Preparation method of 3D printing degradable intravascular stent
By adopting the design of second radiating fibers and immunosuppressive drugs arranged in a concentric ring in the 3D printed vascular stent, the problem of slow degradation speed in the existing technology is solved, and the gradual degradation of the stent and the sustained release of the drug are achieved, improving the treatment effectiveness and personalization of treatment.
Patent Information
- Application Number
- CN202410818953.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-22
AI Technical Summary
The degradation rate of existing 3D printed vascular stents is relatively slow, resulting in a corresponding slowdown in the sustained release rate of drugs, affecting the therapeutic effect.
The second radiating fiber arranged in a concentric ring is used to surround the first radiating fiber, and the immunosuppressive drug is evenly dispersed in the second radiating fiber. Hydrogel is used as the connection medium, and the mass ratio of the polylactic acid-glycolic acid copolymer is adjusted. And the design of the spinning nozzle achieves the gradual degradation of the stent and the sustained release of the drug.
It achieves the mechanical stability and gradual degradation of vascular stents in the early stages of implantation, reduces long-term implantation complications, ensures the sustained release and therapeutic effect of drugs, provides personalized treatment strategies, and improves the accuracy and effectiveness of treatment. sex.
Smart Images

Figure CN118806985A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a 3D printed degradable vascular stent, and in particular to a preparation method of the 3D printed degradable vascular stent. Background Art
[0002] Degradable vascular stents are medical devices made of biodegradable polymer materials, mainly used to treat cardiovascular diseases, such as coronary artery stenosis. Degradable vascular stents are mainly made of biodegradable polymer materials, such as poly-L-lactic acid (PLA). This material can gradually degrade in the human body over time, thus avoiding the complications that may be caused by long-term indwelling metal stents.
[0003] With the rapid development of science and technology, 3D printing technology is increasingly used in the field of tissue engineering, among which 3D printed scaffold technology is particularly eye-catching. 3D printed scaffold technology uses three-dimensional rapid prototyping technology to precisely control the layer-by-layer stacking of materials to print out scaffolds with specific shapes and structures. These scaffolds not only have good biocompatibility and can coexist harmoniously with human tissues, but also have excellent mechanical properties and can withstand various stresses under physiological conditions. Through 3D printing technology, the three-dimensional microstructure of the scaffold, such as pore size, distribution and connectivity, can be precisely controlled to simulate the microenvironment of natural tissues and promote cell growth and differentiation.
[0004] However, in the prior art, the vascular stents prepared by 3D printing technology have a slow degradation rate. If drugs are mixed in the vascular stents, the sustained release rate of the drugs will slow down with the degradation rate of the vascular stents, resulting in a prolonged effective action time of the drugs in the body. In certain cases, the drug concentration will be maintained at a low level for a long time, thus affecting the treatment effect.
[0005] Therefore, there is an urgent need for a method for preparing a 3D printed degradable vascular stent to prepare a degradable vascular stent that can solve the above technical problems. Summary of the invention
[0006] The present invention overcomes the deficiencies of the prior art and provides a method for preparing a 3D printed degradable vascular stent.
[0007] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a 3D printed degradable vascular stent, comprising: a first radiating fiber, a second radiating fiber and an immunosuppressive drug;
[0008] The second radial fibers are evenly arranged in a concentric ring manner on the outer wall around the first radial fibers, and both the first radial fibers and the second radial fibers are biocompatible and biodegradable; in the same biological environment, the second radial fibers will be degraded preferentially compared to the first radial fibers, and the immunosuppressive drug is evenly dispersed and mixed in the internal structure of the second radial fibers.
[0009] In a preferred embodiment of the present invention, hydrogel is used as a connecting medium at the connection between the first radiating fiber and the second radiating fiber.
[0010] In a preferred embodiment of the present invention, the first radiating fiber is made of polylactic acid or polycaprolactone.
[0011] In a preferred embodiment of the present invention, the second radiating fiber is made of a mixed solution of polylactic acid-glycolic acid copolymer and immunosuppressive drugs in a mass ratio of 7-8:2-3 by a bracket 3D printing device.
[0012] In a preferred embodiment of the present invention, the polylactic acid-glycolic acid copolymer is prepared by uniformly mixing lactic acid and glycolic acid in a mass ratio of 4-8:2-6.
