Wire rod for processing high-strength cold-drawn steel wire and manufacturing method thereof

By rationally designing the chemical composition and manufacturing process in the wire rod, a sorbite lamellar structure with high strength and high plastic toughness is formed, which solves the problem of difficulty in balancing strength and plastic toughness in the existing technology, and achieves high strength and high torsion. Performance galvanized steel wire production, reducing costs.

CN118792573AActive Publication Date: 2024-10-18BAOSHAN IRON & STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310400179.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-18
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

It is difficult to improve the strength and plastic toughness of the wire rod at the same time with the existing technology, and the production cost is high, so it cannot meet the requirements of high strength and high torsional performance.

Method used

Through reasonable chemical composition design, wire rods containing elements such as C, Si, Mn, Cr, V, Nb, W, Al, O, etc. adopt simple manufacturing processes, including smelting, billet casting, heating, wire rod The rolling and Stelmer air-cooling processes control the content and structure of carbon, Si, Mn and other elements to form a good sorbite lamellar structure.

Benefits of technology

It achieves both high strength and high plastic toughness, with a tensile strength of ≥1400MPa, an area shrinkage of ≥30%, and a tensile strength of ≥2100MPa and a torsion value of ≥12 times in galvanized steel wire, reducing production costs. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004179172640000071
    Figure BDA0004179172640000071
  • Figure BDA0004179172640000081
    Figure BDA0004179172640000081
  • Figure BDA0004179172640000082
    Figure BDA0004179172640000082
Patent Text Reader

Abstract

The invention discloses a wire rod for processing a high-strength cold-drawn steel wire, which contains Fe and inevitable impurities, and further contains the following chemical elements in percentage by mass: 0.89-0.94% of C, 0.99-0.99% of S, 0.99-0.99% of Cr, 0.99-0.99% of Cr, 0.99- 0.70% to 1.20% of Si; 0.30% to 0.80% of Mn; 0.30% to 0.60% of Cr; 0.03% to 0.10% of V; 0.03% to 0.08% of Nb; w: 0.1 to 0.4%; 0.02 to 0.05 percent of Al; o: 0.0015% to 0.0035%; and 0.004% to 0.008% of N. Correspondingly, the invention further discloses a manufacturing method of the wire rod. Through reasonable chemical component design, the processing requirements of the 2100MPa high-strength and high-torsion galvanized steel wire can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a wire rod and a preparation method thereof, and in particular to a wire rod for cables and a preparation method thereof. Background Art

[0002] Wire rod is the raw material for producing high-strength steel wire and steel strand for bridge cables. Large-sized wire rod can be made into high-strength steel wire through drawing, galvanizing, stabilization and other processes. To complete the drawing process of large-reduction steel wire, wire rod must first have good drawing performance.

[0003] In addition, the improvement of steel wire strength grade also requires the continuous improvement of wire rod strength. Alloy strengthening and microstructure refinement are the two most effective means to improve wire rod strength. For example, by adopting high-carbon and high-silicon alloy composition design, the material strength is improved by increasing the C, Si and Mn elements in the wire rod, and the 0.87-0.92% carbon content material is developed to achieve the improvement of wire rod and steel wire strength.

[0004] Another important means to achieve strength improvement is to obtain a high sorbite structure of high carbon wire rod. At present, high sorbite transformation of wire rod is mainly achieved by controlled cooling after rolling, such as the Stelmor air cooling process, which water cools the wire rod after final rolling and then realizes the continuous sorbite structure transformation in the air cooling section. However, the Stelmor cooling process has the problems of insufficient cooling capacity and poor temperature uniformity when producing large-sized wire rods. In this regard, some existing technologies control the structure by heat treatment after hot rolling of wire rods. For example, the Chinese patent document with publication number CN107299280 and publication date January 16, 2018, titled "A steel for bridge cables with tensile strength ≥2100MPa and production method", has a chemical composition of Nb: 0.04-0.08%, Al: 0.16-0.20%, B: 0.001-0.0015%, Zr: 0.002-0.005%, with a high alloy content and great difficulty in smelting control. At the same time, after continuous casting, the steel must be stacked and slowly cooled in the chamber, the ingot must be cut longitudinally by flame, and then rolled into small square billets after reheating, and then rolled into wire rods, resulting in high production costs.

