White translucent colorable ceramic mixtures based on calcium and sodium frits
Through the combination of calcium and sodium ceramic frit composition and clay kaolin, the realization of high whiteness and high transparency of ceramic materials in large-sized plates and the stress problem during the firing process are solved, and the high color rendering and stability of ceramic materials are achieved. It is suitable for manufacturing ceramic parts of various specifications and thicknesses.
Patent Information
- Application Number
- CN202380024518.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-18
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-18
AI Technical Summary
In the manufacturing of ceramic materials, it is difficult to simultaneously achieve high whiteness and high transparency in large-format sheets, and to avoid stress and deformation problems caused by different thermal expansion coefficients and linear shrinkage rates of white and colored ceramic compositions during the firing process.
Develop a SiO2-Al2O3-CaO-Na2O system based on calcium and sodium ceramic frit composition, devitrified by sodium anorthite, used in ceramic stoneware compositions as the main raw material, combined with clay and kaolin, fogged by a hydraulic press The powder is uniaxially pressed to form the support and fired in a traditional ceramic kiln, using inorganic pigments for coloring.
It achieves high whiteness and high transparency of ceramic materials, and at the same time obtains a wide color range after adding inorganic pigments, and ceramics of different colors can be mixed in the same plate without causing deformation or stress, improving the color rendering of the ceramic composition. effectiveness and stability.
Smart Images

Figure BDA0005018864290000031 
Figure BDA0005018864290000041 
Figure BDA0005018864290000042
Abstract
Description
[0001] Purpose of the Invention
[0002] The present invention relates to the development of a calcium and sodium ceramic frit composition, which makes SiO 2 -Al 2 O 3 -CaO-Na 2 Soda lime feldspar in the O system is devitrified to be used as the main raw material (60%-90%) in a ceramic stoneware composition for the production of large-format plates (up to 2 meters). The frit improves the whiteness of the parts without the addition of opacifiers such as zirconium silicate, although these can also be added together with the alumina to obtain a higher whiteness. On the other hand, it also allows the ceramic composition to have a higher transparency, which will give it a higher color rendering in the case of the addition of inorganic pigments. In this way, a wide range of colors from very intense tones to soft tones can be obtained. In addition, since factors such as viscosity or adhesion to rollers have been taken into account during development, the obtained ceramic composition can be processed in traditional ceramic kilns. The ceramic material can be used to manufacture ceramic pieces of various formats and thicknesses, and can also be used to manufacture large-format plates, where, by mixing its masses, different whites and colors can be produced in the material (even in the form of imitating the texture of natural stone). Until now, white ceramic compositions have been difficult to mix with colored ceramic compositions when trying to mimic natural textures in large format boards because of the stresses that occur during firing due to the differences in coefficient of thermal expansion (CTE) and linear shrinkage between them. White and colored ceramic compositions come from different recipes with different properties, which in the case of low CTE targets are mainly due to the use of opacifiers such as zirconium silicate. The biggest advantage of using the same material to achieve different whites and colors is that they can be mixed in the same board without causing deformation and stress in the final fired board. Technical Field
[0003] The invention is applicable to the ceramic material manufacturing industry. Background Art
[0004] In the field of ceramic material processing, there are already some ceramic material compositions that can achieve a certain degree of whiteness, a certain degree of transparency or a certain degree of coloration.
[0005] However, these treatments are all achieved independently, while the present invention is based on a specific composition of calcium and sodium frits that can achieve high whiteness and high transparency at the same time, and can be colored. The composition of calcium and sodium frits enables different white and color mixtures to be achieved in the same board using the same material without causing deformation or stress in the final fired board.
[0006] We can cite European Patent No. 19382876.1, which relates to an artificial block stone comprising an inorganic filler and a hardened binder, wherein the binder is an organic resin and the inorganic filler includes feldspar. However, the present invention relates to a material different from that used in this patent application, namely "quartz", which consists of a plate made of quartz / feldspar powder / sand and resin. Basically, the powder is mixed with the resin, the mixture is compacted in a vibrating compactor, and the resin is cured; once cured, the surface is polished.
[0007] However, in the patent applied for, the final product consists of an atomized pressed ceramic composition, coated with a thin layer of vitreous enamel, which is heat treated at 1100° C. in a given cycle, depending on the thickness (3-30 mm). Summary of the invention
[0008] The present invention relates to a high whiteness, translucent and colorable ceramic material based on a lime-soda frit which can devitrify soda-lime feldspar, comprising a support fired in a conventional ceramic kiln, the support being formed by uniaxial pressing of atomized powders by a hydraulic press, and the exposed surface of the support being coated with a glaze.
