Solid-state battery cell assembly, preparation method thereof, battery and application of solid-state battery cell assembly
By introducing a base film layer into the solid-state battery cell assembly to absorb the electrolyte, the problem of large solid-solid interface impedance in solid-state batteries is solved, and the electrochemical performance and stability of the battery are improved.
Patent Information
- Application Number
- CN202310398807.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-18
AI Technical Summary
The solid-solid interface resistance between the solid electrolyte and the positive and negative electrodes of solid-state batteries is large, which affects battery performance.
A base film layer is introduced into the solid battery cell assembly. The base film absorbs the electrolyte and is placed between the positive electrode and the solid electrolyte layer and/or between the negative electrode and the solid electrolyte layer to reduce the direct contact between the electrode and the solid electrolyte and improve the interface. Infiltration.
It significantly reduces the solid-solid interface impedance, improves the electrochemical performance and stability of solid-state batteries, and enhances the cycle performance and safety of the battery.
Smart Images

Figure CN118801043A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to solid-state battery cell components and preparation methods thereof, batteries and applications thereof. Background Art
[0002] Solid-state batteries are a new type of battery with solid electrolytes. Compared with traditional liquid batteries, solid-state batteries have higher energy density and better safety.
[0003] Since solid-state batteries contain solid electrolytes, the solid electrolytes contained in solid-state batteries have solid-solid interface contact with the positive and negative electrodes, which is different from the solid-liquid contact of traditional liquid batteries. Through research, it is found that it is precisely because of the solid-solid interface contact between the solid electrolyte of solid-state batteries and the positive and negative electrodes that the impedance of the solid-solid interface is large, which greatly affects the battery performance. Summary of the invention
[0004] In view of the above problems, the embodiments of the present application provide a solid-state battery cell assembly and a preparation method thereof, a positive electrode, a battery and an electrical device, and an energy storage device to solve the technical problem of high solid-state interface impedance between electrodes and solid electrolytes in existing solid-state battery cell assemblies.
[0005] In a first aspect, an embodiment of the present application provides a solid-state battery cell assembly. The solid-state battery cell assembly of the embodiment of the present application includes a positive electrode and a negative electrode and a solid electrolyte layer disposed between the positive electrode and the negative electrode, and a base film is further disposed between the positive electrode and the solid electrolyte layer and / or between the negative electrode and the solid electrolyte layer, and the base film is adsorbed with an electrolyte.
[0006] The base film contained in the solid-state battery cell assembly of the embodiment of the present application can effectively reduce the direct contact between the electrolyte adsorbed by the base film and the electrode (positive electrode and / or negative electrode) and the solid electrolyte layer, and can reduce the consumption of electrolyte during the charging and discharging process. At the same time, it also reduces the absorption of electrolyte by the solid electrolyte layer, and maintains the electrolyte to have a good and stable wetting effect on the solid-solid interface between the electrode and the solid electrolyte layer, thereby significantly reducing the impedance between the solid-solid interface, so as to effectively improve the electrochemical performance of the solid-state battery and the stability of the electrochemical performance.
[0007] In some embodiments, the amount of electrolyte adsorbed per unit area of the base film is 1 to 100 μL cm -2 The adsorbed amount of electrolyte can improve the wettability of the electrolyte to the solid-solid interface between the electrode and the solid electrolyte layer in the solid-state battery cell assembly, thereby reducing the interface impedance.
[0008] In some embodiments, the base film adsorbed with the electrolyte has at least any one of the following (1) to (3):
[0009] (1) The thickness of the single base film is 0.1 to 100 μm;
[0010] (2) Ionic conductivity is 10 -2 ~10 -1 S cm -1 ;
[0011] (3) 0<Electron conductivity≤10 -10 S cm -1 .
[0012] The base membrane adsorbed with the electrolyte having the above characteristics has high ionic conductivity and low electronic conductivity, improves the wettability of the solid-solid interface between the electrode and the solid electrolyte layer in the solid-state battery cell assembly, effectively reduces the interface impedance, and improves the energy density of the solid-state battery cell assembly 10.
[0013] In some embodiments, the base film is bonded to the surface of the solid electrolyte layer.
[0014] In some embodiments, the base film is bonded to a surface of the positive electrode facing the solid electrolyte layer.
[0015] In some embodiments, the base film is bonded to a surface of the negative electrode facing the solid electrolyte layer.
[0016] When the base film is stacked and combined on the positive electrode, solid electrolyte layer and negative electrode surface in the above manner, the stability of the base film in the solid-state battery cell assembly can be enhanced, thereby improving the wettability of the solid-solid contact interface between the electrode and the solid electrolyte layer in the solid-state battery cell assembly, reducing the impedance of the solid-solid contact interface, and improving the safety of the solid-state battery cell assembly.
[0017] In some embodiments, the electrolyte includes at least any one of the following (1) to (4):
[0018] (1) The molar concentration of the electrolyte contained in the electrolyte solution is 0.1 to 5 mol / L;
[0019] (2) The electrolyte contained in the electrolyte includes at least one of lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(oxalatoborate) (LiBOB), and lithium difluorooxalatoborate (LiODFB);
[0020] (3) The solvent contained in the electrolyte includes at least one of cyclic carbonate, chain carbonate, cyclic carboxylate, chain carboxylate, cyclic ether, chain ether, dimethyl sulfoxide, and cyclopentane;
[0021] (4) The electrolyte further contains an additive.
[0022] The electrolyte with the above characteristics has high ionic conductivity and low electronic conductivity, improves the wettability of the solid-solid interface between the electrode and the solid electrolyte layer in the solid-state battery cell assembly, effectively reduces the interface impedance, and improves the cycle performance of the solid-state battery cell assembly 10.
[0023] In the embodiment, the mass percentage of the additive in the electrolyte is 0.1-10%.
[0024] In an embodiment, the additive includes at least one of fluoroethylene carbonate, vinylene carbonate, vinyl ethylene carbonate, ethyl allyl carbonate, vinyl acetate, catechol cyclic carbonate, and lithium difluorooxalatoborate.
[0025] The additive components of this concentration and type can effectively reduce the ohmic impedance and charge transfer impedance of the electrode interface such as the lithium metal interface, and improve the mechanical strength of the solid electrolyte interface (SEI) film.
[0026] In some embodiments, the base film includes at least any one of the following (1) to (6):
[0027] (1) Porosity is 30-60%;
[0028] (2) Air permeability is 100-1000s / 100ml;
[0029] (3) The liquid absorption capacity is 40 to 1000%.
[0030] (4) Tensile strength: transverse > 8N / 25mm, longitudinal > 15N / 25mm;
[0031] (5) Elongation: transverse > 300%, longitudinal > 180%;
[0032] (6) Needle puncture resistance> 20N.
[0033] The base membrane with the above characteristics can effectively absorb an appropriate amount of electrolyte, thereby improving the wettability between the solid-solid interface of the electrode and the solid electrolyte layer, thereby reducing the impedance between the solid-solid interface; at the same time, it has good mechanical strength, stable morphology, and is not easy to deform, which improves the stability of the electrolyte load in the base membrane and the wettability between the solid-solid interface of the electrode and the solid electrolyte layer, and can effectively improve the safety performance of the solid-state battery cell assembly 10.
[0034] In some embodiments, the base film includes a polymer film. The polymer film can give the base film good electrolyte absorption performance and good mechanical properties, so that the amount and stability of the electrolyte loaded by the base film can be effectively adjusted, the wettability between the solid-solid interface of the electrode and the solid electrolyte layer can be improved, and the interface impedance can be reduced.
[0035] In an embodiment, the polymer of the polymer film includes at least one of crystalline saturated polyester, dimethylsiloxane cross-linked polymer, polyolefin, halogenated polyolefin, and MOF structural material.
[0036] In an exemplary embodiment, the crystalline saturated polyester includes at least one of PET, crystalline dimer acid polyester polyol, crystalline polyester imide, polybutylene terephthalate, polyethylene terephthalate-1,4-cyclohexanedimethanol, and VYLON polyester resin.
[0037] In an exemplary embodiment, the dimethylsiloxane cross-linked polymer includes at least one of vinyl dimethylsiloxane cross-linked polymer, amino dimethylsiloxane cross-linked polymer, and aminopropyl dimethylsiloxane.
[0038] In an exemplary embodiment, the polyolefin and the halogenated polyolefin independently include at least one of polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, polyvinyl chloride, polyvinylidene chloride and polyvinylidene fluoride.
[0039] In an exemplary embodiment, the MOF structural material includes at least one structural material of IRMOF series, ZIF series, CPL series, MIL series, PCN series, and UiO series.
[0040] In the exemplary embodiment, the IFMOF series structural materials include at least one of IRMOF-1, IRMOF-3, IRMOF-4, IRMOF-8, IRMOF-9, IRMOF-10, IRMOF-11, IRMOF-12, IRMOF-13, IRMOF-14, IRMOF-16, IRMOF-18, IRMOF-61, IRMOF-62, IRMOF-3-AM1, Fe / IRMOF-3, Mg-IRMOF-74, IRMOF-3-OH, IRMOF-3-SH, Fe / IRMOF-3-900, and IRMOF3-sal.
[0041] In the example, the ZIF series structural materials include IF-1, ZIF-2, ZIF-4, ZIF-5, ZIF-7, ZIF-8, nZIF-8, ZIF-9, ZIF-10, ZIF-11, ZIF-12, ZIF-14, ZIF-20, ZIF-23, ZIF-60, ZIF-61, ZIF-62, ZIF-64, Z At least one of IF-65, ZIF-67, ZIF-68, ZIF-69, ZIF-70, ZIF-71, ZIF-72, ZIF-73, ZIF-74, ZIF-75, ZIF-76, ZIF-77, ZIF-78, ZIF-95, ZIF-100, ZIF-268, ZIF-224, and Zn / Co-ZIF.
[0042] In an exemplary embodiment, the CPL series structural material includes at least one of CPL-5Cu, CPL-5Cu, CPL-5Cu, CPL-5Cu, and CPL-5Cu.
[0043] In the exemplary embodiment, the MIL series structural materials include at least one of MIL-53Cr, MIL-100Cr, MIL-101Cr, MIL-100Fe, MIL-177-LT, MIL-177-HT, MIL-45Co, MIL-45Fe, MIL-53AI, MIL-53Sc, MIL-88Sc, MIL-8, MIL-9, MIL-47, MIL-51, MIL-59, MIL-69, MIL-88, MIL-91, MIL-96, MIL-101, MIL-103, MIL-102, MIL-110, and MIL-125.
[0044] In the exemplary embodiment, the PCN structural material includes at least one of PCN-6, PCN-9, PCN-12, PCN-13, PCN-14, PCN-18, PCN-22, PCN-51, PCN-61, PCN-63, PCN-100, PCN-129, PCN-131, PCN-132, PCN-137, PCN-149, PCN-150, PCN-222, PCN-224, PCN-308, and PCN-333.
[0045] In an exemplary embodiment, the UiO series structural material includes at least one of UiO-66, UiO-67 and UiO-68.
[0046] The base membrane containing the above-mentioned types of polymers has a reasonable porosity, strong liquid absorption capacity, and stable electrochemical performance. It can stably adsorb the electrolyte inside the polymer, improve the stability of the electrolyte loading, thereby improving the wettability of the electrolyte to the solid-solid interface and improving the safety performance of solid-state battery cell components.
[0047] In a second aspect, the present application provides a method for preparing a solid-state battery cell assembly. The method for preparing a solid-state battery cell assembly in the present application comprises the following steps:
[0048] Providing positive electrode, negative electrode and solid electrolyte membrane;
[0049] The positive electrode, the solid electrolyte membrane and the negative electrode are stacked, and a stacked base membrane is provided between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane;
[0050] Wherein, the base film absorbs electrolyte.
[0051] The method for preparing a solid-state battery cell assembly in the embodiment of the present application can form a base film adsorbed with electrolyte between the electrode and the solid electrolyte membrane contained in the prepared solid-state battery cell assembly, giving the base film adsorbed with electrolyte high ionic conductivity and low electronic conductivity, and having a good and stable wetting effect on the solid-solid interface between the electrode and the solid electrolyte membrane, thereby significantly reducing the solid-solid interface impedance.