[0005] However, the current direct hot-rolled high-carbon wire rod cannot meet the requirements of both strength and high plasticity and toughness when the wire strength reaches above 1960MPa. It is necessary to perform offline isothermal treatment on the wire rod, or add a large amount of alloy elements, or produce large square billets by double rolling, etc., which makes quality control difficult and the production cost high.

[0006] Based on this, it is desired to provide a wire rod for high-strength cold-drawn steel wire processing and a manufacturing method thereof, which can produce a wire rod with both high strength and high plasticity and toughness by a relatively simple manufacturing process. Summary of the invention

[0007] One of the purposes of the present invention is to provide a wire rod for processing high-strength cold-drawn steel wire, which, through reasonable chemical composition design, can meet the processing requirements of 2100MPa high-strength and high-torsion performance galvanized steel wire with a simple production process.

[0008] In order to achieve the above object, the present invention provides a wire rod for processing high-strength cold-drawn steel wire, which contains Fe and inevitable impurities, and further contains the following chemical elements in the following mass percentages:

[0009] C: 0.89-0.94%;

[0010] Si: 0.70-1.20%;

[0011] Mn: 0.30-0.80%;

[0012] Cr: 0.30-0.60%;

[0013] V: 0.03-0.10%;

[0014] Nb: 0.03-0.08%;

[0015] W: 0.1-0.4%;

[0016] Al: 0.02-0.05%;

[0017] O: 0.0015-0.0035%;

[0018] N: 0.004-0.008%.

[0019] Furthermore, the present invention also provides a wire rod for processing high-strength cold-drawn steel wire, wherein the mass percentage of each chemical element is:

[0020] C: 0.89-0.94%;

[0021] Si: 0.70-1.20%;

[0022] Mn: 0.30-0.80%;

[0023] Cr: 0.30-0.60%;

[0024] V: 0.03-0.10%;

[0025] Nb: 0.03-0.08%;

[0026] W: 0.1-0.4%;

[0027] Al: 0.02-0.05%;

[0028] O: 0.0015-0.0035%;

[0029] N: 0.004-0.008%;

[0030] The balance is Fe and other inevitable impurities.

[0031] In the wire rod for high-strength cold-drawn steel wire processing of the present invention, the design principles of each chemical element are specifically described as follows:

[0032] C: The C element is a necessary chemical component to ensure the high strength of wire rods and galvanized steel wires. The C element content determines the volume fraction of cementite in the troostite structure of high-carbon wire rods. Increasing the carbon content in the wire rod is conducive to the formation of more cementite lamellae. The refined troostite lamellae structure has better deformation performance and work hardening performance, which is conducive to the improvement of steel wire strength during subsequent processing. Based on this, the present invention controls the carbon content to be above 0.89%. However, as the carbon content in the material increases, it will cause the segregation control during the smelting and continuous casting process to become more difficult, especially the formation of network cementite precipitated along the grain boundaries will sharply reduce the plastic toughness of the material. At the same time, after the carbon content increases, cementite spheroidization is prone to occur during the cooling process after rolling. Therefore, the present invention controls the upper limit of the carbon content to 0.94%.

[0033] Si: Si is often added to steel as a deoxidizer during the smelting process. At the same time, Si dissolved in the ferrite phase of the wire rod will significantly improve the strength of the material. In addition, in the present invention, Si will also be enriched at the interface between the ferrite phase and the cementite phase during the cooling phase transformation of the wire rod. During the lead bath degreasing and hot-dip galvanizing process of the steel wire drawn with a large area reduction rate, the enrichment of Si at the phase interface will slow down the decomposition of the large deformation cementite lamellae and reduce the loss of steel wire strength. Based on this, in order to ensure the high strength of the wire rod and the higher strength of the steel wire after drawing, the present invention controls the Si content to be higher than 0.7%. However, too high Si will significantly reduce the plasticity of the steel, embrittle the material, and split during the torsion process. Therefore, the present invention controls the Si content to be within the range of 0.70-1.20%.

