Hydrophobic anti-icing filler based on thermosetting polymer waste and application of hydrophobic anti-icing filler in coating

Through alkali pretreatment and phytic acid impregnation of melamine formaldehyde sponge, a hollow carbon material with a neuron-like network structure is formed. Combined with other materials, the problem of poor interfacial compatibility in hydrophobic anti-icing coatings is solved and the mechanical stability of the coating is achieved. Improved anti-icing and hydrophobic properties provide effective anti-icing effects and environmentally friendly coating solutions.

CN118791900APending Publication Date: 2024-10-18SHENYANG SHUNFENG NEW MATERIAL CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411226087.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The poor interfacial compatibility between inorganic nanoparticles and organic polymers in existing hydrophobic anti-icing coatings results in poor mechanical properties of the coating, and thermosetting polymer waste cannot be effectively utilized, causing environmental pollution.

Method used

By performing alkali pretreatment and phytic acid impregnation on melamine formaldehyde sponge, a hollow carbon material with a neuron network structure is formed, and combined with hydroxyl polyurethane-modified acrylic and isocyanate curing agents, a coating with excellent mechanical stability and hydrophobic anti-icing properties is prepared. .

Benefits of technology

It achieves high mechanical stability and hydrophobic properties of the coating, provides passive and active anti-icing effects through low surface energy and dielectric loss effects, and improves the chemical stability and environmental friendliness of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791900A_ABST
    Figure CN118791900A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of building coatings, and relates to a hydrophobic anti-icing filler based on thermosetting polymer waste and application of the hydrophobic anti-icing filler in coatings. According to the preparation method, firstly, the melamine formaldehyde sponge is subjected to alkali pretreatment, the surface and the interior of the melamine formaldehyde sponge are impregnated with phytic acid, the phytic acid loaded on the surface can promote a compact carbon layer micro-nano coarse structure and prevent pyrolysis gas from escaping, and the phytic acid loaded on the interior can catalyze pyrolysis to generate gas so as to expand a framework; therefore, the hollow carbon material with the neuron-like network structure is obtained under the combined action of internal blowing and surface plugging. The high-temperature inert carbon material provides low surface energy, the neuron-like structure forms a micro-nano structure, and the dielectric loss effect formed by the neuron-like structure promotes the conversion from electromagnetic waves in the air to heat energy, so that the active and passive composite hydrophobic anti-icing building coating is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building coatings and relates to a hydrophobic anti-icing filler based on thermosetting polymer waste and application of the filler in coatings. Background Art

[0002] The market size of architectural coatings in my country in 2024 is about 400 billion yuan, and architectural coatings account for about 40%, with great demand in the industry. Hydrophobic anti-icing architectural coatings are a special type of coating that prevents the adhesion of water and ice by forming a hydrophobic protective film on the surface of the building. This type of coating usually contains special chemical ingredients, such as silane, fluorocarbon, etc., which can reduce surface tension and make it difficult for water droplets to stay on the surface, thereby reducing the formation of ice and the accumulation of snow. Hydrophobic anti-icing coatings are widely used in outdoor facilities such as bridges, roads, and roofs to improve their safety and durability in severe weather conditions. With the development of technology, this type of coating is also constantly innovating to meet a wider range of application needs and environmental protection standards. The main fillers of hydrophobic anti-icing architectural coatings are inorganic micro / nanoparticles, which can construct the rough structure and low surface energy characteristics required for the coating. The poor interfacial compatibility between inorganic nanoparticles and organic polymers can lead to phase separation and agglomeration of nanofillers, thereby weakening the mechanical stability of the coating.

[0003] Melamine formaldehyde sponge (MS), commonly known as melamine sponge, is a material composed of melamine-formaldehyde polymer with an open honeycomb structure interconnected with struts. It is a thermosetting polymer waste. Global microplastic emissions from the consumption of cleaning sponges will reach 4.9 trillion. These microplastics may enter the food chain, posing potential risks to the environment and human health.