[0052] In some embodiments, the method of providing a stacked base film between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane comprises the following steps:
[0053] forming the base film on at least one of a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte film;
[0054] Loading the electrolyte into the base film;
[0055] The positive electrode, the solid electrolyte membrane and the negative electrode are stacked, and the base membrane adsorbed with the electrolyte is stacked between the positive electrode and the solid electrolyte layer and / or between the negative electrode and the solid electrolyte layer.
[0056] Directly forming a base film on at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane can enhance the bonding strength between the base film and at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane, thereby enhancing the wettability of the electrolyte to the solid-solid interface of the electrode (at least one of the positive electrode and the negative electrode) and the solid electrolyte membrane and the structural stability of the solid-state battery cell assembly.
[0057] In an embodiment, the base film comprises a polymer film, and a method for forming the base film on at least one of a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte film comprises the following steps:
[0058] Forming a mixed solution including a polymer monomer, a solvent, and an initiator on a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte membrane to obtain a polymer precursor film;
[0059] The polymer precursor film is subjected to a polymer reaction to generate the base film.
[0060] An in-situ base film is directly formed on at least one of a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte membrane, thereby effectively enhancing the bonding strength between the base film and the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane.
[0061] In the exemplary embodiment, the film forming method includes at least one of molecular layer deposition, scraping, spraying, spin coating, and casting. The use of these methods for film forming can improve the quality and efficiency of the base film, and can adjust and improve the performance and stability of the base film in adsorbing electrolyte.
[0062] In the embodiment, before the step of forming the base film on at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane, the step of plasma-treating at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane is also included, and the base film is formed on the surface treated with the plasma. Plasma treatment of the base film carrier can etch the corresponding surface, remove the surface impurity layer, defect layer, etc., and can also increase the surface energy of the surface, thereby increasing the bonding strength between the base film and at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane.
[0063] In some embodiments, the method of providing a stacked base film between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane comprises the following steps:
[0064] providing a basement membrane;
[0065] Loading the electrolyte into the base film;
[0066] The positive electrode, the solid electrolyte film, the negative electrode, and the base film on which the electrolyte solution is adsorbed are stacked.
[0067] By adopting the method of separately preparing the base film adsorbed with electrolyte, the base film adsorbed with electrolyte can be prepared simultaneously with the positive electrode, the negative electrode and the solid electrolyte membrane, thereby effectively improving the efficiency and flexibility of preparing solid-state battery cell components, and also improving the quality stability of solid-state battery cell components.
[0068] In a third aspect, the present invention provides a battery. The battery of the present invention comprises a solid-state battery cell assembly of the present invention or a solid-state battery cell assembly prepared by a method for preparing a solid-state battery cell assembly of the present invention.
[0069] The battery cycle performance of the embodiment of the present application is significantly improved, and the electrochemical performance including rate and battery safety is also significantly improved.
[0070] In a fourth aspect, an embodiment of the present application provides an electric device. The electric device of the embodiment of the present application includes a battery as in the embodiment of the present application, and the battery is used to provide electric energy. The electric device of the embodiment of the present application has a long standby or battery life.
[0071] In a fifth aspect, the embodiment of the present application further provides an energy storage device, including the battery of the embodiment of the present application. The capacity of the energy storage device of the embodiment of the present application can be improved and the service life can be extended.
[0072] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0073] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0074] Figure 1 A schematic diagram of the structure of a solid-state battery cell assembly according to an embodiment of the present application;
[0075] Figure 2 Another structural schematic diagram of a solid-state battery cell assembly according to an embodiment of the present application;
[0076] Figure 3 This is another structural schematic diagram of a solid-state battery cell assembly according to an embodiment of the present application;
[0077] Figure 4 This is a schematic diagram of the structure of the interface modification layer contained in the solid-state battery cell assembly of the embodiment of the present application;
[0078] Figure 5 This is a schematic diagram of a process for preparing a solid-state battery cell assembly according to an embodiment of the present application;
[0079] Figure 6This is a schematic structural diagram of an implementation of a solid-state battery cell according to an embodiment of the present application;
[0080] Figure 7 for Figure 6 An exploded schematic diagram of a solid-state battery cell is shown;
[0081] Figure 8 This is a schematic structural diagram of an implementation scheme of a battery module according to an embodiment of the present application;
[0082] Fig. 9 This is a schematic structural diagram of an implementation scheme of a battery pack according to an embodiment of the present application;
[0083] Fig.10 for Fig. 9 A schematic diagram of the exploded structure of the battery pack shown;
[0084] Fig.11 It is a schematic diagram of an implementation of an electrical device including the secondary battery of an embodiment of the present application as a power source.
[0085] The reference numerals in the specific implementation manner are as follows:
[0086] 10-solid-state battery cell assembly 10, 11-positive electrode, 12-solid electrolyte layer, 13-negative electrode, 14-interface modification layer, 141-base film, 142-electrolyte;
[0087] 20-solid-state battery cell, 21-housing, 22-cover plate;
[0088] 30-battery module;
[0089] 40 -battery pack, 41 -box, 42 -lower box. DETAILED DESCRIPTION
[0090] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0091] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0092] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0093] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0094] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0095] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0096] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0097] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0098] In the context of energy conservation and emission reduction, new energy technologies are developing rapidly, among which the research breakthroughs and applications of battery technology are the most significant.
[0099] As battery applications become more and more extensive, especially in recent years with the rapid development of electric vehicles, power batteries have developed rapidly and the demand has increased dramatically. At the same time, the safety performance of batteries has also received more and more attention. Solid-state batteries have higher safety, mechanical strength and energy density than traditional liquid batteries, and are considered to be one of the important development directions of future batteries.
[0100] Solid-state batteries are a type of battery that uses solid electrodes and solid electrolytes. Since solid-state batteries contain solid electrolytes, the solid electrolytes contained in solid-state batteries are in solid-solid interface contact with the positive and negative electrodes, which is different from the solid-liquid contact of traditional liquid batteries. As the research on solid-state batteries gradually deepens, it is found in use and research that it is precisely because the solid electrolytes of solid-state batteries are in solid-solid interface contact with the positive and negative electrodes that the impedance of the solid-solid interface is large, which greatly affects the battery performance and also hinders the further improvement of the performance of solid-state batteries. For example, it has been tested that the contact impedance value of the solid-solid interface of the positive electrode-electrolyte of the all-solid-state battery without any modification is >100Ω, which is more than an order of magnitude larger than the contact impedance of the solid-liquid interface of the liquid electrolyte, which seriously hinders the lithium ion transmission at the interface. These inherent shortcomings lead to large polarization voltage and poor rate performance of all-solid-state batteries, and even in severe cases, they cannot be charged and discharged normally.
[0101] At present, the conventional solution to the problem of excessive solid-solid interface contact impedance between the electrodes and solid electrolytes of solid-state batteries is to add a small amount of wetting agent or liquid electrolyte at the solid-solid interface to reduce the solid-solid interface contact impedance. However, since the nanopores of the solid electrolyte will absorb the wetting agent or electrolyte, and the wetting agent added to the solid-solid interface, especially the electrolyte, is gradually consumed during the charge and discharge process, which again leads to an increase in the solid-solid interface contact impedance, the addition of electrolyte cannot fundamentally solve the solid-solid contact problem of all-solid batteries.
[0102] There are also reports that a transition layer containing trans-isomerized plastic crystals and lithium salts is added between the solid-solid interface of the solid-state battery, or a buffer layer containing lithium fluoride and carbon materials is added between the solid-solid interface of the positive electrode and the solid electrolyte layer, in an attempt to improve the impedance between the solid-solid interface of the solid-state battery. However, studies have found that although the transition layer containing trans-isomerized plastic crystals and lithium salts added to the solid-solid interface can alleviate the impedance of the solid-solid interface to a certain extent, the buffer layer formed by the solidification of trans-isomerized plastic crystals has poor consistency, which still leads to low ionic conductivity of the solid-solid interface and unsatisfactory impedance of the solid-solid interface; the lithium fluoride contained in the buffer layer containing lithium fluoride and carbon materials added to the solid-solid interface is electrochemically inert and almost electrically insulating (both ionic and electronic conductivity are very low), and the electronic conductivity of carbon materials is high, but both are solid-phase materials, and the solid-solid interface contact between the positive electrode and the solid electrolyte cannot be improved to reduce the effect of interface impedance.
[0103] In order to effectively reduce the impedance between the solid-solid interface of the solid-state battery and maintain a stable low impedance of the solid-solid interface, it has been found that the electrolyte is adsorbed in the base film to form a composite film, and the composite film is arranged between the solid-solid interface as an interface modification layer between the electrode and the solid electrolyte interface, which can effectively reduce the direct contact between the electrode and the solid electrolyte and the electrolyte, thereby effectively reducing the consumption of the electrolyte during the charging and discharging process, and also reducing the absorption of the electrolyte by the solid electrolyte, ensuring the stability of the base film to the electrolyte load, and giving the composite film formed by the electrolyte and the base film high ionic conductivity and low electronic conductivity, which has a good wetting effect on the solid-solid interface, thereby significantly reducing the impedance between the solid-solid interface, thereby effectively improving the electrochemical performance of the solid-state battery. Based on this study, the following application scheme is proposed.
[0104] Solid-state battery cell components
[0105] In a first aspect, the present application provides a solid-state battery cell assembly. In some embodiments, the structure of the solid-state battery cell assembly of the present application is as follows: Figures 1 to 4 As shown, the solid-state battery cell assembly 10 of the embodiment of the present application includes a positive electrode 11 and a negative electrode 13 and a solid electrolyte layer 12 disposed between the positive electrode 11 and the negative electrode 13. An interface modification layer 14 is also disposed between the positive electrode 11 and the solid electrolyte layer 12 and / or between the negative electrode 13 and the solid electrolyte layer 12.
[0106] The structure of the interface modification layer 14 contained in the solid-state battery cell assembly 10 of the present embodiment is as follows: Figure 4As shown, the interface modification layer 14 includes a base film 141, and the base film 141 is adsorbed with an electrolyte 142. Based on the structure defined by the interface modification layer 14, it can be understood that the base film 141 is arranged between the positive electrode 11 and the solid electrolyte layer 12 and / or between the negative electrode 13 and the solid electrolyte layer 12, and the electrolyte 142 is adsorbed in the base film 141.
[0107] In the solid-state battery cell assembly 10 of the present embodiment, the interface modification layer 14 contained therein refers to a composite membrane structure including the base film 141 and the electrolyte 142 adsorbed therein. Among them, the base film 141 adsorbing the electrolyte 142 means that the electrolyte 132 is arranged or filled in the base film 141, such as Figure 4 shown.
[0108] Therefore, in the interface modification layer 14, the base film 141 constitutes a carrier of the electrolyte 142, which can effectively adsorb the electrolyte 142 inside the base film 141, improve the stability of the electrolyte 142 loaded in the interface modification layer 14, and give the interface modification layer 14 high ionic conductivity and low electronic conductivity. The interface modification layer 14 is arranged between the solid-solid interface of the positive electrode 11 and the solid electrolyte layer 12 and / or between the solid-solid interface of the negative electrode 13 and the solid electrolyte layer 12, that is, between the solid-solid interface of the electrode and the solid electrolyte layer 12. In this way, based on the structural characteristics of the interface modification layer 14, the direct contact between the electrolyte 142 contained in the interface modification layer 14 and the electrode (positive electrode 11 or / and negative electrode 13) and the solid electrolyte layer 12 can be effectively reduced, thereby effectively reducing the consumption of the electrolyte 142 during the charging and discharging process, and at the same time, the absorption of the electrolyte 142 by the solid electrolyte layer 12 is also reduced, and the interface modification layer 14 is maintained. The solid-solid interface between the electrode (positive electrode 11 or / and negative electrode 13) and the solid electrolyte layer 12 has a good and stable wetting effect, thereby significantly reducing the impedance between the solid-solid interface, so as to effectively improve the electrochemical properties of the solid-state battery, such as the cycle performance and the stability of the electrochemical performance.
