Composite conductive agent and preparation method and application thereof
By using lithium-conducting plastic crystals to coat the conductive agent in all-solid-state batteries, the contact area between the sulfide electrolyte and the positive active material is increased, which solves the problem of insufficient charge and discharge efficiency and rate performance in the first cycle of the battery, and achieves higher battery stability. and high temperature performance.
Patent Information
- Application Number
- CN202410775606.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-17
AI Technical Summary
There is room for improvement in the first-cycle charge-discharge efficiency and rate performance of all-solid-state batteries. Increasing test pressure through traditional methods will promote the growth of lithium dendrites and cause battery short circuit. The ionic conductivity of the oxide/halide interlayer is insufficient to reduce the positive electrode potential.
The conductive agent is coated with lithium-conducting plastic crystals and the composite conductive agent is prepared by melt mixing method to increase the contact area between the sulfide electrolyte and the positive active material, enhance the mass transfer efficiency, and avoid the dissolution of lithium ions and side reactions between the solvent and the electrolyte.
It significantly improves the first charge and discharge efficiency and rate performance of the positive electrode, improves the cycle stability and high-temperature structural stability of the battery, and achieves better charge and discharge performance.
Smart Images

Figure CN118800909A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a composite conductive agent and a preparation method and application thereof. Background Art
[0002] Lithium batteries with liquid / gel electrolytes have been widely used in commercial electronic devices, but in large-scale applications such as electric vehicles and smart grids, their flammability, volatility, thermal instability, narrow electrochemical window, and difficulty in inhibiting the growth of lithium dendrites limit the safety and energy density of traditional liquid batteries. Therefore, it is imperative to develop new electrolytes for the next generation of batteries.
[0003] All-solid-state batteries use thermally stable solid electrolytes such as sulfides, halides and oxides instead of liquid electrolytes. The conductivity of sulfides is close to that of liquid electrolytes, and they have the advantages of being soft, non-corrosive to equipment and environmentally friendly, which has attracted widespread attention. However, their first-cycle charge and discharge efficiency still has room for improvement. The capacity loss of positive electrode materials mainly occurs due to structural changes after the first discharge, and the number of lithium-insertable sites in the material decreases.
[0004] In order to alleviate the material pulverization caused by volume change of high-nickel NCM (nickel, cobalt, manganese) positive electrode materials during the cycle, the main solution is to increase the test pressure or add oxide / halide interlayers. However, the increased test pressure also promotes the growth of lithium dendrites to a certain extent and penetrates the electrolyte to cause battery short circuit. At the same time, oxides / halides also have problems such as insufficient ion conductivity, which reduces the positive electrode potential to a certain extent.
[0005] Therefore, it is urgent to develop a new material or method to further improve the first-cycle charge and discharge efficiency (first efficiency) and rate performance of solid-state batteries. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a composite conductive agent and a preparation method and application thereof, wherein the composite conductive agent adopts a lithium conductive plastic crystal coated conductive agent, which can greatly increase the contact area between the sulfide electrolyte and the positive electrode active material on the positive electrode side, thereby improving the mass transfer efficiency, and further improving the first efficiency and rate performance of the positive electrode.
[0007] The inventive concept of the present invention is: the present invention coats the surface of the conductive agent particles with plastic lithium-conducting plastic crystals, so that the conductive agent has the functions of conducting electrons and lithium ions at the same time, and is beneficial to improving the contact interface in the positive electrode sheet of the battery, thereby improving the first effect and charge and discharge efficiency of the positive electrode active material, improving the cycle stability of the high-nickel NCM battery, and the structural stability and rate performance of the sulfide solid-state battery at high temperature. At the same time, the composite conductive agent of the present invention is beneficial to increase the contact area between the sulfide electrolyte and the positive electrode active material on the positive electrode side by coating the conductive agent with lithium-conducting plastic crystals, improving the mass transfer efficiency, and further improving the first effect and rate performance of the positive electrode. In addition, the composite conductive agent of the present invention is prepared by a melt mixing method, which avoids the dissolution of lithium ions and the side reaction of the solvent and the sulfide electrolyte compared to the traditional solvent method, and therefore exhibits better first effect and charge and discharge performance.