[0004] In view of the problem that the poor interface compatibility of the above-mentioned thermosetting polymer waste and nanofillers in the coating leads to poor mechanical properties of the coating, the present invention comprehensively utilizes the waste melamine formaldehyde sponge to prepare a building coating with excellent mechanical properties and hydrophobic and anti-icing properties, providing ideas for the functionalization and specialization of building coatings. Summary of the invention

[0005] In view of the above technical problems, the present invention provides a method for preparing a hydrophobic anti-icing filler and a coating thereof based on the comprehensive utilization of thermosetting polymer waste. The present invention first performs an alkali pretreatment on the melamine formaldehyde sponge, and phytic acid is impregnated on its surface and interior. The phytic acid loaded on the surface can promote a dense carbon layer-type micro-nano rough structure and prevent the escape of pyrolysis gas, while the phytic acid loaded inside can catalyze pyrolysis to produce gas to expand the skeleton, thereby obtaining a hollow carbon material with a neuron-like network structure under the combined action of internal "blowing" and surface "sealing". The high-temperature inert carbon material provides low surface energy, the neuron-like structure constitutes a micro-nano structure, and the dielectric loss effect formed by it promotes the conversion of electromagnetic waves in the air into thermal energy, forming an active and passive composite hydrophobic anti-icing building coating.

[0006] The present invention is achieved through the following technical solutions.

[0007] A hydrophobic anti-icing filler based on thermosetting polymer waste, comprising the following raw materials in parts by weight: 80-120 parts of alkalized melamine formaldehyde sponge, 3-4 parts of phytic acid, and 100-150 parts of distilled water.

[0008] A method for preparing a hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: Step 1, drying the alkalized melamine formaldehyde sponge at 80-90°C for 12 h, and dissolving phytic acid in distilled water under magnetic stirring at 500-600 r / min; Step 2, then, after magnetic stirring at 500-600 r / min for 120-150 min, ultrasonic treatment for 60-80 min, the phytic acid solution is impregnated on the alkalized melamine formaldehyde sponge; Step 3. Finally, the impregnated sample was vacuum dried at 60 °C overnight and pyrolyzed at 900 °C for 120-150 min at a rate of 5 °C / min in a nitrogen atmosphere to obtain a hollow carbon material with a neuron-like network structure, i.e., a hydrophobic anti-icing filler.

[0009] Furthermore, the preparation steps of the alkalized melamine formaldehyde sponge in step 1 are: ultrasonically cleaning the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immersing the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30 to 50 minutes, and washing with deionized water to obtain the alkalized melamine formaldehyde sponge.

[0010] Furthermore, the volume specification of the melamine formaldehyde sponge treated with alkalization in step 1 is (4cm×2cm×2cm).

[0011] A coating prepared using the above hydrophobic anti-icing filler, the specific steps are as follows: 80-120 parts of the obtained hollow carbon material, 8-12 parts of hydroxyl polyurethane modified acrylic dispersion, and 2-3 parts of isocyanate curing agent are stirred into liquid to obtain a coating; the coating is applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

[0012] Furthermore, the weight ratio of the isocyanate curing agent to the hydroxy polyurethane modified acrylic dispersion is 1:4.

[0013] Compared with the prior art, the beneficial effects of the present invention are as follows.

[0014] 1: Use waste thermosetting polymers to form a structure through carbonization as fillers for the coating. The interfacial strength between polymers is higher than that between inorganic fillers and water-based coatings, which makes the coating have excellent mechanical stability. The cross-linked network structure between polymers steadily improves the chemical stability.

[0015] 2: Single substance phytic acid is used for double-sided regulation. The phytic acid loaded on the surface can promote a dense carbon layer-like micro-nano rough structure and prevent the escape of pyrolysis gas, while the phytic acid loaded inside can catalyze pyrolysis to produce gas to expand the skeleton, thereby obtaining a hollow carbon material with a neuron-like network structure under the combined action of internal "blowing" and surface "sealing".

[0016] 3: The hollow carbon material filler with a neuron-like network structure formed after carbonization has a low surface energy effect under high temperature, forming a micro-nano rough structure, which provides an effective method for passive hydrophobic deicing. The hollow carbon material with a neuron-like network structure produces a dielectric loss effect with electromagnetic waves in the air, converting electromagnetic waves into heat energy, which provides an effective effect for active deicing. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Static water contact angles of coatings prepared using the fillers of Examples and Comparative Examples. DETAILED DESCRIPTION

[0018] In order to make those skilled in the art better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. These embodiments should be understood to be only used to illustrate the present invention and not to limit the protection scope of the present invention. After reading the contents recorded in the present invention, all other embodiments obtained after various changes or modifications made to the present invention based on the technical solution and embodiments of the present invention also fall within the scope of protection of the claims of the present invention.