[0013] A method for preparing a 3D printed degradable vascular stent comprises the following steps:
[0014] S1, preparing electrospinning solutions for preparing the first radiating fiber and the second radiating fiber respectively, and adding immunosuppressive drugs to the electrospinning solution prepared for preparing the second radiating fiber;
[0015] S2, building a 3D printing device for a bracket, and preparing two groups of spinning nozzles, one group of spinning nozzles is located at a central position, and is used to prepare a first radial fiber; the other group of spinning nozzles has multiple spinning nozzles, and are radially arranged around the spinning nozzle at the central position, and is used to prepare a second radial fiber;
[0016] S3, the electrospinning solutions were loaded into the syringe pumps respectively and connected to the corresponding spinnerets, the spacing between the spinning nozzles was adjusted, and the 3D printing of the bracket was started.
[0017] In a preferred embodiment of the present invention, the two groups of spinning nozzles include a first nozzle, a second nozzle and a dispensing nozzle arranged between the first nozzle and the second nozzle; the first nozzle is connected to an electrospinning solution for preparing a first radiating fiber, the second nozzle is connected to an electrospinning solution for preparing a second radiating fiber, and the dispensing nozzle is connected to a hydrogel solution.
[0018] In a preferred embodiment of the present invention, the inner wall of the first nozzle has a plurality of grooves corresponding to the second nozzle, and the grooves are used to accommodate the prepared second radiating fibers.
[0019] In a preferred embodiment of the present invention, the immunosuppressive drug is at least one of rapamycin, paclitaxel, everolimus, atorvastatin, aspirin, clopidogrel, ticagrelor, metoprolol, and Diovan.
[0020] In a preferred embodiment of the present invention, when the second radiating fibers are prepared by the plurality of second nozzles, the immunosuppressive drug components injected by them can be uniform, that is, all the second nozzles use the same drug; or they can be diversified, that is, each second nozzle injects different immunosuppressive drugs according to demand.
[0021] In a preferred embodiment of the present invention, the inner diameter of the first radiating fiber is 2-4 mm, and the thickness is 200-300 μm; the inner diameter of the second radiating fiber is 1-3 mm, and the thickness is 100-150 μm; the thickness of the hydrogel coating is 30-60 μm.
[0022] The present invention solves the defects existing in the background technology and has the following beneficial effects:
[0023] (1) The present invention uses concentric annularly arranged second radiating fibers to surround the first radiating fibers. This structure not only ensures the mechanical stability of the vascular stent, but also achieves the gradual degradation of the stent in the blood vessel through the difference in degradation rates of the inner and outer layers of fibers. This gradual degradation feature helps the vascular stent to provide sufficient support in the early stage of implantation. At the same time, as the vascular tissue recovers, the stent gradually degrades, reducing the complications that may be caused by long-term implantation. In addition, the uniform dispersion and mixing of immunosuppressive drugs inside the second radiating fibers ensure the continuous release of the drugs during the degradation process of the stent. This effectively inhibits inflammatory reactions and bacterial growth in the blood vessels, reduces the risk of postoperative infection, and accelerates the repair and healing of the vascular lining.
[0024] (2) When preparing the second radiation fiber, the multiple second nozzles can inject different immunosuppressive drugs according to needs. This personalized treatment strategy can more accurately meet the treatment needs of patients and improve the treatment effect.
[0025] (3) By changing the mixing mass ratio of lactic acid and glycolic acid in the polylactic acid-glycolic acid copolymer, different degradation rates can be achieved. The polylactic acid-glycolic acid copolymers with different degradation rates are mixed with different immunosuppressive drugs. The drugs can be selected according to the specific stage or pathological characteristics of the disease. The spinning solution containing different drugs and polylactic acid-glycolic acid copolymers is sprayed out using a multi-nozzle to form a second radial fiber arranged in a concentric ring. Since the degradation rate and drug type of the polylactic acid-glycolic acid copolymer in the second radial fibers in different directions are different, the treatment strategy can be further personalized, the accuracy and effectiveness of the treatment can be improved, and it can also be flexibly adjusted according to the specific situation of the patient to ensure the maximization of the treatment effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 It is a schematic diagram of the connection structure between the first nozzle and the second nozzle of the present invention;
[0028] Figure 2 It is a schematic diagram of the exploded structure of the overall structure of the present invention;
[0029] Figure 3 is a schematic diagram of the groove structure of the present invention;
[0030] Figure 4 It is a flow chart of the preparation method of the 3D printed degradable vascular stent of the present invention.