[0109] The solid electrolyte layer 12 contained in the solid-state battery cell assembly 10 of the embodiment of the present application is arranged between the positive electrode 11 and the negative electrode 13, which can be understood as the positive electrode 11, the solid electrolyte layer 12 and the negative electrode 13 are stacked in sequence. Specifically, the solid electrolyte layer 12 has two opposite surfaces, the positive electrode 11 is arranged on one of the surfaces close to the solid electrolyte layer 12, and the negative electrode 13 is arranged on the other surface close to the solid electrolyte layer 12. When the solid-solid interface between the positive electrode 11 and the solid electrolyte layer 12 does not contain an interface modification layer 14 or other functional film layers, the positive electrode 11 and the solid electrolyte layer 12 are stacked. Similarly, when the solid-solid interface between the negative electrode 13 and the solid electrolyte layer 12 does not contain an interface modification layer 14 or other functional film layers, the negative electrode 13 and the solid electrolyte layer 12 are stacked.
[0110] Therefore, in the embodiments, the interface modification layer 14 is disposed between the positive electrode 11 and the solid electrolyte layer 12 and / or between the negative electrode 13 and the solid electrolyte layer 12, which can be understood as a stacked arrangement.
[0111] The interface modification layer 14 is provided between the positive electrode 11 and the solid electrolyte layer 12 and / or between the negative electrode 13 and the solid electrolyte layer 12, which may include at least the following solutions:
[0112] In the embodiment, Figure 1 As shown, the interface modification layer 14 is disposed between the positive electrode 11 and the solid electrolyte layer 12. In this case, the interface modification layer 14 is not disposed between the negative electrode 13 and the solid electrolyte layer 12.
[0113] In the embodiment, based on Figure 1 The interface modification layer 14 is provided at a position shown, and one surface of the interface modification layer 14 can be laminated and bonded on the surface of the solid electrolyte layer 12 close to the positive electrode 11, and the other surface can be laminated and bonded to the surface of the positive electrode 11. In the embodiment, one surface of the interface modification layer 14 can also be laminated and bonded on the surface of the positive electrode 11 close to the solid electrolyte layer 12, and the other surface can be laminated and bonded to the surface of the solid electrolyte layer 12. In the embodiment, one surface of the interface modification layer 14 can also be laminated and bonded on the surface of the solid electrolyte layer 12 close to the positive electrode 11, and the other surface can be laminated and bonded on the surface of the positive electrode 11 close to the solid electrolyte layer 12.
[0114] In the embodiment, Figure 2 As shown, the interface modification layer 14 is disposed between the negative electrode 13 and the solid electrolyte layer 12. In this case, the interface modification layer 14 is not disposed between the positive electrode 11 and the solid electrolyte layer 12.
[0115] In the embodiment, based on Figure 2 The interface modification layer 14 is provided at a position shown, and one surface of the interface modification layer 14 can be laminated and bonded on the surface of the solid electrolyte layer 12 close to the negative electrode 13, and the other surface can be laminated and bonded to the surface of the negative electrode 13. In the embodiment, one surface of the interface modification layer 14 can also be laminated and bonded on the surface of the negative electrode 13 close to the solid electrolyte layer 12, and the other surface can be laminated and bonded to the surface of the solid electrolyte layer 12. In the embodiment, one surface of the interface modification layer 14 can also be laminated and bonded on the surface of the solid electrolyte layer 12 close to the negative electrode 13, and the other surface can be laminated and bonded on the surface of the negative electrode 13 close to the solid electrolyte layer 12.
[0116] In the embodiment, Figure 3 As shown, the interface modification layer 14 is disposed between the positive electrode 11 and the solid electrolyte layer 12. At this time, the interface modification layer 14 is also disposed between the negative electrode 13 and the solid electrolyte layer 12.
[0117] In the embodiment, based on Figure 3 The interface modification layer 14 is set at the position shown in the figure. The interface modification layer 14 set between the positive electrode 11 and the solid electrolyte layer 12 and the surface of the positive electrode 11 and the solid electrolyte layer 12 can be set as shown in the figure. Figure 1 The configuration of the interface modification layer 14 between the positive electrode 11 and the solid electrolyte layer 12; the configuration of the interface modification layer 14 between the negative electrode 13 and the solid electrolyte layer 12 and the negative electrode 13 and the solid electrolyte layer 12 can refer to Figure 2 The configuration of the interface modification layer 14 and the surfaces of the negative electrode 13 and the solid electrolyte layer 12 .
[0118] The above-mentioned stacking and bonding can be understood as requiring a certain external force to separate the two layers, such as when one surface of the interface modification layer 14 is stacked and bonded with one surface of the solid electrolyte layer 12, a certain external force is required to separate the two film layers. The above-mentioned lamination is relative to the stacking and bonding, and can be understood as requiring no external force to separate the two layers, such as when one surface of the interface modification layer 14 is laminated and bonded with one surface of the solid electrolyte layer 12, a certain external force is not required to separate the two film layers.
[0119] When the interface modification layer 14 is stacked and bonded on the surfaces of the positive electrode 11, the solid electrolyte layer 12 and the negative electrode 13, the stability of the interface modification layer 14 in the solid-state battery cell assembly 10 can be enhanced, thereby improving the wettability of the solid-solid contact interface between the electrode and the solid electrolyte layer 12 in the solid-state battery cell assembly 10, reducing the impedance of the solid-solid contact interface, and improving the safety of the solid-state battery cell assembly 10.
[0120] Based on the role of the interface modification layer 14 in the solid-state battery cell assembly 10 of the present embodiment of the application, due to Figure 3 As shown, the interface modification layer 14 is provided between the positive electrode 11 and the solid electrolyte layer 12 and between the negative electrode 13 and the solid electrolyte layer 12. Figure 3 The solid-solid interface between the electrode of the solid-state battery cell assembly 10 and the solid electrolyte layer 12 of the embodiment of the present application is good in wettability, and the impedance is relatively Figure 2 and Figure 3 The solid-state battery cell assembly 10 shown in the embodiment of the present application is lower.
[0121] In the embodiment, Figure 1 As shown, the interface modification layer 14 is disposed between the positive electrode 11 and the solid electrolyte layer 12. In this case, the interface modification layer 14 is not disposed between the negative electrode 13 and the solid electrolyte layer 12.
[0122] In the embodiment, Figure 2As shown, the interface modification layer 14 is disposed between the negative electrode 13 and the solid electrolyte layer 12. In this case, the interface modification layer 14 is not disposed between the positive electrode 11 and the solid electrolyte layer 12.
[0123] In the embodiment, Figure 3 As shown, the interface modification layer 14 is disposed between the positive electrode 11 and the solid electrolyte layer 12. At this time, the interface modification layer 14 is also disposed between the negative electrode 13 and the solid electrolyte layer 12.
[0124] In the embodiment, the positive electrode 11 contained in the solid-state battery cell assembly 10 of the embodiment of the present application may include a positive electrode current collector and a positive electrode active layer combined with the positive electrode current collector. Among them, the positive electrode active layer may be combined on the surface of the positive electrode current collector. Of course, when the positive electrode current collector is a porous structure, the positive electrode active layer may also be embedded in the positive electrode current collector.
[0125] The positive electrode current collector is generally a structure or part that can collect current. It can be various materials in the art that are suitable for use as a positive electrode current collector for an electrochemical energy storage device. As in the exemplary embodiment, the positive electrode current collector can generally be in sheet form, and its material can include but is not limited to metal foil, and more specifically can include but is not limited to nickel foil and aluminum foil. As in the exemplary embodiment, the positive electrode 11 is a positive electrode sheet, that is, the positive electrode current collector is in sheet form, having two opposite surfaces, and the positive electrode active layer is combined on one surface or both surfaces of the sheet-like positive electrode current collector. Of course, when the sheet-like positive electrode current collector is a porous structure, the positive electrode active layer can be further combined in the porous structure of the sheet-like positive electrode current collector.
[0126] The positive electrode active layer contained in the positive electrode 11 may contain components such as positive electrode active materials, conductive agents and binders. The types and contents of the components such as positive electrode active materials, binders and conductive agents are not specifically limited and can be selected and controlled according to actual needs.
[0127] As an example, the positive electrode active material may include at least one of a lithium iron phosphate positive electrode material, a ternary positive electrode material, a lithium manganese-rich positive electrode material, and the like.
[0128] In an exemplary embodiment, the binder may be one or more of polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethylcellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives.
[0129] In an exemplary embodiment, the conductive agent may include one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60, and carbon nanotubes.
[0130] In the embodiment, the negative electrode 13 contained in the solid-state battery cell assembly 10 of the embodiment of the present application can be similar to the positive electrode structure, such as including a negative electrode current collector and a negative electrode active layer combined with the negative electrode current collector. Among them, the negative electrode active layer can be combined on the surface of the negative electrode current collector. Of course, when the negative electrode current collector is a porous structure, the negative electrode active layer can also be embedded in the negative electrode current collector.
[0131] The negative electrode current collector is usually also a structure or part that can collect current. It can be various materials in the art that are suitable for use as negative electrode current collectors for electrochemical energy storage devices. As in the exemplary embodiment, the negative electrode current collector can usually be in sheet form, and its material can include but is not limited to metal foil, and more specifically can include but is not limited to copper foil. As in the exemplary embodiment, the negative electrode 13 is a negative electrode sheet, that is, the negative electrode current collector is in sheet form, having two opposite surfaces, and the negative electrode active layer is combined on one surface or both surfaces of the sheet-like negative electrode current collector. Of course, when the sheet-like negative electrode current collector is a porous structure, the negative electrode active layer can be further combined in the porous structure of the sheet-like negative electrode current collector.
[0132] The negative electrode active layer contained in the negative electrode 13 may contain components such as negative electrode active materials, conductive agents, and binders. The types and contents of the components such as negative electrode active materials, binders, and conductive agents are not specifically limited and can be selected and controlled according to actual needs.
[0133] As an example, the negative electrode active material may include at least one of a carbon-based material, a silicon-based material, and the like.
[0134] In an exemplary embodiment, the binder may be one or more of soluble styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), polyacrylic acid binder (PA series), etc.
[0135] In an exemplary embodiment, the conductive agent may include one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60, and carbon nanotubes.
[0136] In addition, the negative electrode 13 may also be a lithium metal negative electrode.
[0137] In the embodiment, the solid electrolyte layer 12 contained in the solid-state battery cell assembly 10 of the embodiment of the present application may include at least one of an inorganic solid electrolyte (ISE), a solid polymer electrolyte (SPE) and a composite polymer electrolyte (CPE). Among them, the inorganic solid electrolyte (ISE) may include inorganic solid electrolytes such as oxides, sulfides, and halides. For example, in the exemplary embodiment, the oxide may include at least one of garnet-type lithium lanthanum zirconium oxide (LLZO), NASICON type, and LISICON type, wherein the NASICON type oxide solid electrolyte is AM′M″P3O 12The molecular formula is sodium superionic conductor, in which A is usually a monovalent transport cation, such as at least one alkali metal ion such as Na, K, Li, etc., and the positions of M' and M" can be either divalent or trivalent cations (such as Zn 2+ Mg 2+ 、Ni 2+ Cr 3+ 、Al 3+ Sc 3+ , Fe 3+ 、In 3+ and Y 3+ etc.), or a tetravalent or pentavalent cation (such as Ti 4+ 、Zr 4+ ,Ge 4+ Sn 4+ 、V 5+ , Nb 5+ 、As 5+ In addition, P 5+ It can also be replaced by other high-valent ions such as Si 4+ 、V 5+ , Nb 5+ In the exemplary embodiment, the NASICON type oxide solid electrolyte may be but is not limited to Na3Zr2Si2PO 12 .
[0138] LISICON oxide solid electrolyte is a lithium ion conductor, which contains a solid three-dimensional anion skeleton. The skeleton ions provide a transport channel for the transfer of lithium ions. + In the interstitial position, it can migrate and conduct electricity, and the lithium ions in the interstitial have good proton exchange ability. In the exemplary embodiment, the LISICON type oxide solid electrolyte can be but is not limited to Li 4-x Ge 1-x P x S4, wherein x may be 0.01-0.99. In an exemplary embodiment, the value of x may be 0.01, 0.05, 0.1, 0.5, 0.75, 0.9, 0.99, and other typical but non-limiting values.
[0139] The sulfide may include at least one of Li2S-P2S5, Li2S-SiS2, and Li2S-B2S3, and the halide may include LiaMX4, LiaMX6, and LiaMX8, wherein M may include at least one of metals Mn, Zn, Fe, Al, Yb, etc., and X may include at least one of halogens F, Cl, Br, and I.
