Composite lithium strip and preparation method thereof
By using a porous carbon skeleton with a metal wire nucleating agent in the electrode, the problems of loose deposition of metallic lithium and location migration of the nucleating agent are solved, achieving dense deposition of metallic lithium and extending the battery cycle life, improving the battery's performance stability and performance.
Patent Information
- Application Number
- CN202310401893.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-18
AI Technical Summary
During the cycle, metallic lithium becomes loose due to its deposition into dendrites, which increases the consumption of active metals and causes rapid battery capacity attenuation. In addition, the positional migration and polymerization of the nucleating agent weakens its effect, affecting the battery cycle life.
It adopts a porous support skeleton with an amorphous carbon coating layer and contains a metal wire nucleating agent. The metal wire nucleating agent is fixed in the carbon skeleton to provide uniform nucleation sites, inhibit the formation of lithium dendrites, and reduce the volume expansion of the electrode. .
It achieves dense deposition of metallic lithium, extends the battery cycle life, and improves the physical and chemical performance stability of the battery.
Smart Images

Figure CN118800907A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal lithium processing, and in particular relates to a composite lithium belt and a preparation method thereof. Background Art
[0002] Lithium metal has always attracted people's attention as a negative electrode material with future application value. Lithium metal has a high specific capacity (3860mAh / g) and a low electrochemical potential (vs hydrogen standard electrode). Therefore, lithium metal is very suitable for preparing battery systems with high capacity and high output voltage. However, as a negative electrode material, lithium metal deposition will generate a large number of dendrites during the cycle process due to the (110) crystal plane orientation of lithium metal deposition. This is the main reason for the loose deposition of lithium metal. The loose deposition of lithium metal increases the contact area between lithium metal and the electrolyte, resulting in huge consumption of active lithium metal, leading to rapid battery capacity decay.
[0003] Studies have shown that adding nucleation sites to materials and guiding the deposition of metallic lithium can effectively reduce the formation of metallic lithium dendrites, thereby extending the cycle life of the battery. Samsung Research Institute added nanosilver particles to carbon black as nucleation sites, which greatly improved the cycle life of the battery. However, studies have found that as the cycle progresses, the nucleating agent migrates and aggregates, causing its effect to be greatly weakened.
[0004] From the above, it can be seen that it is indeed necessary to develop a composite lithium belt with fixed nucleation sites. Summary of the invention
[0005] In view of the above technical problems, the present invention provides a composite lithium belt, which has a lithium-philic carbon material and can be used as a host material for metallic lithium to reduce volume expansion during electrode cycling. The metal wire nucleating agent in the composite lithium belt provides nucleation sites for the deposition of metallic lithium, and the position of the metal wire nucleating agent does not change with the progress of the cycle, so that the metallic lithium can nucleate and grow uniformly inside the material and be densely deposited, thereby inhibiting the formation of lithium dendrites.
[0006] To achieve the above objectives, one aspect of the present invention provides a composite lithium strip, comprising:
[0007] A ribbon-shaped porous support skeleton, the porous support skeleton comprising a lithium-philic carbon material and a metal wire nucleating agent, the lithium-philic carbon material comprising a crystallized carbon material with an amorphous carbonaceous coating layer and interweaving to form the porous support skeleton, the metal wire nucleating agent being distributed in a monodispersed form and fixed in or on the surface of the amorphous carbonaceous coating layer;
[0008] A metallic lithium matrix supported by the porous support skeleton, wherein the metallic lithium matrix covers the surface of the porous support skeleton and at least a portion of the metallic lithium enters the pores of the porous support skeleton,
[0009] Wherein, the diameter of the metal wire nucleating agent is in the range of 10 nm to 500 nm, and the length is in the range of 100 nanometers to 500 micrometers.
[0010] In some embodiments, the crystallized carbonaceous material includes carbon nanotubes, graphene, mesophase carbon microspheres, soft carbon, hard carbon, carbon fiber, cracked carbon, carbonaceous ordered mesoporous materials and combinations thereof; the crystallized carbonaceous material has a linear, spherical, sea urchin-shaped, oblate spherical or scaly configuration.