[0008] In order to solve the above technical problems, the first aspect of the present invention provides a composite conductive agent, which includes a conductive agent and a lithium-conductive plastic crystal, wherein the lithium-conductive plastic crystal is coated on the surface of the conductive agent, and the lithium-conductive plastic crystal is a mixture of plastic crystal and lithium salt, and the mass ratio of the plastic crystal to the lithium salt is (2-6):1.
[0009] Studies have found that the lithium salt content in lithium-conducting plastic crystals should not be too high. Excessive lithium salt content will reduce the plastic crystal's ability to dissociate lithium salts, which is not conducive to the battery's initial efficiency and charge and discharge performance.
[0010] Preferably, the plastic crystal is selected from N-ethyl-N-methylpyrrole bis(fluorosulfonyl)imide (P 12 FSI), N-ethyl-N-methylpyrrole bis(trifluoromethanesulfonyl)imide (P 12 TFSI), N-ethyl-N-methylpiperidinium bis(fluorosulfonyl)imide (PP 12 FSI), N-ethyl-N-methylpiperidinium bis(trifluoromethanesulfonyl)imide (PP 12 TFSI), N-propyl-N-methylpiperidinium bis(fluorosulfonyl)imide (PP 13 FSI), N-propyl-N-methylpiperidinium bis(trifluoromethanesulfonyl)imide salt (PP 13 TFSI), triethyl (methyl) phosphorus bis (fluorosulfonyl) imide salt (P 1222 FSI), triethyl (methyl) phosphorus bis (trifluoromethanesulfonyl) imide salt (P 1222 TFSI), N,N-dimethylpyrrole bis(fluorosulfonyl)imide salt (P 11 FSI), N,N-dimethylpyrrole bis(trifluoromethanesulfonyl)imide salt (P 11 At least one of TFSI).
[0011] Preferably, the lithium salt is lithium bis(trifluoromethanesulfonyl imide) and / or lithium bis(fluorosulfonyl imide) salt.
[0012] Preferably, the mass proportion of the lithium-conductive plastic crystal in the composite conductive agent is 5-95%; further preferably, the mass proportion of the lithium-conductive plastic crystal in the composite conductive agent is 50-90%; further preferably, the mass proportion of the lithium-conductive plastic crystal in the composite conductive agent is 80-85.7%.
[0013] Preferably, the conductive agent is selected from at least one of vapor-grown carbon fiber, carbon black, conductive graphite, graphene, and carbon nanotubes.
[0014] The second aspect of the present invention provides a method for preparing the composite conductive agent, comprising the following steps:
[0015] (1) mixing plastic crystal and lithium salt to form a lithium-conducting plastic crystal composite solution;
[0016] (2) The lithium-conducting plastic crystal composite solution obtained in step (1) is mixed with a conductive agent, heated, and infiltrated to obtain the composite conductive agent.
[0017] Preferably, in step (2), the infiltration method is selected from any one of room temperature vacuuming, heated vacuuming, solution immersion, and pressure infiltration.
[0018] Preferably, the heating is carried out under vacuum conditions at a temperature of 70-90° C. for 3-15 hours.
[0019] A third aspect of the present invention provides a positive electrode, which includes a positive electrode active material, an electrolyte, a binder and the above-mentioned composite conductive agent.
[0020] Preferably, the positive electrode active material is a nickel-cobalt-manganese ternary material.
[0021] Preferably, the nickel-cobalt-manganese ternary material is LiNi 0.83 Co 0.12 Mn 0.05 O2(NCM83).
[0022] Preferably, the electrolyte is a sulfide electrolyte.
[0023] Preferably, the sulfide electrolyte is Li3PS4.
[0024] Preferably, the binder is polytetrafluoroethylene (PTFE).
[0025] A fourth aspect of the present invention provides an all-solid-state battery, comprising the above-mentioned positive electrode.