[0140] The base film 141 contained in the interface modification layer 14 contained in the solid-state battery cell assembly 10 of the embodiment of the present application determines the basic performance of the interface modification layer 14, and determines the mechanical performance, safety performance and other performance of the interface modification layer 14; it also determines the amount of electrolyte 142 contained in the interface modification layer 14 and the stability of the loaded electrolyte 142. Since the base film 141 adsorbs the electrolyte 142, in some embodiments, the base film 141 contains a porous structure. The porous structure can effectively adsorb the electrolyte 142 and improve the load stability of the electrolyte 142, thereby improving the wettability between the electrode in the interface modification layer 14 and the solid electrolyte layer 12 The solid-solid interface, thereby reducing the impedance between the solid-solid interface.
[0141] In some embodiments, the base film 141 included in the interface modification layer 14 includes at least one of the following (1) to (6):
[0142] (1) The porosity of the base film 141 may be 30% to 60%, further 40% to 60%, 40% to 50%, etc.; in the exemplary embodiment, the porosity may be 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc., which are typical but non-limiting; wherein the porosity refers to the percentage of the total volume of pores in the base film 141 to the total volume of the base film 141 in the natural state. The porosity within this range enables the base film 141 to effectively absorb an appropriate amount of electrolyte 142, thereby improving the wettability between the solid-solid interface of the electrode and the solid electrolyte layer 12, thereby reducing the impedance between the solid-solid interface; at the same time, it can improve the stability of the adsorption of the electrolyte 142 in the base film 141, effectively reducing the self-discharge rate of the solid-state battery cell assembly 10 of the embodiment of the present application.
[0143] (2) The air permeability of the base film 141 is 100-1000 s / 100 ml, and can further be 200-300 s / 100 ml; in the exemplary embodiment, it can be 100 s / 100 ml, 200 s / 100 ml, 300 s / 100 ml, 400 s / 100 ml, 500 s / 100 ml, 600 s / 100 ml, 700 s / 100 ml, 800 s / 100 ml, 900 s / 100 ml, 1000 s / 100 ml, etc., which are typical but non-limiting air permeabilities; wherein the air permeability refers to the degree of difficulty with which the base film 141 allows gas to pass through, such as the time allowed for 100 ml of gas to pass through the base film 141. Therefore, 100-1000 s / 100 ml means that the time allowed for 100 ml of gas to pass through the base film 141 is 100-1000 s. The air permeability within this range can, on the one hand, increase the amount of electrolyte 142 adsorbed by the base film 141 and the stability of adsorption, further reducing the impedance between the solid-solid interfaces in the solid-state battery cell assembly 10; and at the same time, it can increase the migration rate of active ions such as lithium ions.
[0144] (3) The liquid absorption of the base film 141 is 40-1000%, and can further be 70-300%. In the exemplary embodiment, it can be 40%, 100%, 200%, 300%, 400%, 500%, 600%, 700%, 800%, 900%, 1000% and other typical but non-limiting liquid absorption amounts. The liquid absorption refers to the percentage of the total weight of the base film 141 after absorbing the electrolyte 142 to the weight of the base film 141 before absorbing the electrolyte 142. The liquid absorption within this range enables the base film 141 to effectively absorb an appropriate amount of electrolyte 142, thereby improving the wettability of the solid-solid interface between the electrode and the solid electrolyte layer 12 and the electrode, reducing the lithium plating and black spot phenomenon that may be generated at the interface or electrode, and at the same time improving the energy density of the solid-state battery cell assembly 10.
[0145] (4) Tensile strength of the base film 141: 8N / 25mm<lateral, 15N / 25mm<longitudinal; further, 8N / 25mm<lateral<50N / 25mm, 15N / 25mm<longitudinal<100N / 25mm; wherein the tensile strength refers to the tensile strength of the base film 141, which reflects the ability of the base film 141 to resist damage when subjected to tension.
[0146] (5) The elongation of the base film 141: 300% < transverse direction, 180% < longitudinal direction; further, 300% < transverse direction < 1000%, 180% < longitudinal direction < 500%; wherein the elongation refers to the elongation at break of the base film 141. In (4) and (5), the transverse direction refers to the direction perpendicular to the length of the base film 141, and the longitudinal direction refers to the direction along the length of the base film 141.
[0147] (6) The needle puncture resistance of the base film 141 is greater than 0.3N / μm, and further, 0.5N / μm<puncture resistance<5N / μm; wherein the puncture resistance refers to the anti-destructive ability of the base film 141, such as the confinement effect, which inhibits lithium dendrites and prevents lithium dendrites from piercing the diaphragm.
[0148] (7) The thickness of the base film 141 can be controlled to be 0.1 to 100 μm, and can further be 1 to 3 μm. In the exemplary embodiment, the thickness can be 0.1 μm, 1 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, etc., which are typical but non-limiting thicknesses.
[0149] The tensile strength, elongation and needle puncture resistance ranges in (4) to (6) above give the base film 141 good mechanical strength, stable morphology, and are not easy to deform, thereby improving the stability of the electrolyte 142 in the interface modification layer 14 loaded in the base film 141, improving the wettability between the solid-solid interface of the electrode and the solid electrolyte layer 12, and effectively improving the safety performance of the solid-state battery cell assembly 10. In addition, since the base film 141 constitutes the base film layer of the interface modification layer 14, the base film 141 in this thickness range determines the thickness of the interface modification layer 14. The base film 141 in this thickness range can absorb an appropriate amount of electrolyte 142, and the components play the above-mentioned role of the interface modification layer 14, and improve the energy density of the solid-state battery cell assembly 10.
[0150] In some embodiments, the base film 141 contained in the interface modification layer 14 includes a polymer film. The polymer film can give the base film 141 the good pore structure and the performance of absorbing the electrolyte 142 mentioned above (1) to (6), and at the same time has good mechanical properties, so that the amount and stability of the electrolyte 142 loaded by the base film 141 can be effectively adjusted, the wettability between the solid-solid interface of the electrode and the solid electrolyte layer 12 can be improved, the interface impedance can be reduced, and the safety performance of the solid-state battery cell assembly 10 can be improved.
[0151] In an embodiment, when the base film 141 includes a polymer film, the polymer of the polymer film includes at least one of crystalline saturated polyester, dimethylsiloxane cross-linked polymer, polyolefin, halogenated polyolefin, and MOF structural material.
[0152] In an exemplary embodiment, the crystalline saturated polyester may include at least one of polyethylene terephthalate (PET), crystalline dimer acid polyester polyol, crystalline polyester imide, polybutylene terephthalate, polyethylene terephthalate-1,4-cyclohexanedimethanol, and VYLON polyester resin.
[0153] In an exemplary embodiment, the dimethylsiloxane crosspolymer may include at least one of vinyl dimethylsiloxane crosspolymer, amino dimethylsiloxane crosspolymer, and aminopropyl dimethylsiloxane.
[0154] In an exemplary embodiment, the polyolefin and the halogenated polyolefin independently may include at least one of polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, polyvinyl chloride, polyvinylidene chloride and polyvinylidene fluoride;
[0155] In the exemplary embodiment, the MOF structural material may include at least one of the IRMOF series, ZIF series, CPL series, MIL series, PCN series, and UiO series. Among them, the IRMOF series (Isoreticular Metal-Organic Framework) is composed of separated secondary structural units [Zn4O] 6+ Inorganic groups and a series of aromatic carboxylic acid ligands are bridged and self-assembled in the form of octahedrons to form microporous crystalline materials; ZIFs series (Zeolitic imidazolate frameworks) are zeolite-like imidazolate framework materials, which are MOF materials with zeolite structures synthesized by reacting Zn(Ⅲ) or Co(Ⅲ) with imidazole ligands; CPL series (Coordination Pillared-Layer) is composed of hexacoordinated metal elements and neutral nitrogen-containing heterocyclic ligands such as 2,2'-bipyridine, 4,4'-bipyridine, phenol, etc.; MIL series (Materials of Institut Lavoisier) is synthesized using different transition metal elements and dicarboxylic acid ligands such as succinic acid and glutaric acid; PCN series (Porous Coordination Network) contains multiple cubic octahedral nanoporous cages and forms a cage-channel topological structure in space; UiO series (University of Oslo) is composed of a Zr (zirconium)-containing octahedron [Zr6O4(OH)4] connected to 12 terephthalic acid (BDC) organic ligands to form a three-dimensional microporous structure containing an octahedral central pore cage and eight tetrahedral corner cages.
[0156] The above-mentioned polymer materials can improve the mechanical properties and morphological stability of the base film 141, have reasonable porosity, strong liquid absorption capacity, stable electrochemical performance, and can stably adsorb the electrolyte inside the polymer to improve the stability of the electrolyte load, thereby improving the safety performance of the solid-state battery cell assembly 10. Moreover, these polymer materials can improve the rich pore structure of the base film 141, thereby increasing the amount of electrolyte 142 adsorbed by the base film 141, thereby improving the wettability between the solid-solid interface of the electrode and the solid electrolyte layer 12 and reducing the solid-solid interface impedance.
[0157] Among them, MOF structural materials refer to Metal-Organic Frameworks, which are coordination polymers with three-dimensional pore structures. They generally use metal ions as connection points and organic ligands as support to form a 3D extension of space.
[0158] In the exemplary embodiment, when the MOF structural material is an IFMOF series structural material, the IFMOF series structural material may include at least one of IRMOF-1, IRMOF-3, IRMOF-4, IRMOF-8, IRMOF-9, IRMOF-10, IRMOF-11, IRMOF-12, IRMOF-13, IRMOF-14, IRMOF-16, IRMOF-18, IRMOF-61, IRMOF-62, IRMOF-3-AM1, Fe / IRMOF-3, Mg-IRMOF-74, IRMOF-3-OH, IRMOF-3-SH, Fe / IRMOF-3-900, and IRMOF3-sal.
[0159] In the demonstration example, when the MOF structural material is a ZIF series structural material, the ZIF series structural materials include IF-1, ZIF-2, ZIF-4, ZIF-5, ZIF-7, ZIF-8, n ZIF-8, ZIF-9, ZIF-10, ZIF-11, ZIF-12, ZIF-14, ZIF-20, ZIF-23, ZIF-60, ZIF-61, ZIF-6 2. ZIF-64, ZIF-65, ZIF-67, ZIF-68, ZIF-69, ZIF-70, ZIF-71, ZIF-72, ZIF-73, ZIF-74, Z At least one of IF-75, ZIF-76, ZIF-77, ZIF-78, ZIF-95, ZIF-100, ZIF-268, ZIF-224, and Zn / Co-ZIF.
[0160] In an exemplary embodiment, when the MOF structural material is a CPL series structural material, the CPL series structural material includes at least one of CPL-5Cu, CPL-5Cu, CPL-5Cu, CPL-5Cu, and CPL-5Cu.
[0161] In the exemplary embodiment, when the MOF structural material is a MIL series structural material, the MIL series structural material includes at least one of MIL-53Cr, MIL-100Cr, MIL-101Cr, MIL-100Fe, MIL-177-LT, MIL-177-HT, MIL-45Co, MIL-45Fe, MIL-53AI, MIL-53Sc, MIL-88Sc, MIL-8, MIL-9, MIL-47, MIL-51, MIL-59, MIL-69, MIL-88, MIL-91, MIL-96, MIL-101, MIL-103, MIL-102, MIL-110, and MIL-125;
[0162] In the exemplary embodiment, when the MOF structural material is a PCN series structural material, the PCN structural material includes at least one of PCN-6, PCN-9, PCN-12, PCN-13, PCN-14, PCN-18, PCN-22, PCN-51, PCN-61, PCN-63, PCN-100, PCN-129, PCN-131, PCN-132, PCN-137, PCN-149, PCN-150, PCN-222, PCN-224, PCN-308, and PCN-333;
[0163] In an exemplary embodiment, when the MOF structural material is a UiO series structural material, the UiO series structural material includes at least one of UiO-66, UiO-67 and UiO-68.
[0164] The above-mentioned MOF structural materials have rich pore structures and good mechanical properties, which can effectively adjust the amount of electrolyte 142 loaded on the base membrane 141 and improve the stability of the electrolyte 142 loading, improve the wettability between the solid-solid interface between the electrode and the solid electrolyte layer 12 and reduce the interface impedance, thereby improving the safety performance of the solid-state battery cell assembly 10.