[0031] In the figure: 1. first nozzle; 2. second nozzle; 3. dispensing nozzle; 4. groove. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0034] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the scope of protection of the present application. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the invention, unless otherwise specified, "multiple" means two or more.
[0035] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium, and it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood by specific circumstances.
[0036] like Figure 1 As shown, a method for preparing a 3D printed degradable vascular stent includes: a first radiating fiber, a second radiating fiber and an immunosuppressive drug.
[0037] The second radial fibers are evenly arranged in a concentric ring manner on the outer wall of the first radial fibers. Both the first radial fibers and the second radial fibers are biocompatible and biodegradable. In the same biological environment, the second radial fibers will be degraded preferentially compared to the first radial fibers, and the immunosuppressive drugs are evenly dispersed and mixed in the internal structure of the second radial fibers.
[0038] This design allows the vascular stent to provide sufficient support in the early stage of implantation to maintain the morphology and function of the blood vessel. As the vascular tissue recovers and regenerates, the second radial fibers gradually degrade, reducing long-term interference with the blood vessels and contributing to the natural repair of the blood vessels. As the second radial fibers degrade, the drug is gradually released into the vascular environment, inhibiting inflammatory responses, preventing infections, and promoting repair of the vascular lining. This sustained release of drugs improves the therapeutic effect and reduces complications caused by insufficient or excessive drug dosage.
[0039] The connection between the first radiating fiber and the second radiating fiber uses hydrogel as a connecting medium. The hydrogel has good biocompatibility and absorbability and can be gradually degraded in the body. At the same time, the hydrogel can also provide good adhesion and flexibility to ensure that the connection between the first radiating fiber and the second radiating fiber is stable and reliable, and prevent the stent from shifting or falling off in the blood vessel.
[0040] The first radiating fiber is made of one of polylactic acid or polycaprolactone. The second radiating fiber is made of a mixed solution of polylactic acid-glycolic acid copolymer and immunosuppressive drugs at a mass ratio of 7-8:2-3, through a bracket 3D printing device. Polylactic acid-glycolic acid copolymer is made by uniformly mixing lactic acid and glycolic acid at a mass ratio of 4-8:2-6.
[0041] By changing the mixing mass ratio of lactic acid and glycolic acid in polylactic acid-glycolic acid copolymer, different degradation rates can be achieved. Polylactic acid-glycolic acid copolymers with different degradation rates are mixed with different immunosuppressive drugs. The drugs can be selected according to the specific stage or pathological characteristics of the disease. The spinning solution containing different drugs and polylactic acid-glycolic acid copolymers is sprayed out using multiple nozzles to form concentric ring-arranged second radial fibers. Since the degradation rates and drug types of polylactic acid-glycolic acid copolymers in the second radial fibers in different directions are different, the treatment strategy can be further personalized, the accuracy and effectiveness of the treatment can be improved, and it can also be flexibly adjusted according to the specific conditions of the patients to ensure the maximum treatment effect.
[0042] like Figure 4 As shown, a method for preparing a 3D printed degradable vascular stent comprises the following steps:
[0043] S1, preparing electrospinning solutions for preparing the first radiating fiber and the second radiating fiber respectively, and adding immunosuppressive drugs to the electrospinning solution prepared for preparing the second radiating fiber;
[0044] S2, building a 3D printing device for a bracket, and preparing two groups of spinning nozzles, one group of spinning nozzles is located at a central position, and is used to prepare a first radial fiber; the other group of spinning nozzles has multiple spinning nozzles, and are radially arranged around the spinning nozzle at the central position, and is used to prepare a second radial fiber;
[0045] like Figure 1 , 2 As shown in Figures 1 and 3, the two groups of spinning nozzles include a first nozzle 1, a second nozzle 2, and a dispensing nozzle 3 disposed between the first nozzle 1 and the second nozzle 2; the first nozzle 1 is connected to an electrospinning solution for preparing a first radiating fiber, the second nozzle 2 is connected to an electrospinning solution for preparing a second radiating fiber, and the dispensing nozzle 3 is connected to a hydrogel solution. The inner wall of the first nozzle 1 has a plurality of grooves 4 corresponding to the second nozzle 2, and the grooves 4 are used to accommodate the second radiating fibers prepared by the second nozzle 2.