[0011] In some embodiments, the amorphous carbonaceous coating layer contains at least one element of oxygen, carbon, nitrogen, fluorine, silicon, phosphorus, and boron, and is a carbonization product of an organic material blended with a crystallized carbonaceous material, wherein the organic material is selected from the group consisting of an organic binder and a crosslinking agent.
[0012] In some embodiments, the amorphous carbonaceous coating layer has a thickness in the range of 2-300 nm.
[0013] In some embodiments, the metal wire nucleating agent is silver wire, gold wire, copper wire, aluminum wire, magnesium wire, tin wire, iron wire, sodium wire, lead wire, platinum wire, titanium wire, tungsten wire, beryllium wire, zinc wire, nickel wire, indium wire, molybdenum wire or a combination thereof.
[0014] In some embodiments, the composite lithium ribbon has a thickness in the range of 1-300 micrometers and a width in the range of 10-1000 mm.
[0015] In some embodiments, the weight percentage of the metallic lithium is 7% to 95%, the weight percentage of the lithium-philic carbon material is 4% to 85%, and the weight percentage of the metal wire nucleating agent is 1% to 34%.
[0016] In some embodiments, the porous support framework has a porosity in the range of 6%-88% and a pore size in the range of 10-500 nm.
[0017] Another aspect of the present invention provides a method for preparing the above-mentioned composite lithium strip, comprising the following steps:
[0018] Step 1, uniformly dispersing the crystallized carbonaceous material, the organic binder, the crosslinking agent and the metal wire nucleating agent in a solvent;
[0019] Step 2, drying the dispersed slurry;
[0020] Step 3, under the protection of an inert atmosphere, subjecting the dried slurry to a high temperature treatment at a temperature between 400° C. and 1000° C.;
[0021] Step 4, compounding the material after high temperature treatment with metallic lithium to obtain a composite lithium block;
[0022] Step 5: Process the composite lithium block to obtain a composite lithium negative electrode.
[0023] In some embodiments, the solvent in step 1 is deionized water, N-methylpyrrolidone or a combination thereof.
[0024] In some embodiments, the drying process in step 2 includes high temperature dehydration and low temperature dehydration.
[0025] In some embodiments, the compounding method described in step 4 is at least one of molten lithium injection, mechanical kneading, and roller pressing compounding.
[0026] In some embodiments, in step 1, the mass ratio of the crystallized carbonaceous material, the organic binder and the cross-linking agent is (45-85):(5-34):(1-50).
[0027] In some embodiments, the organic binder is selected from the group consisting of polyvinyl alcohol, polyvinylidene fluoride, polybutylene styrene, polystyrene, polycarboxycellulose, cyanoacrylate, polyacrylic acid, cyclodextrin, cyclic ether derivatives, polyurethane, methacrylate, epoxy resin, vinyl acetate polymer, polyimide, organic fluorine polymer, organosiloxane, polyethylene glycol, polyethylene, polyvinyl chloride, polypropylene, glycerol, ethyl hydroxybenzoate and its derivatives, monosaccharide or polysaccharide polymers,
[0028] In some embodiments, the crosslinking agent is selected from the group consisting of styrene peroxide, benzoyl peroxide, diethylenetriamine, hydrated sodium borate, cellulose derivatives, and isothiazolinone.
[0029] In summary, the composite lithium negative electrode of the present invention has at least the following advantages:
[0030] 1. The composite lithium belt has a lithium-philic carbon material, which can be used as a host material for metallic lithium to reduce volume expansion during electrode cycling;
[0031] 2. The metal wire nucleating agent in the composite lithium belt provides nucleation sites for the deposition of metallic lithium, so that the metallic lithium can be uniformly nucleated and grown inside the material, and deposited densely, thereby inhibiting the formation of lithium dendrites;
[0032] 3. The metal wire nucleating agent in the composite lithium belt will not change position as the cycle progresses, and the physical and chemical properties of the composite lithium negative electrode are more stable and reliable. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a scanning electron microscope image of the carbon material after high temperature treatment in Example 1 of the present invention.