[0165] In some embodiments, it has been tested that the amount of electrolyte 142 adsorbed per unit area of the base film 141 in the above embodiments can be controlled to be 1-100 μL cm -2 , and further can be 5 to 50 μL cm -2 , in this example, it can be 1 μL cm -2 , 10 μL cm -2 , 20 μL cm -2 , 30 μL cm -2 , 40 μL cm -2 , 50 μL cm -2 , 60 μL cm -2 , 70 μL cm -2 , 80 μL cm -2 , 90 μL cm -2 , 100 μL cm -2 The amount of electrolyte 142 adsorbed by the base film 141 is controlled within this range, which can improve the good wettability of the interface modification layer 14 to the solid-solid interface between the electrode and the solid electrolyte layer 12 in the solid-state battery cell assembly 10, and effectively reduce the interface impedance.
[0166] In some embodiments, the electrolyte 142 contained in the interface modification layer 14 includes at least one of the following (1) to (4):
[0167] (1) The molar concentration of the electrolyte contained in the electrolyte solution may be 0.1 to 5 mol / L, and may further be 0.5 to 3 mol / L. In the exemplary embodiment, the molar concentration may be 0.1 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, etc., which are typical but non-limiting molar concentrations. The electrolyte solution of this molar concentration has good wettability to the solid-solid interface between the electrode and the solid electrolyte layer 12 in the solid-state battery cell assembly 10, and effectively reduces the interface impedance.
[0168] (2) The electrolyte contained in the electrolyte may include at least one of lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(oxalate)borate (LiBOB), and lithium difluorooxalateborate (LiODFB). These lithium salts are rich in lithium, can provide a large amount of active lithium ions, and have stable performance, and can improve the good wettability of the interface modification layer 14 to the solid-solid interface between the electrode and the solid electrolyte layer 12 in the solid-state battery cell component 10, effectively reducing the interface impedance.
[0169] (3) The solvent contained in the electrolyte includes at least one of cyclic carbonate, chain carbonate, cyclic carboxylic acid ester, chain carboxylic acid ester, cyclic ether, chain ether, dimethyl sulfoxide (DMSO), and sulfolane (SL). In an exemplary embodiment, the cyclic carbonate may include at least one of propylene carbonate (PC) and ethylene carbonate (EC), the chain carbonate may include at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), the cyclic carboxylic acid ester may include γ-butyrolactone (BL), the chain carboxylic acid ester may include at least one of methyl propionate (MP), methyl acetate (MA), the cyclic ether may include at least one of tetrahydrofuran (THF), 1,3-dioxolane (DOL), the chain ether may include at least one of dimethoxymethane (DMM), 1.2-dimethoxyethane (DME), etc. These solvents have stable chemical properties and can improve the ion conductivity of the electrolyte.
[0170] (4) The electrolyte also contains additives. In the embodiment, the mass percentage of the additive in the electrolyte can be 0.1-10%. In the exemplary embodiment, it can be 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% and other typical but non-limiting contents. In the exemplary embodiment, the additive can include at least one of fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), ethyl allyl carbonate (AEC), vinyl acetate (VA), catechol carbonate (CC), and lithium difluoroborate (C2BF2LiO4). By adding additive components to the electrolyte, or further controlling the concentration and type of the additive to the above range and type, the ohmic impedance and charge transfer impedance of the electrode interface such as the lithium metal interface can be effectively reduced, and the mechanical strength of the solid electrolyte interface (SEI) film can be improved.
[0171] In addition, in the embodiments, after testing, the interface modification layer 14 in each of the above embodiments has at least any one of the following (1) to (3):
[0172] (1) The thickness of the interface modification layer 14 is 0.1-100 μm, which is the thickness of the base film 141 mentioned above. Therefore, the thickness of the interface modification layer 14 can further be 1-3 μm. In the exemplary embodiment, the thickness can be 0.1 μm, 1 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, etc. Typical but non-limiting thicknesses can be selected;
[0173] (2) The ionic conductivity of the interface modification layer 14 is 10 -2 ~10 -1 S cm -1 ;
[0174] (3) The electronic conductivity of the interface modification layer 14 is greater than 0 and less than or equal to 10 -10 S cm -1 , further 10 -14 S cm -1 ≤Electronic conductivity≤10 -10 S cm -1 .
[0175] The interface modification layer 14 in the above thickness range has high ionic conductivity and low electronic conductivity, such as ionic conductivity can reach the order of magnitude of ionic conductivity of conventional liquid electrolyte, which can give full play to the above role, improve the solid-solid interface between the electrode and the solid electrolyte layer 12 in the solid-state battery cell assembly 10, and effectively reduce the interface impedance. At the same time, the energy density of the solid-state battery cell assembly 10 can be improved.
[0176] Preparation method of solid-state battery cell assembly
[0177] In a second aspect, the present application provides a method for preparing a solid-state battery cell assembly. The process flow of the method for preparing a solid-state battery cell assembly in the present application is as follows: Figure 5 As shown, the method for preparing the solid-state battery cell assembly of the embodiment of the present application may include the following steps:
[0178] S10: providing a positive electrode, a negative electrode and a solid electrolyte membrane;
[0179] S20: stacking the positive electrode, the solid electrolyte membrane and the negative electrode, and providing an interface modification layer between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane.
[0180] In the preparation method of the solid-state battery cell assembly of the embodiment of the present application, the positive electrode in step S10 is the positive electrode 11 contained in the solid-state battery cell assembly 10 of the embodiment of the above text application, the negative electrode is the negative electrode 13 contained in the solid-state battery cell assembly 10 of the embodiment of the above text application, and the solid electrolyte membrane is the solid electrolyte 12 contained in the solid-state battery cell assembly 10 of the embodiment of the above text application. Therefore, it should be understood that the positive electrode and the negative electrode are respectively arranged on opposite sides of the solid electrolyte membrane in step S20. After the interface modification layer is arranged between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane, the interface modification layer can be arranged between the positive electrode and the solid electrolyte membrane, such as Figure 1 As shown; the interface modification layer can also be arranged between the negative electrode and the solid electrolyte membrane, such as Figure 2 As shown; the interface modification layer can also be arranged between the positive electrode and the solid electrolyte membrane and between the negative electrode and the solid electrolyte membrane, such as Figure 3 As shown. Since the preparation method of the solid-state battery cell assembly of the embodiment of the present application is the preparation method of the solid-state battery cell assembly 10 of the embodiment of the above text application, the interface modification layer formed in step S20 is the interface modification layer 14 contained in the solid-state battery cell assembly 10 of the embodiment of the above text application, then the interface modification layer formed in step S20 includes a base film, and the base film is adsorbed with an electrolyte. Among them, the base film is the base film 141 contained in the interface modification layer 14 of the solid-state battery cell assembly 10 of the embodiment of the above text application, and the electrolyte adsorbed by it is the electrolyte 142 contained in the interface modification layer 14 of the solid-state battery cell assembly 10 of the embodiment of the above text application. Based on the structure of the interface modification layer 14, in step S20, a stacked base film may be provided between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane; wherein, the base film is adsorbed with an electrolyte.
[0181] Therefore, the present application embodiment solid-state battery core assembly preparation method can form an interface modification layer between the electrode (positive pole and / or negative pole) contained in the solid-state battery core assembly of the preparation and the solid electrolyte film, so that the interface modification layer is adsorbed with electrolyte, the stability of the electrolyte load in the interface modification layer is enhanced, and the interface modification layer is given high ionic conductivity and low electronic conductivity. And the consumption of the electrolyte contained in the interface modification layer during charge and discharge can be effectively reduced, while the solid electrolyte film also reduces the absorption of the electrolyte, the interface modification layer is kept to play a good and stable wetting effect on the solid-solid interface between the electrode (positive pole or / and negative pole) and the solid electrolyte film, so as to significantly reduce the impedance between the solid-solid interface, to effectively improve the electrochemical performance of the solid-state battery and the stability of the electrochemical performance. In addition, the present application embodiment solid-state battery core assembly preparation method condition is controllable, and the quality and performance stability of the solid-state battery core assembly prepared can be effectively guaranteed, and the efficiency is high.
[0182] Step S10
[0183] The positive electrode in step S10 can be prepared according to the structure and type of the positive electrode 11 contained in the solid-state battery cell assembly 10 of the above-mentioned application embodiment. For example, in the exemplary embodiment, the prepared positive electrode can be, but is not limited to, a lithium iron phosphate positive electrode, a ternary positive electrode, a lithium manganese-rich positive electrode, etc.
[0184] Similarly, the negative electrode can also be prepared according to the structure and type of the negative electrode 13 contained in the solid-state battery cell assembly 10 of the above text application embodiment. As shown in the demonstration example, the prepared negative electrode can be but not limited to a carbon-based negative electrode, a silicon-based negative electrode, a lithium metal negative electrode, etc.
[0185] The solid electrolyte membrane can also be prepared according to the type of the solid electrolyte layer 14 contained in the solid-state battery cell assembly 10 of the above application embodiment. For example, in the exemplary embodiment, the prepared solid electrolyte membrane can be, but is not limited to, an inorganic solid electrolyte membrane.
[0186] Step S20
[0187] The order of stacking the positive electrode, the solid electrolyte membrane and the negative electrode in sequence and providing an interface modification layer between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane can be determined according to the formation method of the interface modification layer.
[0188] As in the embodiment, when the interface modification layer is formed separately, the positive electrode, the solid electrolyte membrane and the negative electrode and the interface modification layer can be referred to as Figures 1 to 3 The structure of the solid-state battery cell assembly 10 shown in any one of the above can also be stacked. The positive electrode, the solid electrolyte membrane and the negative electrode can also be stacked first, and then stacked as shown in the following Figures 1 to 3In any of the solid-state battery cell components 10 structures shown in the figure, the interface modification layer is inserted and stacked at the corresponding position, such as inserted and stacked between the positive electrode and the solid electrolyte membrane, or inserted and stacked between the negative electrode and the solid electrolyte membrane, or inserted and stacked between the positive electrode and the solid electrolyte membrane and between the negative electrode and the solid electrolyte membrane at the same time.
[0189] When the interface modification layer is first formed on the surface of any one of the positive electrode, the negative electrode and the solid electrolyte membrane, the interface modification layer is first formed, and then the interface modification layer is formed according to the reference Figures 1 to 3 In any of the structures of the solid-state battery cell assembly 10 shown in the figure, the positive electrode, the solid electrolyte membrane and the negative electrode are stacked.
[0190] In some embodiments, the method of providing an interface modification layer between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane in step S20 comprises the following steps:
[0191] S21: forming a base film on at least one of a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte membrane;
[0192] S22: loading the electrolyte into the base film to form an interface modification layer;
[0193] S23: stacking the positive electrode, the solid electrolyte membrane and the negative electrode, and stacking the interface modification layer between the positive electrode and the solid electrolyte layer and / or between the negative electrode and the solid electrolyte layer.
[0194] Directly forming a base film on at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane, that is, forming an interface modification layer, can enhance the bonding strength between the interface modification layer and at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane, thereby enhancing the structural stability of the solid-state battery cell assembly 10. At the same time, the wettability of the interface modification layer to the solid-solid interface of the electrode (at least one of the positive electrode and the negative electrode) and the solid electrolyte membrane can be enhanced, reducing the impedance of the solid-solid interface.
[0195] The base film formed in step S21 is the base film 141 contained in the interface modification layer 14 of the solid-state battery cell assembly 10 of the above-mentioned embodiment of the present application. Therefore, the method of forming the base film on at least one of the surface of the positive electrode, the surface of the negative electrode, and the surface of the solid electrolyte membrane can be determined according to the material of the base film.
[0196] As in the embodiment, the method for forming a base film on at least one of a surface of a positive electrode, a surface of a negative electrode, and a surface of a solid electrolyte membrane comprises the following steps:
[0197] S211: performing film-forming treatment on a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte membrane by treating a mixed solution including a polymer monomer, a solvent, and an initiator to obtain a polymer precursor film;
[0198] S212: subjecting the polymer precursor film to a polymer reaction to generate the base film.