[0026] Compared with the prior art, the above technical solution of the present invention has at least the following technical effects or advantages:
[0027] (1) The composite conductive agent of the present invention coats the surface of the conductive agent particles with plastic lithium-conducting plastic crystals, so that the conductive agent has the functions of conducting electrons and lithium ions at the same time, and is conducive to improving the contact interface in the positive electrode sheet of the battery, thereby improving the first efficiency and charge and discharge efficiency of the positive electrode active material. At the same time, the composite conductive agent of the present invention is conducive to increasing the contact area between the sulfide electrolyte and the positive electrode active material on the positive electrode side, improving the mass transfer efficiency, and further improving the first efficiency and rate performance of the positive electrode.
[0028] (2) The composite conductive agent of the present invention is prepared by a melt mixing method. Compared with the traditional solvent method, it avoids the dissolution of lithium ions and the side reaction between the solvent and the sulfide electrolyte, and therefore exhibits better first efficiency and charge and discharge performance. The first charge specific capacity of the all-solid-state battery is 225.15-233.13%, and the first coulomb efficiency is 81.05-89.41%. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The charge-discharge specific capacity-voltage diagram for cycles 1-3 of the all-solid-state battery prepared in Application Example 3. DETAILED DESCRIPTION
[0030] The present invention is described in detail below in conjunction with the examples, so that the technical personnel of the relevant technical field can understand the present invention. It is necessary to point out here that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The non-essential improvements and adjustments made to the present invention by the skilled person in the relevant field according to the above invention content should still belong to the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods that are not mentioned in detail are all process steps or preparation methods known to those skilled in the art.
[0031] Example 1
[0032] A method for preparing a composite conductive agent, the preparation method is a melt mixing method, comprising the following steps:
[0033] (1) Plastic crystal P 12 TFSI and lithium salt LiFSI are mixed in a mass ratio of 2.1:1 and stirred to form a lithium-conducting plastic crystal composite solution;
[0034] (2) 0.2 g of the lithium-conducting plastic crystal composite solution prepared in step (1) was mixed with 0.05 g of VGCF powder, stirred evenly at 80° C., vacuumed, and soaked overnight to obtain a lithium-conducting plastic crystal coated with VGCF composite conductive agent P 12 TFSI / FSI-2.1@VGCF.
[0035] A method for preparing a positive electrode comprises the following steps:
[0036] Take 0.0125 g of the composite conductive agent P prepared in this embodiment 12 TFSI / FSI-2.1@VGCF, 0.4 g of NCM83 positive electrode material, 0.09 g of sulfide electrolyte Li3PS4 and 0.005 g of binder PTFE were dry-ground to form a positive electrode sheet, which was then cut into discs with a diameter of 0.9 cm to obtain the positive electrode of this embodiment.
[0037] Example 2
[0038] A method for preparing a composite conductive agent, the preparation method is a melt mixing method, comprising the following steps:
[0039] (1) Plastic crystal P 12 TFSI and lithium salt LiFSI are mixed in a mass ratio of 2.1:1 and stirred to form a lithium-conducting plastic crystal composite solution;
[0040] (2) 0.3 g of the lithium-conducting plastic crystal composite solution prepared in step (1) was mixed with 0.05 g of VGCF powder, stirred evenly at 80° C., vacuumed, and soaked overnight to obtain a lithium-conducting plastic crystal coated with VGCF composite conductive agent P 12 TFSI / FSI-2.1@VGCF.
[0041] A method for preparing a positive electrode comprises the following steps:
[0042] Take 0.0175 g of the composite conductive agent P prepared in this embodiment 12 TFSI / FSI-2.1@VGCF, 0.4 g of NCM83 positive electrode material, 0.085 g of sulfide electrolyte Li3PS4 and 0.005 g of binder PTFE were dry-ground to form a positive electrode sheet, which was then cut into discs with a diameter of 0.9 cm to obtain the positive electrode of this embodiment.
[0043] Example 3
[0044] A method for preparing a composite conductive agent, the preparation method is a melt mixing method, comprising the following steps:
[0045] (1) Plastic crystal P 12 TFSI and lithium salt LiFSI are mixed in a mass ratio of 5.68:1 and stirred to form a lithium-conducting plastic crystal composite solution;
[0046] (2) 0.2 g of the lithium-conducting plastic crystal composite solution prepared in step (1) was mixed with 0.05 g of VGCF powder, stirred evenly at 80° C., vacuumed, and soaked overnight to obtain a lithium-conducting plastic crystal coated with VGCF composite conductive agent P 12 TFSI / FSI-5.68@VGCF.