[0034] Mn: Mn is also often added as a deoxidizer during the steelmaking process. At the same time, Mn is easy to combine with the harmful element S in the steel to form MnS, reducing its harm. Mn is also a commonly used strengthening element in steel, mainly playing the role of solid solution strengthening. The formed alloy cementite has higher strength, so the Mn content in the alloy needs to be controlled to be higher than 0.30%. However, for the present invention, when the Mn content is too high, it will increase the tendency of grain coarsening during the material heating process and increase the difficulty of controlling the cooling structure, especially when the C and Si contents in the material are high. Based on this, the present invention controls the addition amount of Mn element to be lower than 0.80%.

[0035] Cr: The present invention refines the lamellar structure of the troostite structure in the wire rod by adding the Cr element, and at the same time improves the strength of the cementite, thereby improving both the strength and plasticity of the material. Based on this, the present invention adds a Cr content higher than 0.30%. On the other hand, in order to prevent the occurrence of abnormal martensitic structure and reduce the difficulty of structure control, the Cr content is controlled to be lower than 0.60% because the cementite spheroidization tendency is stronger after the Cr content is increased.

[0036] W: The addition of W element in the present invention will be beneficial to the growth of cementite lamellae during the controlled rolling and cooling process of the wire rod. The dragging effect of W atoms will enhance the stability and toughness of the alloy cementite lamellae and reduce the proportion of degraded cementite. In order to give full play to the beneficial effects of W element, the present invention controls the W content to be higher than 0.1%. However, the addition of too much W element has a tendency to coarsen carbides. Therefore, the present invention controls the upper limit of the W content to 0.4%.

[0037] V, Nb, N: V and Nb elements are easy to combine with C and N to form nano-scale carbon and nitrogen precipitates, which are beneficial to refine the austenite structure and precipitation strengthening during the hot rolling process of the wire rod, especially when V and Nb are added in combination. The effect is more significant. For the present invention, grain refinement will increase the grain boundary area in the structure, provide more nucleation points for the transformation of the sorbite structure, facilitate the formation of a good lamellar sorbite lamellar structure, reduce the proportion of spherical and short rod-shaped degenerate cementite, and be beneficial to the improvement of the strength of the steel wire and the improvement of the torsional performance of the hot-rolled wire rod in the subsequent direct drawing process.

[0038] In order to control the nitrogen carbides of V and Nb elements to account for about 10% at a temperature of 1150° C., the composite carbonitrides of V, Nb and W are fully precipitated within a temperature range of 850-950° C., and prevent excessive V and Nb from promoting the nucleation growth of large-particle spheroidized carbides, the V addition range is controlled to be 0.03-0.10%, the Nb addition range is controlled to be 0.03-0.08%, and the N element content is controlled to be 0.004-0.008%.

[0039] Al and O: Al and O combine to form aluminum oxide. To give full play to the grain refining effect of Al, the present invention controls the Al content to be in the range of 0.02-0.05% and the O content to be higher than 0.0015%. To prevent excessive aluminum oxide from deteriorating the performance, the O content is controlled to be lower than 0.0035%.

[0040] Furthermore, in the wire rod for high-strength cold-drawn steel wire processing described in the present invention, the mass percentage of chemical elements also satisfies: (V+2Nb) / (C+100N)+W / C≥1 / 5, where each chemical element is substituted into the value before the percentage sign of the mass percentage of the corresponding chemical element.