[0199] Wherein, the polymer monomer in step S211 is a polymer monomer for forming a base film, and in the exemplary embodiment, it can be the polymer monomer of the above-mentioned crystalline saturated polyester, dimethylsiloxane cross-linked polymer, polyolefin, halogenated polyolefin, and MOF structural material. In the exemplary embodiment, it can be a mixed monomer containing HOCH2CH2OH and ethylene glycol, a mixed monomer containing ethylene terephthalate monomer, purified terephthalic acid (PTA), 1,4-cyclohexanedimethanol (CHDM) and ethylene glycol, or a mixed monomer containing dimethyl terephthalate and 1,4-butanediol, etc. The polymer formed by these polymer monomers can give the base film good mechanical properties, and the stability of the morphology, reasonable porosity, strong liquid absorption capacity, improve the load stability of the electrolyte, thereby improving the interface modification layer to improve the wettability between the solid-solid interface of the electrode and the solid electrolyte and reduce the solid-solid interface impedance.
[0200] The solvent in step S211 should have no side effects on the positive electrode, the negative electrode and the solid electrolyte membrane, and be able to effectively dissolve components such as polymer monomers and initiators.
[0201] The initiator in step S211 should be an initiator that can promote the polymerization reaction of the polymer monomer to generate a polymer to form a base film, and can be selected specifically according to the characteristics of the polymerization reaction of the polymer monomer.
[0202] In the embodiment, the mixed solution in step S211 may further be added with corresponding film-forming modifiers, such as plasticizers, etc., to improve the corresponding properties of the base film, such as improving the mechanical properties, thereby improving the stability of the interface modification layer.
[0203] In an embodiment, the film forming method in step S211 may include at least one of molecular layer deposition, scraping, spraying, spin coating, and casting. Among them, molecular layer deposition refers to MLD molecular layer deposition (Molecular Layer Deposition), which is to introduce two reaction gases (or steam) into the reactor alternately in the form of gas pulses, and rely on the adsorbed molecules (such as hydroxyl or amino groups) left on the surface of the substrate to react to form a thin film. Using these methods for film forming treatment can improve the quality and efficiency of the base film, and can adjust and improve the performance of the base film in adsorbing the electrolyte and the stability of the adsorption.
[0204] The polymerization reaction in step S212 can be selectively controlled and adjusted according to the characteristics of the polymer monomer and the initiator that initiate the polymerization reaction, such as by increasing the temperature or light initiating the polymerization reaction.
[0205] In some embodiments, before the step of forming a base film on at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane in step S21, a step of plasma-treating at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane may be included, and the base film formed is formed on the plasma-treated surface. In this way, by plasma-treating the surfaces such as the surface of the positive electrode, the surface of the negative electrode, and the solid electrolyte membrane where the base film is to be formed, the corresponding surface can be etched to remove the surface impurity layer, defect layer, etc., and the surface energy of the surface can be increased, thereby increasing the bonding strength between the base film and at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane.
[0206] In step S22, the electrolyte can be loaded into the base film by adsorption loading in an infiltration manner, such as dripping the electrolyte onto the base film for adsorption, or immersing the base film in the electrolyte for adsorption. The electrolyte in step S22 is the electrolyte 142 contained in the interface modification layer 14 of the solid-state battery cell assembly 10 of the above-mentioned embodiment of the application.
[0207] In step S23, the positive electrode, solid electrolyte membrane and negative electrode are stacked and arranged. The positive electrode, solid electrolyte membrane and negative electrode can be stacked and arranged according to the structure of the solid-state battery cell assembly, but it should be ensured that the interface modification layer is arranged between the positive electrode and the solid electrolyte membrane or between the negative electrode and the solid electrolyte membrane or between the positive electrode and the solid electrolyte membrane, and between the negative electrode and the solid electrolyte membrane at the same time, so as to play the role of the interface modification layer in improving the wettability of the solid-solid interface between the electrode and the solid electrolyte layer in the solid-state battery cell assembly and reducing the solid-solid interface impedance.
[0208] When the interface modification layer is formed separately, as in the embodiment, the method of providing the interface modification layer between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane comprises the following steps:
[0209] S24: providing a basement membrane;
[0210] S25: loading the electrolyte into the base film to form an interface modification layer;
[0211] S26: stacking the positive electrode, the solid electrolyte membrane and the negative electrode.
[0212] By adopting the method of separately preparing the interface modification layer, the interface modification layer can be prepared simultaneously with the positive electrode, the negative electrode and the solid electrolyte membrane, thereby effectively improving the efficiency and flexibility of preparing solid-state battery cell components, and also improving the quality stability of solid-state battery cell components.
[0213] The method of providing the base film in step S24 can refer to the method of forming the base film in the above step S21, except that the substrate for forming the base film is not the positive electrode, the negative electrode or the solid electrolyte membrane, and other substrates can be selected.
[0214] The method of loading the electrolyte into the base film in step S25 may refer to the method of forming the base film in step S22 above.
[0215] The stacking arrangement in step S26 can refer to the stacking arrangement in step S23 above. After the stacking arrangement, the interface modification layer is arranged between the positive electrode and the solid electrolyte membrane or between the negative electrode and the solid electrolyte membrane or between the positive electrode and the solid electrolyte membrane and the negative electrode and the solid electrolyte membrane at the same time, so as to play the role of the interface modification layer in improving the wettability of the solid-solid interface between the electrode and the solid electrolyte layer in the solid-state battery cell assembly and reducing the solid-solid interface impedance.
[0216] Battery
[0217] In a third aspect, the present application provides a battery comprising a solid-state battery cell assembly formed by assembling a positive electrode, a solid electrolyte layer and a negative electrode, wherein the solid-state battery cell assembly is the solid-state battery cell assembly 10 of the present application embodiment.
[0218] Since the battery of the embodiment of the present application contains the above-mentioned solid-state battery cell assembly 10 of the embodiment of the present application, the cycle performance of the battery of the embodiment of the present application is significantly improved, and the electrochemical performance including the rate and battery safety is also significantly improved.
[0219] In an embodiment, the battery of the embodiment of the present application may include any one of a solid-state battery cell, a battery module, and a battery pack.
[0220] The solid-state battery cell refers to a solid-state battery cell assembly including a battery housing and a battery cell assembly encapsulated in the battery housing. The shape of the solid-state battery cell is not particularly limited, and it can be cylindrical, square, or any other shape. In an exemplary embodiment, the solid-state battery cell can be as follows: Figure 6 The solid-state battery cell 20 is shown in a square structure.
[0221] In some embodiments, Figure 7 As shown, the outer packaging of the solid-state battery cell 20 may include a shell 21 and a cover plate 22. The shell 21 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 21 has an opening connected to the receiving cavity, and the cover plate 22 is used to cover the opening to close the receiving cavity. The solid-state battery cell 20 of the embodiment of the present application contains the solid-state battery cell assembly 10 of the embodiment of the present application. The solid-state battery cell assembly 10 is encapsulated in the receiving cavity. The number of solid-state battery cell assemblies 10 contained in the solid-state battery cell 20 may be one or more, which can be adjusted according to actual needs.
[0222] The preparation method of the solid-state battery cell 20 is well known. The solid-state battery cell assembly 10 is placed in an outer package, and is subjected to vacuum packaging, static placement, formation, shaping and other processes to obtain the solid-state battery cell 20 .
[0223] The battery module is assembled from battery cells, wherein the battery cells include solid-state battery cells 20, that is, it may contain a plurality of solid-state battery cells 20, and the specific number can be adjusted according to the application and capacity of the battery module.
[0224] In some embodiments, Figure 8 FIG. 3 is a schematic diagram of a battery module 30 as an example. Figure 8 As shown, in the battery module 30, a plurality of solid-state battery cells 20 may be arranged in sequence along the length direction of the battery module 30. Of course, they may also be arranged in any other manner. Further, the plurality of solid-state battery cells 20 may be fixed by fasteners.
[0225] Optionally, the battery module 20 may further include a housing having a receiving space, and a plurality of solid-state battery cells 20 are received in the receiving space.
[0226] The battery pack is composed of the above-mentioned solid-state battery cells 20, that is, it can contain multiple solid-state battery cells 20, wherein multiple solid-state battery cells 20 can be assembled into the above-mentioned battery module 30. The specific number of solid-state battery cells 20 or battery modules 30 contained in the battery pack can be adjusted according to the application and capacity of the battery pack.
[0227] As in the embodiment, Fig. 9 and Fig.10 4 is a schematic diagram of an exemplary battery pack 40. The battery pack 40 may include a battery box and a plurality of battery modules 30 disposed in the battery box. The battery box includes an upper box body 41 and a lower box body 42, wherein the upper box body 41 is used to cover the lower box body 42 and form a closed space for accommodating the battery modules 30. The plurality of battery modules 30 may be arranged in the battery box in any manner.
[0228] Electrical devices
[0229] In a fourth aspect, the present application also provides an electric device, which includes the battery of the above-mentioned embodiment of the present application, and further can be a secondary battery. The battery can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. Therefore, the electric device of the present application embodiment has a long standby or battery life.
[0230] The electrical device may be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc. The electrical device may select a secondary battery, a battery module or a battery pack according to its use requirements.
[0231] Fig.11 Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used.
[0232] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a secondary battery may be used as a power source.
[0233] Energy storage device
[0234] In a fifth aspect, the present application also provides an energy storage device, which includes the battery of the above application embodiment, and further can be a secondary battery. The battery can be used as an energy storage unit of the energy storage device to increase the capacity and service life of the energy storage device.
[0235] Example
[0236] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0237] Example 1
[0238] The present embodiment provides a solid-state battery cell assembly, a solid-state battery cell, and a method for preparing the same.
[0239] The solid-state battery cell assembly of this embodiment includes a lithium iron phosphate positive electrode sheet, a graphite negative electrode sheet and a lithium lanthanum zirconium oxide solid electrolyte, and the positive electrode sheet, the lithium lanthanum zirconium oxide solid electrolyte and the graphite negative electrode sheet are stacked in sequence, and a 1 μm PET film layer is stacked between the positive electrode sheet and the oxide solid electrolyte and between the negative electrode sheet and the oxide solid electrolyte, and the PET film layer is adsorbed with an electrolyte, wherein the content of the electrolyte in the PET film layer is 5 μL / cm 2 The electrolyte is 1moL / L LiPF6+EC / EMC (volume ratio 1:1).
[0240] The method for preparing a solid-state battery cell assembly in this embodiment includes the following steps:
[0241] S1: Take a lithium iron phosphate positive electrode sheet and a graphite negative electrode sheet, and etch them with Ar plasma for 30 seconds to obtain a lithium iron phosphate positive electrode sheet and a graphite negative electrode sheet with clean surfaces;
[0242] S2: taking terephthalic acid and ethylene glycol solution, preparing a reaction precursor solution, spraying the precursor solution with a thickness of 1 μm on the surface of the lithium iron phosphate positive electrode sheet and the graphite negative electrode sheet respectively by a spraying method, and performing an esterification reaction to synthesize dihydroxyethyl terephthalate, and then obtaining PET by a condensation reaction;
[0243] S3: Add 5 μL / cm onto the PET film 2 The electrolyte is completely infiltrated and adsorbed inside the PET to form an interface modification layer; that is, a lithium iron phosphate positive electrode sheet and a graphite negative electrode sheet with a high ion conductivity polymer layer on the surface are obtained;
[0244] S4: stacking the positive electrode sheet, oxide solid electrolyte, and negative electrode sheet in sequence to obtain a solid-state battery cell assembly.
[0245] The solid-state battery cell assembly is placed in an outer package, and after the post-cell manufacturing process, a solid-state battery monomer is obtained.
[0246] Example 2
[0247] The present embodiment provides a solid-state battery cell assembly, a solid-state battery cell, and a method for preparing the same.
[0248] The solid-state battery cell assembly of this embodiment includes a ternary positive electrode sheet, a lithium metal negative electrode sheet and a sulfide solid electrolyte, and the positive electrode sheet, the LiP2S7 sulfide solid electrolyte and the negative electrode sheet are stacked in sequence, and a P (VDF-HFP) film layer of 1.5 μm is stacked between the positive electrode sheet and the sulfide solid electrolyte and between the negative electrode sheet and the sulfide solid electrolyte, and the P (VDF-HFP) film layer is adsorbed with an electrolyte, wherein the content of the electrolyte in the P (VDF-HFP) film layer is 3 μL / cm 2 The electrolyte is 1 moL / L LiTFSI+DME / DOL (volume ratio 3:7).