[0047] A method for preparing a positive electrode comprises the following steps:
[0048] Take 0.0125 g of the composite conductive agent P prepared in this embodiment 12 TFSI / FSI-5.68@VGCF, 0.4 g of NCM83 positive electrode material, 0.09 g of sulfide electrolyte Li3PS4 and 0.005 g of binder PTFE were dry-ground to form a positive electrode sheet, which was then cut into discs with a diameter of 0.9 cm to obtain the positive electrode of this embodiment.
[0049] Comparative Example 1
[0050] In Comparative Example 1, the sulfide electrolyte is first coated by a solvent method, and then a composite positive electrode sheet is prepared.
[0051] A method for preparing a composite electrolyte, the preparation method being a solvent method, comprising the following steps:
[0052] (1) Plastic crystal P 12 TFSI and lithium salt LiFSI are mixed in a mass ratio of 2.1:1 and stirred to form a lithium-conducting plastic crystal composite solution;
[0053] (2) 0.2 g of the lithium-conducting plastic crystal composite solution obtained in step (1) was dispersed in 20 mL of ethyl acetate solvent, and after ultrasonic dispersion, 1.8 g of sulfide electrolyte Li3PS4 was added. After stirring, the ethyl acetate solvent was removed by rotary evaporation, and after vacuum drying, a lithium-conducting plastic crystal-coated SE composite electrolyte P was obtained. 12 TFSI / FSI-2.1@SE.
[0054] A method for preparing a positive electrode comprises the following steps:
[0055] Take 0.1 g of the composite electrolyte P prepared in this comparative example 12 TFSI / FSI-2.1@SE (the composite electrolyte contains 0.01 g of lithium-conducting plastic crystal and 0.09 g of sulfide), 0.4 g of NCM83 positive electrode material, 0.0025 g of VGCF and 0.005 g of binder PTFE, dry-grinded to form a positive electrode sheet, and cut into discs with a diameter of 0.9 cm to obtain the positive electrode of this comparative example.
[0056] Comparative Example 2
[0057] The conductive agent of Comparative Example 2 is uncoated VGCF.
[0058] A method for preparing a positive electrode comprises the following steps:
[0059] Take 0.0025 g of VGCF, 0.4 g of NCM83 positive electrode material, 0.1 g of sulfide electrolyte Li3PS4 and 0.005 g of binder PTFE, dry grind them into positive electrode sheets, and cut them into discs with a diameter of 0.9 cm to obtain the positive electrode of this comparative example.
[0060] Comparative Example 3
[0061] A method for preparing a composite conductive agent, the preparation method is a melt mixing method, comprising the following steps:
[0062] (1) Plastic crystal P 12 TFSI and lithium salt LiFSI are mixed in a mass ratio of 1.42:1 and stirred to form a lithium-conducting plastic crystal composite solution;
[0063] (2) 0.2 g of the lithium-conducting plastic crystal composite solution prepared in step (1) was mixed with 0.05 g of VGCF powder, stirred evenly at 80° C., vacuumed, and soaked overnight to obtain a lithium-conducting plastic crystal coated with VGCF composite conductive agent P 12 TFSI / FSI-1.42@VGCF.
[0064] A method for preparing a positive electrode comprises the following steps:
[0065] Take 0.0125 g of the composite conductive agent P prepared in this comparative example 12 TFSI / FSI-1.42@VGCF, 0.4 g of NCM83 positive electrode material, 0.09 g of sulfide electrolyte Li3PS4 and 0.005 g of binder PTFE were dry-ground into positive electrode sheets, which were then cut into discs with a diameter of 0.9 cm to obtain the positive electrode of this comparative example.
[0066] Application Example 1
[0067] A sulfide solid-state battery, which is composed of a sulfide electrolyte Li3PS4 as an intermediate electrolyte layer, a LiIn alloy (Li foil diameter 6 mm, In sheet diameter 9 mm) as a negative electrode, and is assembled with a positive electrode prepared in Example 1 of the present invention.
