056] Comparative Example 2 An integrally formed composite sheet, which is different from Example 1 in that it does not contain white carbon black.
[0057] Comparative Example 3 An integrally formed composite sheet, which is different from Example 1 in that it does not contain diethyl succinate.
[0058] Comparative Example 4 An integrally formed composite sheet, which is different from Example 1 in that it does not contain glyceryl monostearate, white carbon black and diethyl succinate.
[0059] Comparative Example 5 An integrally formed composite sheet, which is different from Example 5 in that it does not contain glyceryl monostearate, white carbon black and diethyl succinate.
[0060] Performance Testing Test samples: composite sheets of the above embodiments and comparative examples.
[0061] According to GB / T1040.3-2006 standard, tensile strength and elongation at break are tested.
[0062] According to GB / T29336-2012 standard, the oxygen transmission rate is tested for 24 hours at standard atmospheric pressure and relative humidity of 65%-75%.
[0063] According to GB / T29336-2012 standard, a moisture permeability meter is used to test the water vapor transmission rate for 24 hours under standard atmospheric pressure and an ambient relative humidity of 90%.
[0064] The above test results are shown in Table 1.
[0065] Table 1: Combining Examples 1-5, Comparative Examples 1-5 and Table 1, it is not difficult to see that Examples 1-5 have better barrier properties and mechanical properties.
[0066] Specifically combining the analysis of Example 1 and Comparative Examples 1-4, it is not difficult to see that the difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not add glyceryl monostearate, the difference between Comparative Example 2 and Example 1 is that Comparative Example 2 does not add white carbon black, the difference between Comparative Example 3 and Example 1 is that Comparative Example 3 does not add diethyl succinate, and the mechanical properties and barrier properties of Example 1 are better. It can be seen that the synergistic effect between glyceryl monostearate, white carbon black and diethyl succinate can effectively improve the barrier properties and mechanical properties of the composite sheet. The applicant specifically analyzed that this is because glyceryl monostearate, white carbon black and diethyl succinate can synergistically enhance the compatibility between low-density polyethylene and ethylene-vinyl alcohol copolymer, and improve the dispersibility of ethylene-vinyl alcohol copolymer in low-density polyethylene.
[0067] Specifically combining the analysis of Example 1 and Example 4-5, it is not difficult to see that the difference between Example 4-5 and Example 1 is that Example 4-5 adds amino silicone oil, and Example 4-5 has better mechanical properties. It can be seen that adding amino silicone oil to the composite sheet can further improve the flexibility of the composite sheet. Combined with the analysis of Comparative Example 5, compared with Example 5, Comparative Example 5 does not add glyceryl monostearate, white carbon black and diethyl succinate. The mechanical properties of Comparative Example 5 are to a certain extent not as good as those of Example 5 and Comparative Example 4. It can be seen that glyceryl monostearate, white carbon black and diethyl succinate can also promote the uniform dispersion of amino silicone oil in the composite sheet.
[0068] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An integrally formed composite sheet, characterized in that: The raw materials for preparing the composite sheet include the following components in parts by mass: 80-90 parts of low-density polyethylene, 5-10 parts of ethylene-vinyl alcohol copolymer, 2-3 parts of glyceryl monostearate, 2-4 parts of white carbon black, 1-3 parts of diethyl succinate, 1-2 parts of antioxidant, and 1-2 parts of light stabilizer.
2. The integrally formed composite sheet according to claim 1, characterized in that: The mass ratio of glyceryl monostearate, white carbon black and diethyl succinate is 2:(2-3):(1-2).
3. The integrally formed composite sheet according to claim 1, characterized in that: The antioxidants are antioxidant 1010 and antioxidant 168.
4. The integrally formed composite sheet according to claim 1, characterized in that: The light stabilizer is UV-531.
5. The integrally formed composite sheet according to claim 1, characterized in that: The raw materials for preparing the integrally formed composite sheet also include 1-2 parts of amino silicone oil.
6. A method for preparing an integrally formed composite sheet according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: drying the formulated amount of ethylene-vinyl alcohol copolymer; Step 2: premixing the remaining raw materials in the formula with the ethylene-vinyl alcohol copolymer treated in step 1 at a high speed to obtain a premix; Step 3: After the premix is melted, it is subjected to a film blowing process to obtain an integrally formed composite sheet.
7. The method for preparing an integrally formed composite sheet according to claim 6, characterized in that: The drying temperature of step 1 is 80-90°C, the drying time is 7-9h, and the melting temperature of step 3 is 190-210°C.
8. A composite hose, characterized in that: The composite hose is made of the composite sheet material as described in any one of claims 1 to 5.
Citation Information
Patent Citations
Polyester blends with improved stress whitening for film and sheet applications
CN101056938A
Plastic profiled bar decorative layer combination material with metal-like natural texture, preparation method and application thereof
CN101717554A
High-barrier material, plastic pipe with high barrier property and preparation method
CN111808351A
PVC product and preparation method thereof
CN115612227A
Anti-yellowing ethylene-vinyl alcohol copolymer (EVOH) and preparation method thereof
CN118146603A