[0249] The method for preparing a solid-state battery cell assembly in this embodiment includes the following steps:
[0250] S1: Take a NCM811 ternary positive electrode sheet and a lithium metal negative electrode sheet, and etch them with Ar plasma for 60s to obtain a ternary positive electrode sheet and a lithium metal negative electrode sheet with clean surfaces;
[0251] S2: Using MLD technology, a layer of P (VDF-HFP) film with a thickness of 1.5 μm is deposited on the surface of the positive electrode sheet and the negative electrode sheet;
[0252] S3: Add 3 μL / cm onto the P(VDF-HFP) membrane. 2 The electrolyte is completely infiltrated and adsorbed inside the P(VDF-HFP) to form an interface modification layer; that is, a ternary positive electrode sheet and a lithium metal negative electrode sheet with a high ion conductivity polymer layer on the surface are obtained;
[0253] S4: Stack the positive electrode sheet, sulfide solid electrolyte, and negative electrode sheet in order to obtain a solid-state battery cell assembly.
[0254] The solid-state battery cell assembly is placed in an outer package, and after the post-cell manufacturing process, a solid-state battery monomer is obtained.
[0255] Example 3
[0256] The present embodiment provides a solid-state battery cell assembly, a solid-state battery cell, and a method for preparing the same.
[0257] The solid-state battery cell assembly of this embodiment is the same as that of Embodiment 2 except that the thickness of the interface modification layer is different.
[0258] The method for preparing a solid-state battery cell assembly in this embodiment includes the following steps:
[0259] The preparation method of the solid-state battery cell assembly is referred to in Example 2, with the only difference being that a layer of P (VDF-HFP) film is first deposited on the surface of the positive electrode sheet, the negative electrode sheet and the solid electrolyte by MLD, and then the electrolyte is adsorbed to form an interface modification layer.
[0260] The solid-state battery cell assembly is placed in an outer package, and after the post-cell manufacturing process, a solid-state battery monomer is obtained.
[0261] Example 4
[0262] The present embodiment provides a solid-state battery cell assembly, a solid-state battery cell, and a method for preparing the same.
[0263] The solid-state battery cell assembly of this embodiment includes a lithium iron phosphate positive electrode sheet, a graphite negative electrode sheet and a LISICON oxide solid electrolyte, and the positive electrode sheet, the oxide solid electrolyte and the graphite negative electrode sheet are stacked in sequence, and a 2μm ZIF series MOF structural membrane layer is stacked between the positive electrode sheet and the oxide solid electrolyte and between the negative electrode sheet and the oxide solid electrolyte, and the MOF structural membrane layer is adsorbed with an electrolyte, wherein the content of the electrolyte in the MOF structural membrane layer is 5μL / cm 2 The electrolyte is 1.2moL / L LiPF6+EC / EMC / DMC (volume ratio 1:1:1).
[0264] The method for preparing a solid-state battery cell assembly in this embodiment includes the following steps:
[0265] S1: Take a lithium iron phosphate positive electrode sheet, a graphite negative electrode sheet, and an oxide solid electrolyte, and etch the oxide solid electrolyte with Ar plasma for 30 seconds to obtain an oxide solid electrolyte with a clean surface;
[0266] S2: MOF monomer is evenly mixed with a binder, a dispersant, and a solvent, and a 2 μm MOF monomer is sprayed on the surface of the oxide solid electrolyte. After drying, a MOF film layer is obtained;
[0267] S3: Add 5 μL / cm onto the MOF membrane layer 2 The electrolyte is completely infiltrated and adsorbed inside the MOF film layer to form an interface modification layer; that is, an oxide solid electrolyte with a MOF film layer on the surface is obtained;
[0268] S4: stacking the positive electrode sheet, oxide solid electrolyte, and negative electrode sheet in sequence to obtain a solid-state battery cell assembly.
[0269] The solid-state battery cell assembly is placed in an outer package, and after the post-cell manufacturing process, a solid-state battery monomer is obtained.
[0270] Example 5
[0271] The present embodiment provides a solid-state battery cell assembly, a solid-state battery cell, and a method for preparing the same.
[0272] The solid-state battery cell assembly of this embodiment includes a LiCoO2 positive electrode sheet, a Si negative electrode sheet and a NASICON oxide solid electrolyte, and the positive electrode sheet, the oxide solid electrolyte and the silicon negative electrode sheet are stacked in sequence, and a 3μm fluorinated polyethylene film layer is stacked between the positive electrode sheet and the oxide solid electrolyte and between the negative electrode sheet and the oxide solid electrolyte, and the fluorinated polyethylene film layer is adsorbed with electrolyte, wherein the content of the electrolyte in the fluorinated polyethylene film layer is 7μL / cm 2 The electrolyte is 2M LiClO4+EC / DEC / PC (volume ratio 5:2:3) and 5% by mass of film-forming additive FEC.
[0273] The method for preparing a solid-state battery cell assembly in this embodiment includes the following steps:
[0274] S1: Take a lithium cobalt oxide positive electrode sheet, a silicon negative electrode sheet, and a NASICON oxide solid electrolyte, and etch the oxide solid electrolyte with Ar plasma for 60 seconds to obtain an oxide solid electrolyte with a clean surface;
[0275] S2: Using MLD technology, a 20μm VYLON polyester resin film layer is grown on both sides of the NASICON solid electrolyte;
[0276] S3: Add 20 μL / cm2 of liquid to the film layer on the surface of NASICON solid electrolyte. 2 The electrolyte is completely infiltrated and adsorbed inside the film layer to form an interface modification layer; that is, a NASICON oxide solid electrolyte with an interface enhancement film layer on the surface is obtained;
[0277] S4: stacking the positive electrode sheet, the oxide solid electrolyte after the composite membrane layer, and the negative electrode sheet in sequence to obtain a solid-state battery cell assembly.
[0278] The solid-state battery cell assembly is placed in an outer package, and after the post-cell manufacturing process, a solid-state battery monomer is obtained.
[0279] Example 6
[0280] The present embodiment provides a solid-state battery cell assembly, a solid-state battery cell, and a method for preparing the same.
[0281] The solid-state battery cell assembly of this embodiment includes an M3P (lithium manganese iron phosphate) positive electrode sheet, a lithium metal negative electrode sheet and a Li2S-GeS2-P2S sulfide solid electrolyte, and the positive electrode sheet, the sulfide solid electrolyte and the lithium metal negative electrode sheet are stacked in sequence, and a 20μm 8-polyethylene oxide (PEO) film layer is stacked between the positive electrode sheet and the sulfide solid electrolyte and between the negative electrode sheet and the sulfide solid electrolyte, and the PEO film layer is adsorbed with an electrolyte, wherein the content of the electrolyte in the PEO film layer is 7μL / cm 2 The electrolyte is 2M LiClO4+EC / MP / DMSO (volume ratio 6:2:2) and 8% by mass of film-forming additive FEC.
[0282] The method for preparing a solid-state battery cell assembly in this embodiment includes the following steps:
[0283] S1: Take an M3P (lithium manganese iron phosphate) positive electrode sheet, a lithium metal negative electrode sheet, and a Li2S-GeS2-P2S sulfide solid electrolyte, and etch the solid electrolyte with Ar plasma for 120s to obtain a sulfide solid electrolyte with a clean surface;
[0284] S2: Using in-situ polymerization technology (reaction of ethylene oxide and Lewis acid), a 50 μm PEO film layer is grown on both sides of the sulfide solid electrolyte;
[0285] S3: Add 50 μL / cm2 of the PEO film layer on the surface of the sulfide solid electrolyte. 2 The electrolyte is completely infiltrated and adsorbed inside the film layer to form an interface modification layer; that is, a solid electrolyte with an interface enhancement film layer on the surface is obtained;
[0286] S4: stacking the positive electrode sheet, the sulfide solid electrolyte after the film layer is composited, and the negative electrode sheet in sequence to obtain a solid-state battery cell assembly.
[0287] The solid-state battery cell assembly is placed in an outer package, and after the post-cell manufacturing process, a solid-state battery monomer is obtained.
[0288] Example 7
[0289] The present embodiment provides a solid-state battery cell assembly, a solid-state battery cell, and a method for preparing the same.
[0290] The solid-state battery cell assembly of this embodiment includes Li 1.2 Mn 0.54 Co 0.13 N i0.13 (Li-rich manganese-based positive electrode) positive electrode sheet, lithium metal negative electrode sheet and Li2SC 2 / 3 Cl4 halide solid electrolyte, and the positive electrode sheet, the halide solid electrolyte and the lithium metal negative electrode sheet are stacked in sequence, and a 50μm polyethylene / polypropylene film layer is stacked between the positive electrode sheet and the halide solid electrolyte and between the negative electrode sheet and the halide solid electrolyte, and the polyethylene / polypropylene film layer is adsorbed with electrolyte, wherein the content of the electrolyte in the polyethylene / polypropylene film layer is 80μL / cm 2 The electrolyte is 3M LiBF4+VC / MA / DMSO (volume ratio 7:2:1) and 10% by mass of film-forming additive FEC.
[0291] The method for preparing a solid-state battery cell assembly in this embodiment includes the following steps:
[0292] S1: Take a Li 1.2 Mn 0.54 Co 0.13 N i0.13 (Li-rich manganese-based positive electrode) positive electrode sheet, lithium metal negative electrode sheet, Li2SC 2 / 3Cl4 halide solid electrolyte, the oxide solid electrolyte is etched by Ar plasma for 120s to obtain a halide solid electrolyte with a clean surface;
[0293] S2: Using MLD, a 80 μm fluorinated polyethylene film layer is grown on both sides of the halide solid electrolyte;
[0294] S3: Add 80 μL / cm2 of the polyethylene / polypropylene film layer on the surface of the halide solid electrolyte. 2 The electrolyte is completely infiltrated and adsorbed inside the film layer to form an interface modification layer; that is, a solid electrolyte with an interface enhancement film layer on the surface is obtained;
[0295] S4: stacking the positive electrode sheet, the halide solid electrolyte after the composite membrane layer, and the negative electrode sheet in sequence to obtain a solid-state battery cell assembly.
[0296] The solid-state battery cell assembly is placed in an outer package, and after the post-cell manufacturing process, a solid-state battery monomer is obtained.
[0297] Comparative Example A1
[0298] This comparative example provides a solid-state battery cell assembly, a solid-state battery cell, and a preparation method thereof.
[0299] Compared with Example 1, the solid-state battery cell assembly in this comparative example does not have an interface modification layer of a PET film containing an electrolyte between the interfaces of the lithium iron phosphate positive electrode sheet and the oxide solid electrolyte, and between the interfaces of the graphite negative electrode sheet and the oxide solid electrolyte. That is, compared with Example 1, the solid-state battery cell assembly does not contain an interface modification layer, and the rest is the same as the solid-state battery cell assembly in Example 1.
[0300] The method for preparing a solid-state battery cell assembly in this comparative example comprises the following steps:
[0301] S1: stacking the positive electrode sheet, oxide solid electrolyte, and negative electrode sheet in sequence to obtain a solid-state battery cell assembly.
[0302] S2: Place the solid-state battery cell assembly in an outer package and undergo post-cell manufacturing processes to obtain a solid-state battery cell.
[0303] Solid-state battery cell related performance test
[0304] The solid-state battery cells in the above-mentioned Examples 1 to 7 and Comparative Example 1 were respectively subjected to the relevant electrochemical performance tests shown in Table 1 below. The test methods and conditions for the relevant performances are as follows:
[0305] Testing method of interface impedance (Ω): After the solid-state battery monomers in Examples 1 to 7 and Comparative Example 1 are formed, they are tested using a Chenhua electrochemical workstation at a frequency range of 100 kHz to 0.01 Hz.
[0306] Polarization overpotential test: Using the Blue Electric Battery Test System, the solid-state battery cell was left to stand for 3 minutes, the voltage value V1 was recorded, and it was discharged at 0.1C, and the instantaneous discharge voltage V2 was recorded. The polarization overpotential was V1-V2.