[0068] Application Example 2
[0069] A sulfide solid-state battery, which is composed of a sulfide electrolyte Li3PS4 as an intermediate electrolyte layer, a graphite negative electrode (mixed by VGCF, graphite, Li3PS4 and PTFE in a mass ratio of 0.005:0.2:0.3:0.005), and a positive electrode prepared in Example 1 of the present invention.
[0070] Application Example 3
[0071] A sulfide solid-state battery, which is composed of a sulfide electrolyte Li3PS4 as an intermediate electrolyte layer, a graphite negative electrode (mixed by VGCF, graphite, Li3PS4 and PTFE in a mass ratio of 0.005:0.2:0.3:0.005), and an assembled positive electrode prepared in Example 2 of the present invention.
[0072] Application Example 4
[0073] A sulfide solid-state battery, which is composed of a sulfide electrolyte Li3PS4 as an intermediate electrolyte layer, a LiIn alloy (Li foil diameter 6 mm, In sheet diameter 9 mm) as a negative electrode, and is assembled with a positive electrode prepared in Example 3 of the present invention.
[0074] Comparative application example 1
[0075] A sulfide solid-state battery, which is composed of a sulfide electrolyte Li3PS4 as an intermediate electrolyte layer, a LiIn alloy (Li foil diameter 6 mm, In sheet diameter 9 mm) as a negative electrode, and is assembled with a positive electrode prepared in comparative example 1 of the present invention.
[0076] Comparative Application Example 2
[0077] A sulfide solid-state battery, which is composed of a sulfide electrolyte Li3PS4 as an intermediate electrolyte layer, a LiIn alloy (Li foil diameter 6 mm, In sheet diameter 9 mm) as a negative electrode, and is assembled with a positive electrode prepared in comparative example 2 of the present invention.
[0078] Comparative Application Example 3
[0079] A sulfide solid-state battery, which is composed of a sulfide electrolyte Li3PS4 as an intermediate electrolyte layer, a LiIn alloy (Li foil diameter 6 mm, In sheet diameter 9 mm) as a negative electrode, and is assembled with a positive electrode prepared in comparative example 3 of the present invention.
[0080] Performance Testing
[0081] The sulfide solid-state batteries assembled in Application Examples 1-4 and Comparative Application Examples 1-3 were subjected to charge and discharge tests respectively. The test conditions were: the surface density of the active material of the electrode was 22-33 mg cm -2 , assembly pressure 4T, test pressure 5Nm, 0.1C cycle, 25℃ / 60℃, voltage range 2.2-3.7V (vs.Li + / Li), 100 cycles.
[0082] The test results are shown in Table 1.
[0083] Table 1:
[0084]
[0085] As can be seen from Table 1, from the test results of Application Example 1, it can be concluded that when the same positive and negative electrodes are used and the test temperature is higher, the battery shows better charge and discharge specific capacity and first efficiency, indicating that the battery has good high temperature stability.
[0086] Comparative Application Example 1 uses a solvent method to coat the lithium-conducting plastic crystal on the electrolyte. Although it also shows good charge-discharge specific capacity and initial efficiency, lithium ions are inevitably dissolved during the solvent method. At the same time, it is difficult for the solvent used to completely avoid side reactions with the sulfide electrolyte. Therefore, the electrochemical performance of the battery is lower than that of Application Example 1.
[0087] Compared with Application Example 1, Application Example 2 replaces the LiIn alloy negative electrode with a graphite negative electrode. The battery still has a discharge specific capacity and first efficiency comparable to those of Application Example 1, further illustrating the feasibility of the composite conductive agent prepared by the present invention.
[0088] Application Example 3 The positive electrode prepared in Example 2 and the graphite negative electrode are assembled into an all-solid-state battery. The first cycle discharge capacity reaches 201.44 mAh / g at 60°C. At the same time, the third cycle 0.3C still has a discharge capacity of 188.82 mAh / g and 186.02 mAh / g (as shown in Figure 3). Figure 1 As shown), it further illustrates that the battery prepared by the present invention has good high temperature stability.