[0009] The atomized powder is produced by drying the wet-ground ceramic slurry in the ball mill in an atomizer. The slurry consists of frit, clay, kaolin, water, deflocculant and plasticizer additives. Inorganic pigments can also be added depending on the desired color of the sintered support. In a preferred embodiment of the present invention, the frit has the function of increasing the translucency of the ceramic material without affecting the whiteness of the material. Clay and kaolin have different roles in various stages of the process:
[0010] On the one hand, it promotes the suspension of the slurry to ensure the grinding and atomization process; and
[0011] On the other hand, it provides the atomized product with appropriate plasticity so that it can be easily pressed in a hydraulic press. In addition, clay and kaolin also enable the support to absorb part of the moisture of the glaze, thereby maintaining the consistency of the workpiece during the glazing and decoration process.
[0012] Process of obtaining ceramic materials:
[0013] 1. Characteristics of frit
[0014] 2. Characteristics of the support
[0015] 2.1 Original support
[0016] 2.2 Firing support parts
[0017] 2.2.1 Color coordinates of the firing support
[0018] 2.2.2 Characteristics of the support
[0019] 3. Conclusion
[0020] 1. Characteristics of frit
[0021] Frit is a mixture of inorganic chemicals obtained by rapidly cooling a melt, converting the resulting chemicals into insoluble glassy compounds in the form of particles.
[0022] To obtain the frit, the different raw materials were dry mixed. The resulting mixture was then placed in an alumina crucible and subjected to a thermal cycle in a laboratory electric furnace, including heating from 500°C to a maximum temperature (1500-1550°C) at a rate of 10°C / min. Depending on the characteristics of the frit, the crucible containing the mixture was kept at the maximum temperature for as short a time as possible (30-45 minutes), and then the melt was poured into water to cool, thereby obtaining the frit.
[0023] To obtain the frit, a formulation of the pure mineral anorthite (calcium aluminosilicate) is started.
[0024] Since the latter formula cannot be fired, K is added 2 O to melt it. Then, Na 2 O instead of K 2 O. Finally, for Na 2 O frit SiO 2 / Al 2 O 3 Ratio and Na 2 The O / CaO ratio was optimized.
[0025] The main components expressed as oxides in the final frit tested are shown below. The percentage of each oxide depends on the desired flux value, whiteness, translucency and color development.
[0026] Table 1. Oxide composition of the frit
[0027]
[0028]
[0029] Sodium feldspar, quartz, alumina, calcium carbonate and sodium nitrate are used in the frit recipe.
[0030] The feed formula used is as follows:
[0031] Table 2. Feed formula of the tested frits
[0032] raw material % Sodium feldspar 40.1-63.2 quartz 0.0-24.7 Alumina 5.4-18.4 Calcium carbonate 13.4-30.3 Sodium nitrate 0.0-16.3
[0033] Of the ceramic compositions tested (frit + clay and kaolin), the frit formulated for the preferred embodiment resulted in a ceramic composition that best balanced the desired properties (whiteness, translucency, and optimal color development).
[0034] The shrinkage-temperature curve and characteristic temperature ( Figure 1 Shrinkage rate-temperature curve).
[0035] The frit starts to shrink at a temperature of 865°C. In the temperature range of 950-1150°C, the frit crystallizes. Then, the frit continues to shrink until the temperature reaches 1335°C. It starts to soften at 1370°C and melts at 1380°C. Due to the nature of the material, its ball temperature (ST) cannot be measured.
[0036] Table 3 Characteristic temperature of frit
[0037]
[0038]
[0039] 2. Characteristics of the support
[0040] 2.1 Original support
[0041] The raw support is formed by uniaxially pressing atomized powder obtained by drying in an atomizer a ceramic slurry wet-milled in a ball mill.
[0042] A deflocculant (0.7% of dry solids) is used during the grinding process, which allows the density and viscosity of the slurry to be adjusted, thus obtaining a particle size profile of the atomized material suitable for the subsequent pressing stage. Before spraying, the decorative slurry (barbotine) is mixed with a plasticizing additive (1% of dry solids), which will give the pressed support the appropriate mechanical resistance to withstand the conveying process of the glazing and decoration line before firing.