[0307] Cycle Performance Method:
[0308] The solid-state battery monomer cycle performance test method and conditions in Example 1 to Example 4 and Comparative Example 1 are as follows: the relevant electrochemical performance tests in Table 2 are respectively carried out, and the test conditions are as follows: the test temperature is 45°C, the charge and discharge rate is 1C, and the charge and discharge voltage range is 2.5V~4.2V (vs.Li+ / Li).
[0309] The solid-state battery monomer cycle performance test method and conditions in Example 5 are as follows: the relevant electrochemical performance tests in Table 2 are carried out respectively, and the test conditions are as follows: the test temperature is 25°C, the charge and discharge rate is 0.33C, and the charge and discharge voltage range is 2.5V~4.5V (vs.Li + / Li).
[0310] The solid-state battery monomer cycle performance test method and conditions in Example 6 are as follows: the relevant electrochemical performance tests in Table 2 are carried out respectively, and the test conditions are as follows: the test temperature is 25°C, the charge and discharge rate is 0.33C, and the charge and discharge voltage range is 2.5V~4.2V (vs.Li + / Li).
[0311] The solid-state battery monomer cycle performance test method and conditions in Example 7 are as follows: the relevant electrochemical performance tests in Table 2 are carried out respectively, and the test conditions are as follows: the test temperature is 20°C, the charge and discharge rate is 0.5C, and the charge and discharge voltage range is 2.8V~4.8V (vs.Li + / Li).
[0312] The test results of Examples 1 to 7 and Comparative Example 1 are shown in Table 1.
[0313] Table 1
[0314]
[0315]
[0316] As shown in Table 1, after the modification of the interface modification layer, i.e., the composite film formed by the base film and the electrolyte adsorbed in the base film, the impedance values of the positive electrode-solid electrolyte and the negative electrode-solid electrolyte interface have been significantly reduced, from the original impedance value>100Ω to <100Ω, specifically, the impedance value of the positive electrode and the solid electrolyte interface in Comparative Example 1 is reduced from 873Ω to 75Ω in Example 1, and the impedance value of the negative electrode and the solid electrolyte interface is reduced from 536Ω to 72Ω in Example 1. The reduction of impedance is also conducive to improving the polarization overpotential of the interface. When charging and discharging at a rate of 0.1C, the polarization overpotential of the battery is reduced from the original>100mV to below 100mV, specifically, from 872mV in Comparative Example 1 to 82mV in Example 1, which significantly improves the charge and discharge capacity of the battery. At the same time, the interface modification layer also significantly improves the cycle performance of the battery. This is mainly due to the fact that the introduction of the interface modification layer transforms the original solid-solid interface into a solid-liquid interface with good interface contact and wettability, and no ion bridging. The introduction of the solid-liquid interface also hinders the electron pathway at the solid-solid interface, reduces the leakage current of the battery, and promotes the charge and discharge stability of the battery. Therefore, the cycle performance of the battery has been significantly improved.
[0317] It can be seen from this that the solid-state battery cell assembly provided in this embodiment can have a good and stable wetting effect on the solid-solid interface between the electrode and the solid electrolyte layer, because the interface modification layer is added at the solid-solid interface between the electrode and the solid electrolyte, thereby significantly reducing the impedance between the solid-solid interface, so as to effectively improve the electrochemical performance and electrochemical performance stability of the solid-state battery. At the same time, it also indirectly proves that the interface modification layer can effectively reduce the direct contact between the electrolyte contained therein and the electrode (positive electrode or / and negative electrode) and the solid electrolyte layer, thereby effectively reducing the consumption of the electrolyte during the charge and discharge process, and also reducing the absorption of the electrolyte by the solid electrolyte layer.
[0318] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A solid-state battery cell assembly, comprising a positive electrode and a negative electrode and a solid electrolyte layer arranged between the positive electrode and the negative electrode, characterized in that: A base film is further arranged between the positive electrode and the solid electrolyte layer and / or between the negative electrode and the solid electrolyte layer, and the base film absorbs electrolyte.
2. The solid-state battery cell assembly according to claim 1, characterized in that: The amount of electrolyte adsorbed per unit area of the base film is 1 to 100 μL cm -2 .
3. The solid-state battery cell assembly according to claim 1 or 2, characterized in that: The base film on which the electrolyte is adsorbed has at least any one of the following (1) to (3): (1) The thickness of the single base film is 0.1 to 100 μm, and can be 1 to 3 μm; (2) Ionic conductivity is 10 -2 ~10 -1 S cm -1 ; (3) 0<Electron conductivity≤10 -10 S cm -1 .
4. The solid-state battery cell assembly according to any one of claims 1 to 3, characterized in that: The base film is bonded to the surface of the solid electrolyte layer; and / or The base film is bonded to the surface of the positive electrode facing the solid electrolyte layer; and / or The base film is bonded to a surface of the negative electrode that faces the solid electrolyte layer.
5. The solid-state battery cell assembly according to any one of claims 1 to 4, characterized in that: The electrolyte includes at least any one of the following (1) to (4): (1) The molar concentration of the electrolyte contained in the electrolyte solution is 0.1 to 5 mol / L; (2) The electrolyte contained in the electrolyte solution includes at least one of lithium hexafluoroarsenate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalatoborate), and lithium difluorooxalatoborate; (3) The solvent contained in the electrolyte includes at least one of cyclic carbonate, chain carbonate, cyclic carboxylate, chain carboxylate, cyclic ether, chain ether, dimethyl sulfoxide, and cyclopentane; (4) The electrolyte further contains an additive.
6. The solid-state battery cell assembly according to claim 5, characterized in that: The mass percentage of the additive in the electrolyte is 0.1-10%; and / or The additive includes at least one of fluoroethylene carbonate, vinylene carbonate, vinyl ethylene carbonate, ethyl allyl carbonate, vinyl acetate, catechol cyclic carbonate, and lithium difluorooxalate borate.
7. The solid-state battery cell assembly according to any one of claims 1 to 6, characterized in that: The base film includes at least any one of the following (1) to (6): (1) Porosity is 30-60%; (2) Air permeability is 100-1000s / 100ml; (3) Liquid absorption is 40 to 1000%. (4) Tensile strength: transverse > 8N / 25mm, longitudinal > 15N / 25mm; (5) Elongation: transverse > 300%, longitudinal > 180%; (6) Needle puncture resistance> 20N.
8. The solid-state battery cell assembly according to any one of claims 1 to 7, characterized in that: The base film includes a polymer film.
9. The solid-state battery cell assembly according to claim 8, characterized in that: The polymer of the polymer film includes at least one of crystalline saturated polyester, dimethylsiloxane cross-linked polymer, polyolefin, halogenated polyolefin, and MOF structural material.
10. The solid-state battery cell assembly according to claim 9, characterized in that: The crystalline saturated polyester includes at least one of PET, crystalline dimer acid polyester polyol, crystalline polyester imide, polybutylene terephthalate, polyethylene terephthalate-1,4-cyclohexanedimethanol, and VYLON polyester resin; The dimethylsiloxane cross-linked polymer includes at least one of vinyl dimethylsiloxane cross-linked polymer, amino dimethylsiloxane cross-linked polymer, and aminopropyl dimethylsiloxane; The polyolefin and halogenated polyolefin independently include at least one of polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, polyvinyl chloride, polyvinylidene chloride and polyvinylidene fluoride; The MOF structural material includes at least one structural material of IRMOF series, ZIF series, CPL series, MIL series, PCN series, and UiO series.
11. The solid-state battery cell assembly according to claim 10, characterized in that: The IFMOF series structural materials include at least one of IRMOF-1, IRMOF-3, IRMOF-4, IRMOF-8, IRMOF-9, IRMOF-10, IRMOF-11, IRMOF-12, IRMOF-13, IRMOF-14, IRMOF-16, IRMOF-18, IRMOF-61, IRMOF-62, IRMOF-3-AM1, Fe / IRMOF-3, Mg-IRMOF-74, IRMOF-3-OH, IRMOF-3-SH, Fe / IRMOF-3-900, and IRMOF3-sal; The ZIF series structural materials include IF-1, ZIF-2, ZIF-4, ZIF-5, ZIF-7, ZIF-8, nZIF-8, ZIF-9, ZIF-10, ZIF-11, ZIF-12, ZIF-14, ZIF-20, ZIF-23, ZIF-60, ZIF-61, ZIF-62, ZIF-64, ZIF At least one of -65, ZIF-67, ZIF-68, ZIF-69, ZIF-70, ZIF-71, ZIF-72, ZIF-73, ZIF-74, ZIF-75, ZIF-76, ZIF-77, ZIF-78, ZIF-95, ZIF-100, ZIF-268, ZIF-224, Zn / Co-ZIF; The CPL series structural materials include at least one of CPL-5Cu, CPL-5Cu, CPL-5Cu, CPL-5Cu, and CPL-5Cu; The MIL series structural materials include at least one of MIL-53Cr, MIL-100Cr, MIL-101Cr, MIL-100Fe, MIL-177-LT, MIL-177-HT, MIL-45Co, MIL-45Fe, MIL-53AI, MIL-53Sc, MIL-88Sc, MIL-8, MIL-9, MIL-47, MIL-51, MIL-59, MIL-69, MIL-88, MIL-91, MIL-96, MIL-101, MIL-103, MIL-102, MIL-110, and MIL-125; The PCN structural material includes at least one of PCN-6, PCN-9, PCN-12, PCN-13, PCN-14, PCN-18, PCN-22, PCN-51, PCN-61, PCN-63, PCN-100, PCN-129, PCN-131, PCN-132, PCN-137, PCN-149, PCN-150, PCN-222, PCN-224, PCN-308, and PCN-333; The UiO series structural materials include at least one of UiO-66, UiO-67 and UiO-68.
12. A method for preparing a solid-state battery cell assembly, characterized in that: The steps include: Providing positive electrode, negative electrode and solid electrolyte membrane; The positive electrode, the solid electrolyte membrane and the negative electrode are stacked, and a stacked base membrane is provided between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane; Wherein, the base film absorbs electrolyte.
13. The preparation method according to claim 12, characterized in that: The method of providing a stacked base film between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane comprises the following steps: forming the base film on at least one of a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte film; Loading the electrolyte into the base film; The positive electrode, the solid electrolyte membrane and the negative electrode are stacked, and the base membrane adsorbed with the electrolyte is stacked between the positive electrode and the solid electrolyte layer and / or between the negative electrode and the solid electrolyte layer.
14. The preparation method according to claim 13, characterized in that: The base film includes a polymer film, and a method for forming the base film on at least one of a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte film includes the following steps: Forming a mixed solution including a polymer monomer, a solvent, and an initiator on a surface of the positive electrode, a surface of the negative electrode, and a surface of the solid electrolyte membrane to obtain a polymer precursor film; The polymer precursor film is subjected to a polymer reaction to generate the base film.
15. The preparation method according to claim 14, characterized in that: The film forming treatment method includes at least one of molecular layer deposition, scraping, spraying, spin coating and casting.
16. The preparation method according to any one of claims 13 to 15, characterized in that: Before the step of forming the base film on at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane, the step also includes a step of plasma-treating at least one of the surfaces of the positive electrode, the negative electrode, and the solid electrolyte membrane, and the base film is formed on the surface treated with plasma.
17. The preparation method according to claim 12, characterized in that: The method of providing a stacked base film between the positive electrode and the solid electrolyte membrane and / or between the negative electrode and the solid electrolyte membrane comprises the following steps: providing the base film; Loading the electrolyte into the base film; The positive electrode, the solid electrolyte film, the negative electrode, and the base film on which the electrolyte solution is adsorbed are stacked.
18. A battery, characterized in that: It comprises the solid-state battery cell assembly according to any one of claims 1 to 11 or the solid-state battery cell assembly prepared by the preparation method according to any one of claims 12 to 17.
19. The battery according to claim 18, characterized in that The battery includes any one of a solid-state battery cell, a battery pack, and a battery pack.
20. An electrical device, characterized in that: The electrical device comprises the battery according to claim 18 or 19, and the battery is used to provide electrical energy.
21. An energy storage device, characterized in that: Comprising the battery according to claim 18 or 19.
Citation Information
Cited By
Solid-state battery cell assembly and preparation method therefor, and battery and application thereof
EP4632931A1
Solid-state battery cell assembly and preparation method therefor, and battery and application thereof
WO2024212528A1