[0041] In order to further better control the nitrogen carbides of V and Nb elements to account for about 10% at a temperature of 1150°C, the composite carbonitrides of V, Nb and W are fully precipitated within a temperature range of 850-950°C, and at the same time prevent excessive V and Nb from promoting the nucleation growth of large-particle spheroidized carbides, and control (V+2Nb) / (C+100N)+W / C≥1 / 5.

[0042] Furthermore, among other inevitable impurities in the wire rod for processing high-strength cold-drawn steel wire described in the present invention: Ti≤0.003%, P≤0.010%, S≤0.010%.

[0043] The inevitable impurities in the present invention are mainly P, S and Ti. Excessive content of P and S elements will increase the brittleness of the material, especially when segregation occurs. Therefore, in some embodiments of the present invention, the P content is controlled to be less than 0.010% and the S content is controlled to be less than 0.010%.

[0044] When the Ti content is too high, a large amount of carbonitrides will be formed in the steel, which is not conducive to the torsional performance and fatigue life of the steel wire. Therefore, in some embodiments of the present invention, the Ti content is controlled to be below 0.003%.

[0045] Furthermore, in the wire rod for processing high-strength cold-drawn steel wire described in the present invention, its microstructure includes sorbite pellets, and the size of the sorbite pellets ranges from 2 to 25 μm.

[0046] Furthermore, in the wire rod for processing high-strength cold-drawn steel wire described in the present invention, the volume proportion of spherical and short rod-shaped degenerate cementite in its microstructure is less than 0.5%.

[0047] Furthermore, in the wire rod for processing high-strength cold-drawn steel wire described in the present invention, its tensile strength is ≥1400MPa and its area reduction ratio is ≥30%.

[0048] Another object of the present invention is to provide a method for manufacturing wire rods for high-strength cold-drawn steel wire processing, which adopts a relatively simple processing technology to produce high-carbon steel wire rods that meet the processing requirements of 2100MPa high-strength and high-torsion performance galvanized steel wire.

[0049] Based on the above purpose, the present invention also provides a method for manufacturing a wire rod for processing high-strength cold-drawn steel wire, which comprises the steps of:

[0050] (1) Smelting;

[0051] (2) Using a billet continuous casting machine to cast billets;

[0052] (3) Heating: Heat to 950-1150°C and keep warm for 1.5-2.5 hours;

[0053] (4) Wire rod rolling: control the rolling speed to 20-60m / s;

[0054] (5) Stelmore fan cooling.

[0055] In the manufacturing method of the present invention, argon protection can be used in the casting process, the size of the small square billet can be ≤260 mm, and the width-to-thickness ratio can be ≤4:3. In addition, the carbon segregation in the center of the billet can be controlled to be lower than 1.08 by adjusting the drawing speed, cooling and terminal light reduction parameters during the continuous casting process.

[0056] Furthermore, in step (4) of the manufacturing method of the present invention, the inlet temperature of the finishing mill is controlled to be 920-980°C, the inlet temperature of the sizing mill is controlled to be 920-980°C, and the spinning temperature is controlled to be 900-970°C.

[0057] Furthermore, in step (5) of the manufacturing method described in the present invention, the air volume adjustment range of the Stelmore line is controlled as follows: the air volume of the F1-F7 fans is 80-100%, and the air volume of the F8-F14 fans is 0-45%.

[0058] In the manufacturing method of the present invention, after the wire rod is rolled, the wire rod structure transformation is controlled by adjusting the Stelmor wire fan component to optimize the wire rod structure. After Stelmor cooling, the wire rod forms a good lamellar troostite structure without abnormal martensite structure, the size of the troostite pellets is 2-25 μm, and the proportion of spherical and short rod-shaped degenerate cementite in the wire rod is less than 0.5%, which is conducive to subsequent wire drawing.

[0059] The present invention also provides a galvanized steel wire, which is obtained by drawing, galvanizing and stabilizing the wire rod for high-strength cold-drawn steel wire processing as described above, and the tensile strength of the galvanized steel wire is ≥2100MPa; and the torsion value is ≥12 times.