[0043] Table 4 Feeding formula of ceramic composition
[0044] raw material % clay 10-20 Kaolin 10-30 Frit 60-90
[0045] 2.2 Fired support
[0046] The bulk density and water absorption of the support were measured to determine the temperature suitable for firing the support ( Figure 3 , the bulk density and water absorption of the support parts change with the firing temperature)
[0047] 2.2.1 Color coordinates of fired support
[0048] Besides the high whiteness of the support, it is also interesting that the ceramic composition obtained therefrom can be colored very well. For this purpose, white (calcined alumina), black and blue inorganic pigments were selected.
[0049] Table 5 Color coordinates of colored ceramic compositions
[0050] nature +2% Black +2% Blue +4% Alumina +6% Alumina Temperature(℃) 1150 1170 1170 1190 1210 L* 89.3 29.4 45.6 93.2 94.0 a* -1.6 0.7 0.5 -1.1 -0.8 b* 6.5 0.1 -29.0 4.3 4.2
[0051] It can be seen that the black color rendering is good, but the blue color rendering is poor, with a less negative value of the b* coordinate. The addition of aluminum oxide to the latter composition can increase the whiteness value at appropriate temperatures, which was one of the original proposed goals.
[0052] 2.2.2 Characterization of Support Parts
[0053] The coefficient of thermal expansion (CTE) of the ceramic compositions was determined using a dilatometer. CTE measures the relative change in length or volume of a solid body when its temperature changes.
[0054] Table 6 Expansion coefficient of the ceramic composition
[0055] nature Preferred ceramic compositions <![CDATA[α25-300(oC-1)x 10 -7 ]]> 54.2 <![CDATA[α25-500(oC-1)x 10 -7 ]]> 59.1 <![CDATA[α25-650(oC-1)x 10 -7 ]]> 64.0 <![CDATA[α500-650(oC-1)x 10 -7 ]]> 79.4
[0056] To characterize the support, the crystalline phase was determined by X-ray diffraction (XRD).
[0057] Figure 2 (The crystalline phase was determined by XRD of the ceramic composition) shows the diffraction pattern obtained from a support sample, with the maximum intensity peak of the determined phase marked, as well as other characteristic reflections of lower intensity. Please note the following:
[0058] Sodium calcium feldspar (Ca 2 Na)Al 2 Si 2 O 8) As the majority phase, calcium aluminate (hexagonal structure) (Ca 2 Na 6 AI 8 Si 8 O 32 ) is a minority phase.
[0059] 3. Conclusion
[0060] It has been noted that it is very complex to obtain a single frit that meets all requirements: sufficient firing temperature, good colour development and high whiteness, with or without the addition of calcined alumina.
[0061] During testing of compositions, the compositions obtained using the preferred embodiment frits were the compositions that best balanced the following properties:
[0062] The proposed ceramic composition has good dry bulk density, has high bulk density when fired, but is temperature stable at operating temperatures (1100-1200°C) and does not undergo thermoplastic deformation below the glass transition temperature.
[0063] Black color rendering is good, but blue color rendering is not good, with the b* coordinate being slightly less negative. Adding alumina to this ceramic composition provides higher whiteness values at appropriate temperatures.
[0064] Figure 4 The appearance of the ceramic specimen without added pigment is shown;
[0065] Figure 5 The appearance of the ceramic sample with 2% black pigment added is shown;
[0066] Figure 6 The appearance of the ceramic sample with 2% blue pigment added is shown. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] The accompanying drawings show exemplary schematic diagrams and diffraction patterns of high whiteness, translucent and colorable ceramic materials based on calcium frit.
[0068] Figure 1 shows the shrinkage-temperature curve of the frit;
[0069] Figure 2 shows a diffraction pattern for determining the crystalline phase of the ceramic composition by X-ray diffraction (XRD);
[0070] Figure 3 Schematic diagram showing pottery vitrification of a ceramic composition; changes in bulk density and water absorption of a support as a function of firing temperature;
[0071] Figure 4 The appearance of a ceramic sample without added pigment is shown;
[0072] Figure 5 The appearance of a ceramic sample containing 2% black pigment is shown;
[0073] Figure 6 Shown is the appearance of a ceramic sample containing 2% blue pigment. DETAILED DESCRIPTION
[0074] The preferred ceramic composition is prepared by wet grinding (with water and deflocculants) a mixture of atomized raw materials (frit, clay and kaolin). It is then pressed, glazed and fired. The atomization process gives it only the necessary fluidity to allow it to be evenly distributed in the mold and pressed. The pressed slab is fired, and it is this fired ceramic material that has the above-mentioned whiteness, translucency and the characteristics of optimal color development achieved by the addition of inorganic pigments.