[0034] Figure 2The scanning electron microscope image and electron energy spectrum of the composite lithium negative electrode prepared in Example 1.
[0035] Figure 3 This is a scanning electron microscope image of the carbon material after high temperature treatment in Example 2.
[0036] Figure 4 The half-cell cycle curves of button cells assembled using lithium ribbons prepared in Example 1, Example 2, Example 3 and Comparative Example 1. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0038] Example 1
[0039] Carbon nanotubes (Shandong Dazhan), polyvinyl alcohol, styrene peroxide and metal silver wire nucleating agent (Suzhou Nofei Nanotechnology Co., Ltd.) were uniformly dispersed in deionized water in a mass ratio of 9:4.5:0.5:1. The dispersed slurry was dried. Under the protection of argon atmosphere, the dried slurry was subjected to high temperature treatment at 800°C. The scanning electron microscope image of the carbon material after high temperature treatment is shown in Figure 1. Figure 1 As shown in the figure, it can be seen that the metal wire nucleating agents are distributed on the surface of the carbon skeleton, and the lengths of the two metal wire nucleating agents shown in the figure are 131nm and 398nm respectively.
[0040] The molten lithium is injected into the material after high temperature treatment to obtain a composite lithium negative electrode block. The composite lithium negative electrode block is processed to obtain a composite lithium negative electrode with a thickness of 50 microns. The scanning electron microscope image and electron energy spectrum of the prepared composite lithium negative electrode are as follows: Figure 2 As shown. Figure 2 It can be seen that the mass proportion of lithium metal elements in the prepared composite lithium is 80.4%, the mass proportion of silver elements is 14.2%, the mass proportion of carbon materials is 4%, and there are also small amounts of oxygen elements and other trace elements.
[0041] Example 2
[0042] Carbon nanotubes (Shandong Dazhan), polyvinyl alcohol and styrene peroxide were uniformly dispersed in deionized water in a mass ratio of 9:4.5:0.5. The dispersed slurry was dried. Under the protection of argon atmosphere, the dried slurry was subjected to high temperature treatment at 800°C. The scanning electron microscope image of the carbon material after high temperature treatment is shown in Figure 1. Figure 3As shown. Molten lithium is injected into the material after high temperature treatment to obtain a composite lithium negative electrode block. The composite lithium negative electrode block is processed to obtain a composite lithium negative electrode with a thickness of 50 microns.
[0043] Example 3
[0044] The same as Example 2, except that the metallic silver wire nucleating agent and the material after high temperature treatment are mixed in a mass ratio of 1:14, and then molten lithium is injected into the mixed material.
[0045] Comparative Example 1
[0046] A commercial lithium ribbon with a thickness of 50 microns was used.
[0047] The strips in Example 1, Example 2 and Comparative Example 1 were used as negative electrodes and assembled into button-type half-cells with metal lithium counter electrodes. The separator was a Celgard 2500 polypropylene (PP) film, and the electrolyte was 1M LiPF6, EC:EMC=3:7 (vol / vol). The assembled button cells were charged and discharged with a charge and discharge current of 2mA and a charge and discharge time of 1 hour. The cycle was continued until the battery life ended, and the charge and discharge times were recorded. The test curve is shown in Figure 1. Figure 4 shown.
[0048] from Figure 4 It can be seen that the cycle life of the button battery half-cell assembled with lithium ribbon in Comparative Example 1 is only 250 hours, while the cycle life of the button battery assembled with the lithium-carbon material prepared in Example 2 or the mixed material prepared in Example 3 can reach about 500 hours. Although its cycle life is greatly improved, the button battery assembled with the composite lithium negative electrode of the present invention (Example 1) can reach a maximum cycle life of 1500 hours. The composite lithium ribbon of the present invention shows great performance advantages.