[0019] A hydrophobic anti-icing filler based on thermosetting polymer waste, comprising the following raw materials in parts by weight: 80-120 parts of alkalized melamine formaldehyde sponge, 3-4 parts of phytic acid, and 100-150 parts of distilled water.

[0020] A method for preparing a hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: Step 1, drying the alkalized melamine formaldehyde sponge at 80-90°C for 12 h, and dissolving phytic acid in distilled water under magnetic stirring at 500-600 r / min; Step 2, then, after magnetic stirring at 500-600 r / min for 120-150 min, ultrasonic treatment for 60-80 min, the phytic acid solution is impregnated on the alkalized melamine formaldehyde sponge; Step 3. Finally, the impregnated sample was vacuum dried at 60 °C overnight and pyrolyzed at 900 °C for 120-150 min at a rate of 5 °C / min in a nitrogen atmosphere to obtain a hollow carbon material with a neuron-like network structure, i.e., a hydrophobic anti-icing filler.

[0021] Furthermore, the preparation steps of the alkalized melamine formaldehyde sponge in step 1 are: ultrasonically cleaning the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immersing the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30 to 50 minutes, and washing with deionized water to obtain the alkalized melamine formaldehyde sponge.

[0022] Furthermore, the volume specification of the melamine formaldehyde sponge treated with alkalization in step 1 is (4cm×2cm×2cm).

[0023] A coating prepared using the above hydrophobic anti-icing filler, the specific steps are as follows: 80-120 parts of the obtained hollow carbon material, 8-12 parts of hydroxyl polyurethane modified acrylic dispersion, and 2-3 parts of isocyanate curing agent are stirred into liquid to obtain a coating; the coating is applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

[0024] Furthermore, the weight ratio of the isocyanate curing agent to the hydroxy polyurethane modified acrylic dispersion is 1:4.

[0025] Example 1.

[0026] The preparation steps of the alkalized melamine formaldehyde sponge are as follows: ultrasonically clean the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immerse 80 parts of the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30-50 min, and wash with deionized water to obtain 80 parts of the alkalized melamine formaldehyde sponge.

[0027] A hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: 80 parts of alkalized melamine formaldehyde sponge were dried at 80 °C for 12 h. 3 parts of phytic acid were dissolved in 100 parts of distilled water under magnetic stirring at 500-600 r / min, and then the phytic acid solution was impregnated on the alkalized melamine formaldehyde sponge after magnetic stirring at 500-600 r / min for 120 min and ultrasonic treatment for 60 min. Finally, the impregnated sample was vacuum dried overnight at 60 °C. The hollow carbon material with a neuron-like network structure was obtained by pyrolysis at 900 °C for 120 min at a rate of 5 °C / min in a nitrogen atmosphere.

[0028] A coating prepared using the above hydrophobic anti-icing filler, the specific steps are as follows: 80 parts of the obtained hollow carbon material, 8 parts of hydroxyl polyurethane modified acrylic dispersion, and 2 parts of isocyanate curing agent were stirred into a liquid, applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

[0029] Example 2.

[0030] The preparation steps of the alkalized melamine formaldehyde sponge are as follows: ultrasonically cleaning the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immersing 100 parts of the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30-50 min, and washing with deionized water to obtain 100 parts of the alkalized melamine formaldehyde sponge.

[0031] A hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: 100 parts of alkalized melamine formaldehyde sponge were dried at 80 °C for 12 h. 3 parts of phytic acid were dissolved in 100 parts of distilled water under magnetic stirring at 500-600 r / min, and then the phytic acid solution was impregnated on the alkalized melamine formaldehyde sponge after magnetic stirring at 500-600 r / min for 120 min and ultrasonic treatment for 60 min. Finally, the impregnated sample was vacuum dried overnight at 60 °C. The hollow carbon material with a neuron-like network structure was obtained by pyrolysis at 900 °C for 120 min at a rate of 5 °C / min in a nitrogen atmosphere.

[0032] A coating prepared using the above hydrophobic anti-icing filler, the specific steps are as follows: 80 parts of the obtained hollow carbon material, 8 parts of hydroxyl polyurethane modified acrylic dispersion, and 2 parts of isocyanate curing agent were stirred into a liquid, applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

[0033] Example 3.