[0060] The drawing, galvanizing and stabilization treatment are all conventional processes in the art, and the present invention does not improve them, so they will not be described in detail here.

[0061] The high-strength cold-drawn steel wire processing wire rod of the present invention has the following advantages and beneficial effects:

[0062] The method for manufacturing the wire rod for high-strength cold-drawn steel wire processing described in the present invention has a simple process and does not require steps such as isothermal treatment to obtain a wire rod with good strength-plasticity matching ability, which can meet the requirements of 2100MPa strength steel wire drawing and galvanizing processing.

[0063] The microstructure of the wire rod for high-strength cold-drawn steel wire processing described in the present invention is mainly dominated by troostite, and the size of the troostite pellets is refined to 2-30μm, the volume proportion of spherical and short rod-shaped degenerate cementite in the wire rod is less than 0.6%, the core carbon segregation is less than 1.06, and there is no abnormal structure in the structure.

[0064] The wire rod for processing high-strength cold-drawn steel wire of the present invention has a tensile strength of more than 1400MPa, good plasticity, and a surface shrinkage rate of more than 30%. Therefore, the wire rod can be directly drawn, galvanized, and stabilized to produce galvanized steel wire for bridge cables and high-strength steel strands with a strength of more than 2100MPa and a torsion value of more than 12 times. The processing cost is low, and the requirements for use of large-span bridges and construction projects can be met, thereby reducing project investment and saving costs. DETAILED DESCRIPTION

[0065] The high-strength cold-drawn steel wire processing wire rod and the preparation method thereof described in the present invention will be further explained and illustrated below in conjunction with specific embodiments. However, such explanation and illustration do not constitute an improper limitation on the technical solution of the present invention.

[0066] Examples 1-10 and Comparative Examples 1-3

[0067] The high-strength cold-drawn steel wire processing wire rods of Examples 1-10 are all prepared by the following steps:

[0068] (1) After smelting in an electric furnace or converter, refining is carried out outside the furnace. The refining outside the furnace adopts the LF furnace plus VD or RH degassing treatment process. During the smelting process, the composition and addition amount of the synthetic slag are adjusted to control the P and S content in the steel to be less than 0.010% and 0.010% respectively. The vacuum degassing time is 18-28min, and the end point O content is controlled to be 0.0015-0.0035%, and the N content is 0.004-0.008%.

[0069] (2) The billet continuous casting machine was used to cast the billet. Argon protection was used during the casting process. The billet size was ≤260 mm, and the width-to-thickness ratio was ≤4:3. The carbon segregation in the center of the billet was controlled to be lower than 1.08 by adjusting the casting speed, cooling and terminal soft reduction parameters during the continuous casting process. The chemical composition of the obtained billet is shown in Table 1. The billet was subjected to eddy current flaw detection, magnetic particle flaw detection, grinding wheel mold repair, additional magnetic particle flaw detection and grinding to remove defects such as cracks and pits on the surface of the billet. The defect depth was ≤0.5 mm.

[0070] (3) Heat the billet to 950-1150°C and keep it warm for 1.5-2.5 hours.

[0071] (4) Wire rod rolling: the rolling speed is controlled at 20-60 m / s, the inlet temperature of the finishing mill is controlled at 920-980°C, the inlet temperature of the sizing mill is controlled at 920-980°C, the spinning temperature is controlled at 900-970°C, and the size of the wire rod obtained by rolling is controlled at Ф11-16 mm.

[0072] (5) Stelmore fan cooling: The air volume of F1-F7 fans is 80-100%, and the air volume of F8-F14 fans is 0-45%.

[0073] The comparative wire rods of Comparative Examples 1-3 are also prepared by the above-mentioned steps and processes, but their chemical compositions and specific process parameters in each step fail to meet the design requirements of the present invention.

[0074] Table 1 lists the mass percentages of the chemical elements of the wire rods for high-strength cold-drawn steel wire processing of Examples 1-10 and Comparative Examples 1-3.