[0049] It is understood that, in the embodiments of the present invention, although the composite lithium belt and the preparation method thereof are described in detail in combination with specific implementation methods, the above description is only made to meet legal requirements, and the present invention is not limited to the given embodiments. Those skilled in the art can complete the replication of the composite lithium belt and the preparation method thereof through appropriate operations according to the disclosure and teaching of the specification.
[0050] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can make appropriate changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the present invention should also fall within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A composite lithium belt, It is characterized in that include: A ribbon-shaped porous support skeleton, the porous support skeleton comprising a lithium-philic carbon material and a metal wire nucleating agent, the lithium-philic carbon material comprising a crystallized carbon material with an amorphous carbonaceous coating layer and interweaving to form the porous support skeleton, the metal wire nucleating agent being distributed in a monodispersed form and fixed in or on the surface of the amorphous carbonaceous coating layer; A metallic lithium matrix supported by the porous support skeleton, wherein the metallic lithium matrix covers the surface of the porous support skeleton and at least a portion of the metallic lithium enters the pores of the porous support skeleton, The diameter of the metal wire nucleating agent is in the range of 10 nm to 500 nm, and the length is in the range of 100 nanometers to 500 micrometers.
2. The composite lithium strip according to claim 1, It is characterized in that The crystallized carbonaceous materials include carbon nanotubes, graphene, mesophase carbon microspheres, soft carbon, hard carbon, carbon fiber, cracked carbon, carbonaceous ordered mesoporous materials and combinations thereof; the crystallized carbonaceous materials have linear, spherical, sea urchin-shaped, oblate spherical or scaly configurations.
3. The composite lithium strip according to claim 1, It is characterized in that The amorphous carbonaceous coating layer contains at least one element of oxygen, carbon, nitrogen, fluorine, silicon, phosphorus, and boron, and is a carbonized product of an organic material blended with a crystallized carbonaceous material, wherein the organic material is selected from the group consisting of an organic binder and a crosslinking agent.
4. The composite lithium strip according to claim 3, It is characterized in that The thickness of the amorphous carbonaceous coating layer is in the range of 2-300 nm.
5. The composite lithium strip according to claim 1, It is characterized in that The metal wire nucleating agent is silver wire, gold wire, copper wire, aluminum wire, magnesium wire, tin wire, iron wire, sodium wire, lead wire, platinum wire, titanium wire, tungsten wire, beryllium wire, zinc wire, nickel wire, indium wire, molybdenum wire or a combination thereof.
6. The composite lithium strip according to claim 1, It is characterized in that The composite lithium belt has a thickness in the range of 1-300 micrometers and a width in the range of 10-1000 mm.
7. The composite lithium strip according to claim 1, It is characterized in that The mass proportion of the metallic lithium is 7% to 95%, the mass proportion of the lithium-philic carbon material is 4% to 85%, and the mass proportion of the metal wire nucleating agent is 1% to 34%.
8. A method for preparing the composite lithium strip according to any one of claims 1 to 7, It is characterized in that The steps include: IB231433 Step 1, uniformly dispersing the crystallized carbonaceous material, the organic binder, the crosslinking agent and the metal wire nucleating agent in a solvent; Step 2, drying the dispersed slurry; Step 3, under the protection of an inert atmosphere, subjecting the dried slurry to a high temperature treatment at a temperature between 400° C. and 1000° C.; Step 4, compounding the material after high temperature treatment with metallic lithium to obtain a composite lithium block; Step 5: Processing the composite lithium block to obtain a composite lithium belt.
9. The method according to claim 8, It is characterized in that The drying process described in step 2 includes high temperature dehydration and low temperature dehydration.
10. The method according to claim 8, It is characterized in that The compounding method described in step 4 is at least one of molten lithium injection, mechanical mixing, and roller pressing compounding.