[0075] As shown in Table 4, the ceramic composition is a composition based on a frit (60-90%) and a mixture of clay and kaolin (10-40%). The use of such a frit can make the device have a high whiteness without adding a light-shielding agent, and can improve its translucency without affecting the whiteness, and can also obtain a high color rendering after adding an inorganic pigment.
[0076] Shrinkage rate-temperature curve measured by high temperature microscope ( Figure 1 ) reflects the characteristic temperature of the obtained melt, which shows that the melt starts to shrink at 865°C, then crystallizes in the temperature range of 950-1150°C, and then continues to shrink until the temperature reaches 1335°C. Finally, it starts to soften at 1370°C and melts at 1380°C. Due to the nature of the material, its spherical temperature cannot be detected.
[0077] As for the support member of the ceramic composition, the ceramic composition diagram ( Figure 3 ) detected the changes in bulk density and water absorption of the support with firing temperature. From the figure, it can be concluded that its maximum densification temperature is about 1100-1200°C, and it remains at a higher value at subsequent temperatures. In addition, it was observed that no water absorption was detected in the fired object during the entire firing process.
[0078] To complete the characterization of the fired support, the X-ray diffraction pattern (XRD) ( Figure 2 ) identified the presence of a crystalline phase.
[0079] Finally, the suitability of the ceramic composition for color development was tested, verifying that the addition of inorganic pigments resulted in higher color values, and that the addition of aluminum oxide resulted in an improved whiteness. The ceramic material obtained can therefore be used to manufacture large-format panels in which different white and colored colors can be fully mixed without causing deformation or inducing stress in the final fired panel.
Claims
1. A white translucent colorable ceramic mixture based on calcium sodium frit, Features: It includes: 60%-90% SiO 2 -Al 2 O 3 -CaO-Na 2 O-series frits to be used as the main raw material for ceramic stone compositions, which will provide devices with high whiteness without the need for the addition of opacifiers such as zirconium silicate; The composition of the frit expressed as the percentage of the main oxides is: The feeding formula of the frit is: The ceramic mixture further comprises 10%-40% of inorganic raw materials, wherein the inorganic raw materials are a mixture of 10%-30% of kaolin and 10%-20% of clay; The formula of the ceramic mixture is: 。 2. A method for producing a white translucent colorable ceramic mixture based on calcium-sodium frit according to claim 1, Features: The product consists of a pressed and / or extruded atomized ceramic composition covered with a thin layer of vitreous enamel, heat treated at 1100°C in a cycle lasting a certain time, depending on the thickness (3-30 mm).
3. The white translucent colorable ceramic mixture based on lime-sodium frit according to claim 1, Features: In order to make the composition white, during the firing process, the sodium calcium feldspar (Ca 2 Na)Al 2 Si 2 O 8 ) and the hexagonal structure of calcium aluminate (Ca 2 Na 6 Al 8 Si 8 O 32 ) Devitrification.
4. The white translucent colorable ceramic mixture based on lime-sodium frit according to claim 1, Features: Inorganic pigments are added, such as black based on Fe-Cr with a hematite crystal structure, brown based on Ti-W-Cr with a rutile crystal structure, brown based on Fe-Cr-Al with a hematite crystal structure, pink based on Al-Mn with a corundum crystal structure, orange based on Ti-Sb-Cr with a rutile crystal structure, or blue based on Zr-Si-V with a zircon crystal structure.
5. The white translucent colorable ceramic mixture based on lime-soda frit according to claim 1, Features: Its whiteness is improved by adding alumina and opacifiers such as zirconium silicate.
6. Use of the white translucent colorable ceramic mixture based on lime-soda frit as claimed in claim 1, Features: It can be used to make pressed and / or extruded ceramic parts of any thickness and shape.
7. Use of the white translucent colorable ceramic mixture based on lime-soda frit as claimed in claim 1, Features: It is used to manufacture large format slabs and by mixing the qualities of said mixture it is possible to develop different whites and materials on said slabs and even to imitate the grain forms of natural stone without causing deformations and inducing stresses in the final fired slab.
Citation Information
Patent Citations
Glass-ceramic tiles and preparation method thereof
CN109095778A
Wear-resistant transparent glaze, wear-resistant glazed brick and preparation method thereof
CN111423124A
Microcrystal wear-resistant transparent glaze as well as preparation method and application of glaze slip of microcrystal wear-resistant transparent glaze
CN112851120A
Super white ceramic tile
CN1962535A
Feldspar-rich dental porcelain composition
DE19850266A1