[0075] Table 1. (wt%, the balance is Fe and other inevitable impurities except P, S, Ti)

[0076]

[0077]

[0078] Note: In the above formula (V+2Nb) / (C+100N)+W / C, each chemical element is substituted with the value before the percentage sign of the corresponding chemical element mass percentage content.

[0079] Table 2 lists the specific process parameters of the wire rods of Examples 1-10 and the comparative wire rods of Comparative Examples 1-3 in the above steps.

[0080] Table 2.

[0081]

[0082] The wire rods of Examples 1-10 and the comparative wire rods of Comparative Examples 1-3 were sampled respectively, and the microstructure of the steel plate samples of each example was observed and analyzed. The relevant observation and analysis results are listed in Table 3 below.

[0083] Table 3 lists the microstructure characteristics of the wire rods of Examples 1-10 and the comparative wire rods of Comparative Examples 1-3.

[0084] Table 3.

[0085]

[0086] As shown in Table 3, the size of the troostite pellets in the wire rods in Examples 1-10 ranges from 2 to 25 μm, while the size of the troostite pellets in the comparative examples is larger than that of the present invention. In addition, the volume proportions of spherical and short rod-shaped degenerate cementite in the wire rod microstructures in Examples 1-10 of the present invention are all less than 0.5%, while those in Comparative Examples 1-3 are all higher than 0.5%.

[0087] In order to verify the mechanical properties of the wire rods of each embodiment and comparative example, the inventors sampled the wire rods of embodiments 1-10 and the comparative wire rods of comparative examples 1-3 obtained through the above process steps again, and conducted mechanical property tests according to GB / T 228.1 Metallic Material Tensile Test Part 1: Room Temperature Test Method, and the mechanical property test results are listed in Table 4.

[0088] Table 4 lists the performance test results of the wire rods of Examples 1-10 and the comparative wire rods of Comparative Examples 1-3.

[0089] Table 4.

[0090]

[0091] It can be seen from Table 4 that the tensile strength of the wire rods of Examples 1-10 of the present invention is ≥1400MPa, and the area shrinkage is ≥30%. Although the area shrinkage of Comparative Example 1 meets the requirements of the present invention, its tensile strength is much lower than that of the present invention. Although the tensile strength of Comparative Example 2 meets the requirements of the present invention, its area shrinkage is <30%. Both the area shrinkage and tensile strength of Comparative Example 3 are lower than those of the present invention, which indicates that Comparative Examples 1-3 cannot achieve both strength and plasticity.

[0092] In order to prove that high-strength galvanized steel wire can be obtained by using the wire rod of the present invention, the wire rods of Examples 1-10 and the comparative wire rods of Comparative Examples 1-3 were subjected to 6-9 drawing, wire galvanizing and stabilization treatments to obtain galvanized steel wire. The galvanized steel wires obtained in Examples 1-10 and Comparative Examples 1-3 were tested for various related properties, and the obtained performance test results are listed in Table 5. The related performance testing methods are as follows:

[0093] Tensile test: The tensile test was carried out using GB / T 228.1 Metallic material tensile test Part 1: Room temperature test method to measure the tensile strength of the steel wires of Examples 1-10 and the comparative steel wires of Comparative Examples 1-3.

[0094] Torsion test: GB / T 239.1 Metallic wire Part 1: Unidirectional torsion test method was used to measure the 100D gauge length specimen torsion values ​​of the steel wires of Examples 1-10 and the comparative steel wires of Comparative Examples 1-3.

[0095] Table 5 lists the performance test results of the steel wires of Examples 1-10 and the comparative steel wires of Comparative Examples 1-3.

[0096] Table 5.

[0097]

[0098]

[0099] It can be seen from Table 5 that the tensile strength of the steel wires of Examples 1-10 obtained from the above-mentioned wire rods after drawing, galvanizing and stabilization treatment is further improved, and the tensile strength is all greater than 2100 MPa; the torsion value is ≥12 times.

[0100] In addition, the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.