[0034] The preparation steps of the alkalized melamine formaldehyde sponge are as follows: ultrasonically clean the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immerse 120 parts of the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30-50 min, and wash with deionized water to obtain 120 parts of the alkalized melamine formaldehyde sponge.

[0035] A hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: 120 parts of alkalized melamine formaldehyde sponge were dried at 80 °C for 12 h. 3 parts of phytic acid were dissolved in 100 parts of distilled water under magnetic stirring at 500-600 r / min, and then the phytic acid solution was impregnated on the alkalized melamine formaldehyde sponge after magnetic stirring at 500-600 r / min for 120 min and ultrasonic treatment for 60 min. Finally, the impregnated sample was vacuum dried overnight at 60 °C. The hollow carbon material with a neuron-like network structure was obtained by pyrolysis at 900 °C for 120 min at a rate of 5 °C / min in a nitrogen atmosphere.

[0036] A coating prepared using the above hydrophobic anti-icing filler, the specific steps are as follows: 80 parts of the obtained hollow carbon material, 8 parts of hydroxyl polyurethane modified acrylic dispersion, and 2 parts of isocyanate curing agent were stirred into a liquid, applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

[0037] Comparative example 1.

[0038] The preparation steps of the alkalized melamine formaldehyde sponge are as follows: ultrasonically clean the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immerse 80 parts of the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30-50 min, and wash with deionized water to obtain 80 parts of the alkalized melamine formaldehyde sponge.

[0039] A hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: 80 parts of alkalized melamine formaldehyde sponge were dried at 80 °C for 12 h and pyrolyzed at 900 °C for 120 min at a rate of 5 °C / min in a nitrogen atmosphere to obtain the carbon material.

[0040] A coating prepared using the above hydrophobic anti-icing filler, the specific steps are as follows: 80 parts of the obtained carbon material, 8 parts of hydroxyl polyurethane modified acrylic dispersion, and 2 parts of isocyanate curing agent were stirred into a liquid, applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

[0041] Comparative example 2.

[0042] The preparation steps of the alkalized melamine formaldehyde sponge are as follows: ultrasonically clean the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immerse 180 parts of the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30-50 min, and wash with deionized water to obtain 180 parts of the alkalized melamine formaldehyde sponge.

[0043] A hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: 180 parts of alkalized melamine formaldehyde sponge were dried at 80 °C for 12 h. 3 parts of phytic acid were dissolved in 100 parts of distilled water under magnetic stirring at 500-600 r / min, and then the phytic acid solution was impregnated on the alkalized melamine formaldehyde sponge after magnetic stirring at 500-600 r / min for 120 min and ultrasonic treatment for 60 min. Finally, the impregnated sample was vacuum dried overnight at 60 °C. The hollow carbon material with a neuron-like network structure was obtained by pyrolysis at 900 °C for 120 min at a rate of 5 °C / min in a nitrogen atmosphere.

[0044] A coating prepared using the above hydrophobic anti-icing filler, the specific steps are as follows: 80 parts of the obtained hollow carbon material, 8 parts of hydroxyl polyurethane modified acrylic dispersion, and 2 parts of isocyanate curing agent were stirred into a liquid, applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

[0045] Comparative example 3.

[0046] The preparation steps of the alkalized melamine formaldehyde sponge are as follows: ultrasonically clean the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immerse 60 parts of the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30-50 min, and wash with deionized water to obtain 60 parts of the alkalized melamine formaldehyde sponge.

[0047] A hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: 60 parts of alkalized melamine formaldehyde sponge were dried at 80 °C for 12 h. 3 parts of phytic acid were dissolved in 100 parts of distilled water under magnetic stirring at 500-600 r / min, and then the phytic acid solution was impregnated on the alkalized melamine formaldehyde sponge after magnetic stirring at 500-600 r / min for 120 min and ultrasonic treatment for 60 min. Finally, the impregnated sample was vacuum dried overnight at 60 °C. The hollow carbon material with a neuron-like network structure was obtained by pyrolysis at 900 °C for 120 min at a rate of 5 °C / min in a nitrogen atmosphere.

[0048] A hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste comprises the following steps: 80 parts of the obtained hollow carbon material, 8 parts of hydroxyl polyurethane modified acrylic dispersion, and 2 parts of isocyanate curing agent were stirred into a liquid, applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

[0049] Test: The deicing effect of the coating is quantitatively characterized by the hydrophobic angle of the coating. When the static water contact angle of the coating surface is greater than 150°, the coating is considered to have excellent hydrophobic and anti-icing effect. Therefore, we dripped 1μL of water on the surface of 6 groups of samples and observed their static contact angles.