[0089] Application Example 4: Using PP with different mass ratios 12 The positive electrode prepared by coating VGCF with TFSI / LiTFSI composite also has high discharge capacity and first efficiency. In contrast, in Application Example 3, the content of lithium salt was further increased, and the first cycle charge and discharge capacity and first efficiency of the prepared electrode were significantly reduced, which may be because the excessively high lithium salt concentration reduced the plastic crystal's ability to dissociate lithium salt.
[0090] Therefore, the composite conductive agent prepared by the lithium-conducting plastic crystal coated VGCF of the present invention has the function of conducting lithium ions and electrons, can significantly improve the first-cycle discharge capacity of the battery, and has good high-temperature stability.
[0091] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, without having to go through creative labor. Therefore, simple improvements made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the protection scope of the present invention. The above embodiments are preferred embodiments of the present invention, and all processes similar to the present invention and equivalent changes made should belong to the protection scope of the present invention.
Claims
1. A composite conductive agent, characterized in that: The composite conductive agent includes a conductive agent and a lithium-conductive plastic crystal, wherein the lithium-conductive plastic crystal is coated on the surface of the conductive agent, and the lithium-conductive plastic crystal is a mixture of plastic crystal and lithium salt, and the mass ratio of the plastic crystal to the lithium salt is (2-6):
1.
2. The composite conductive agent according to claim 1, characterized in that: The plastic crystal is selected from at least one of N-ethyl-N-methylpyrrole bis(fluorosulfonyl)imide, N-ethyl-N-methylpyrrole bis(trifluoromethanesulfonyl)imide, N-ethyl-N-methylpiperidine bis(fluorosulfonyl)imide, N-ethyl-N-methylpiperidine bis(trifluoromethanesulfonyl)imide, N-propyl-N-methylpiperidine bis(fluorosulfonyl)imide, N-propyl-N-methylpiperidine bis(trifluoromethanesulfonyl)imide, triethyl(methyl)phosphorus bis(fluorosulfonyl)imide, triethyl(methyl)phosphorus bis(trifluoromethanesulfonyl)imide, N,N-dimethylpyrrole bis(fluorosulfonyl)imide, and N,N-dimethylpyrrole bis(trifluoromethanesulfonyl)imide.
3. The composite conductive agent according to claim 1, characterized in that: The lithium salt is lithium bis(trifluoromethanesulfonyl imide) and / or lithium bis(fluorosulfonyl imide) salt.
4. The composite conductive agent according to claim 1, characterized in that: The mass proportion of the lithium-conductive plastic crystal in the composite conductive agent is 5-95%.
5. The composite conductive agent according to any one of claims 1 to 4, characterized in that: The conductive agent is selected from at least one of vapor-grown carbon fibers, carbon black, conductive graphite, graphene, and carbon nanotubes.
6. A method for preparing a composite conductive agent according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing plastic crystal and lithium salt to form a lithium-conducting plastic crystal composite solution; (2) The lithium-conducting plastic crystal composite solution obtained in step (1) is mixed with a conductive agent, heated, and infiltrated to obtain the composite conductive agent.
7. The method for preparing the composite conductive agent according to claim 6, characterized in that: In step (2), the infiltration method is selected from any one of room temperature vacuuming, heated vacuuming, solution immersion, and pressure infiltration.
8. The method for preparing the composite conductive agent according to claim 6, characterized in that: In step (2), the heating temperature is 70-90°C.
9. A positive electrode, characterized in that The positive electrode comprises a positive electrode active material, an electrolyte, a binder and the composite conductive agent according to any one of claims 1 to 5.
10. An all-solid-state battery, characterized in that: The all-solid-state battery comprises the positive electrode according to claim 9.
Citation Information
Patent Citations
Porous plastic crystal electrolyte for all-solid-state metal-air battery, preparation method of porous plastic crystal electrolyte and all-solid-state metal-air battery
CN111269509A
Organic ion plastic crystal doped composite electrolyte membrane and preparation method and application thereof
CN115224357A
Sulfide solid electrolyte elastic membrane, preparation method thereof and lithium ion battery
CN117996165A
Lithium-ion rechargeable accumulators including an ionic liquid electrolyte
US20110206979A1
Electrolyte, secondary battery, battery module, battery pack, and electric device
WO2023221113A1