[0101] It should also be noted that the above-listed embodiments are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therewith can be directly derived or easily associated with the contents disclosed by those skilled in the art from the present invention, and all should belong to the protection scope of the present invention.

Claims

1. A wire rod for processing high-strength cold-drawn steel wire, containing Fe and unavoidable impurities, characterized in that: It also contains the following chemical elements in the following mass percentages: C:0.89-0.94%; Si: 0.70-1.20%; Mn: 0.30-0.80%; Cr:0.30-0.60%; V:0.03-0.10%; Nb: 0.03-0.08%; W:0.1-0.4%; Al:0.02-0.05%; O:0.0015-0.0035%; N:0.004-0.008%。 2. The wire rod for processing high-strength cold-drawn steel wire according to claim 1, characterized in that: The mass percentage of each chemical element is: C:0.89-0.94%; Si: 0.70-1.20%; Mn: 0.30-0.80%; Cr:0.30-0.60%; V:0.03-0.10%; Nb: 0.03-0.08%; W:0.1-0.4%; Al:0.02-0.05%; O:0.0015-0.0035%; N:0.004-0.008%; The balance is Fe and other inevitable impurities.

3. The wire rod for processing high-strength cold-drawn steel wire according to claim 1 or 2, characterized in that: The mass percentage of chemical elements also satisfies: (V+2Nb) / (C+100N)+W / C≥1 / 5, where each chemical element is substituted into the value before the percentage sign of the mass percentage of the corresponding chemical element.

4. The wire rod for processing high-strength cold-drawn steel wire according to claim 1 or 2, characterized in that: Among other inevitable impurities: Ti≤0.003%, P≤0.010%, S≤0.010%.

5. The wire rod for processing high-strength cold-drawn steel wire according to claim 1 or 2, characterized in that: Its microstructure includes sorbite globules with a size range of 2-25 μm.

6. The wire rod for processing high-strength cold-drawn steel wire according to claim 1 or 2, characterized in that: The volume proportion of spherical and short rod-shaped degenerate cementite in its microstructure is less than 0.5%.

7. The wire rod for processing high-strength cold-drawn steel wire according to claim 1 or 2, characterized in that: Its tensile strength is ≥1400MPa and its surface shrinkage is ≥30%.

8. The method for manufacturing a wire rod for processing high-strength cold-drawn steel wire according to any one of claims 1 to 7, characterized in that: It includes the steps of: (1) Smelting; (2) Using a billet continuous casting machine to cast billets; (3) Heating: Heat to 950-1150°C and keep warm for 1.5-2.5 hours; (4) Wire rod rolling: control the rolling speed to 20-60m / s; (5) Stelmore fan cooling.

9. The manufacturing method according to claim 8, characterized in that: In step (4), the inlet temperature of the finishing mill is controlled to be 920-980°C, the inlet temperature of the sizing mill is controlled to be 920-980°C, and the spinning temperature is controlled to be 900-970°C.

10. The manufacturing method according to claim 8, characterized in that: In step (5), the air volume of the F1-F7 fans of the Stelmore blower group is controlled to be 80-100%, and the air volume of the F8-F14 fans is controlled to be 0-45%.

11. A galvanized steel wire, which is obtained by drawing, galvanizing and stabilizing the high-strength cold-drawn steel wire processing wire rod as described in any one of claims 1 to 7, wherein the tensile strength of the galvanized steel wire is ≥2100MPa and the torsion value is ≥12 times.

Citation Information

Patent Citations

  • Wire, steel wire and their manufacturing methods

    CN102301024A

  • Steel wire rod for 1860MPa-level bridge cable galvanized steel wire and manufacturing method thereof

    CN102634730A

  • High-strength coil rod excellent in low-temperature performance and manufacturing method of high-strength coil rod

    CN105506500A

  • 2000 MPa-grade bridge cable galvanized steel wire and preparation method thereof

    CN110066963A

  • Steel for 2100 MPa grade marine steel wire rope and production method thereof

    CN110819899A