[0050] Results and Discussion The static water contact angles of Example 1, Example 2 and Example 3 are all greater than 150°. This is because the homemade neuron-like carbon material forms a micro-nano rough structure in the coating that is conducive to superhydrophobicity. Furthermore, the high temperature and low surface energy cause the coating to have excellent superhydrophobic properties, thereby achieving the purpose of passive anti-icing. The dielectric loss formed is converted into heat energy to achieve the purpose of active anti-icing.

[0051] Comparative Example 1 is a self-made neuron-like carbon material, and only waste thermosetting polymer is added. The coating does not have a substance with low surface energy change, nor can it form an effective hydrophobic rough structure, and dielectric loss cannot occur, which results in the static contact angle of the coating of Comparative Example 1 reaching only 73°, which belongs to the hydrophilic category.

[0052] Comparative Examples 2 and 3 are melamine formaldehyde sponges with excessive and small amounts of alkalized treatment, respectively. Both are less than 150° and greater than 90°, achieving hydrophobic but not super-hydrophobic effects. This is because higher or lower than the formula dosage will lead to changes in the rough structure, and the accumulation or absence of neuron-like carbon materials in the coating will cause the super-hydrophobic performance of the coating to decrease, and the hydrophobic and anti-icing effect cannot be achieved.

Claims

1. A hydrophobic anti-icing filler based on thermosetting polymer waste, It is characterized in that Including the following raw materials by mass: 80-120 parts of alkalized melamine formaldehyde sponge, 3-4 parts of phytic acid, and 100-150 parts of distilled water.

2. A method for preparing a hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste, It is characterized in that The following steps are involved: Step 1, drying the alkalized melamine formaldehyde sponge at 80-90°C for 12 h, and dissolving phytic acid in distilled water under magnetic stirring at 500-600 r / min; Step 2, then, after magnetic stirring at 500-600 r / min for 120-150 min, ultrasonic treatment for 60-80 min, the phytic acid solution is impregnated on the alkalized melamine formaldehyde sponge; Step 3. Finally, the impregnated sample was vacuum dried at 60 °C overnight and pyrolyzed at 900 °C for 120-150 min at a rate of 5 °C / min in a nitrogen atmosphere to obtain a hollow carbon material with a neuron-like network structure, i.e., a hydrophobic anti-icing filler.

3. The method for preparing the hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste according to claim 2, It is characterized in that In step 1, the preparation steps of the alkalized melamine formaldehyde sponge are: ultrasonically cleaning the melamine formaldehyde sponge with ultrapure water and ethanol respectively, then immersing the cleaned melamine formaldehyde sponge in 5 parts of NaOH for 30 to 50 minutes, and washing with deionized water to obtain the alkalized melamine formaldehyde sponge.

4. The method for preparing a hydrophobic anti-icing filler based on comprehensive utilization of thermosetting polymer waste according to claim 2, It is characterized in that In the step 1, the volume specification of the melamine formaldehyde sponge treated with alkalization is (4 cm×2 cm×2 cm).

5. A coating prepared using the hydrophobic anti-icing filler according to any one of claims 1 to 4, It is characterized in that The specific steps are as follows: 80-120 parts of the obtained hollow carbon material, 8-12 parts of hydroxyl polyurethane modified acrylic dispersion, and 2-3 parts of isocyanate curing agent are stirred into liquid to obtain a coating; the coating is applied to an asbestos-free fiberboard using an air pump spray gun, and waited for 12 hours at 25°C to cure into a coating.

6. The coating according to claim 5, It is characterized in that The weight ratio of the isocyanate curing agent to the hydroxy polyurethane modified acrylic dispersion is 1:4.

Citation Information

Patent Citations

  • Preparation method of porous hydrophobic oleophylic sponge

    CN104163934A

  • One-step preparation method and use of PDMS-constructed super-hydrophobic melamine sponge carbon material

    CN107159129A

  • Preparation method of porous graphitized hollow carbon microsphere

    CN110980719A

  • Biomass-based multifunctional photo-thermal protective coating with photo-thermal temperature rise function and preparation method of biomass-based multifunctional photo-thermal protective coating

    CN114350259A