[0046] The immunosuppressive drug is at least one of rapamycin, paclitaxel, everolimus, atorvastatin, aspirin, clopidogrel, ticagrelor, betaloc, and diovan. When the second radiation fibers are prepared by the multiple second nozzles 2, the immunosuppressive drug components injected by them can be unified, that is, all the second nozzles 2 use the same drug; or they can be diversified, that is, each second nozzle 2 injects different immunosuppressive drugs according to needs.
[0047] S3, the electrospinning solutions were loaded into the syringe pumps respectively and connected to the corresponding spinnerets, the spacing between the spinning nozzles was adjusted, and the 3D printing of the bracket was started.
[0048] The inner diameter of the first radiating fiber is 2-4 mm, and the thickness is 200-300 μm; the inner diameter of the second radiating fiber is 1-3 mm, and the thickness is 100-150 μm; and the thickness of the hydrogel coating is 30-60 μm.
[0049] It should be noted that: rapamycin is used to treat coronary artery atherosclerosis and stenosis; paclitaxel is used to treat vascular obstruction caused by malignant tumors; everolimus is used to reduce the restenosis rate after coronary revascularization; sirolimus is used to treat coronary heart disease; atorvastatin is used to improve cardiovascular lesions caused by dyslipidemia; aspirin is used to prevent thrombosis in stents or other coronary arteries; clopidogrel is used in combination with aspirin to prevent stent thrombosis; ticagrelor is used in combination with aspirin to prevent stent thrombosis; metoprolol is used to lower heart rate and blood pressure and reduce cardiac load; Diovan, as an angiotensin II receptor blocker, is used to treat hypertension and heart failure.
[0050] Embodiment 1
[0051] The electrospinning solution of the first radiating fiber was prepared using polylactic acid, and the electrospinning solution of the second radiating fiber was prepared by mixing polylactic acid-glycolic acid copolymer (lactic acid to glycolic acid mass ratio of 6:4) with immunosuppressive drug (rapamycin) at a mass ratio of 7:3. PEG / α-CD polyrotaxane hydrogel was used for bonding the first radiating fiber to the second radiating fiber.
[0052] Build a 3D printing device for the bracket and prepare two groups of spinning nozzles. One group is the first nozzle at the center. The inner diameter of the nozzle of the first nozzle is 3mm, which is used to prepare the first radial fiber. The thickness of the first radial fiber is 250μm. The other group is a plurality of second nozzles, which are radially arranged around the first nozzle. The inner diameter of the nozzle of the second nozzle is 2mm, which is used to prepare the second radial fiber. The thickness of the second radial fiber is 120μm. The spinning speed of the first nozzle and the second nozzle is 12mm / s.
[0053] A dispensing nozzle is arranged between the first nozzle and the second nozzle to apply hydrogel at the connection between the first radiating fiber and the second radiating fiber. The thickness of the hydrogel coating is 40 μm.
[0054] The electrospinning solution and the hydrogel solution were loaded into the syringe pumps respectively and connected to the corresponding spinnerets. The spacing between the spinning nozzles was adjusted and the stent 3D printing was started. By controlling the movement of the syringe pump and the spinning nozzle, a vascular stent with a diameter of 5 mm and a length of 20 mm was prepared.
[0055] The total mass of the vascular stent prepared in Example 1 was measured by an electronic balance to be 0.3 g, of which the mass of the first radiating fiber was 0.08 g, and the mass of the second radiating fiber was 0.22 g.
[0056] Degradation experiment
[0057] The vascular stent prepared in Example 1 was placed in a PBS buffer. It should be noted that the pH value of the PBS buffer was 7.4, thereby more realistically simulating the physiological environment of the human body. The temperature of the PBS buffer was set to 37° C., thereby realistically simulating the normal temperature of the human body.
[0058] The vascular stent was taken out every other day and its morphological changes were observed under a microscope. The observation and recording were continued for 5 days. The mass of the stent was measured using an electronic balance and the mass loss was recorded. The degradation rates of the first radiating fiber and the second radiating fiber were evaluated by measuring the diameter change, breakage or mass loss of the fiber. The mass loss of the first radiating fiber and the second radiating fiber are shown in Table 1.
[0059] Table 1
[0060]
[0061] As shown in Table 1, the degradation rate of the first radial fiber within five days is 0.0002g / day, which proves that the degradation rate of the first radial fiber is very low; the degradation rate of the second radial fiber within five days is 0.0096g / day, which is faster than the first radial fiber. Therefore, the gradual degradation of the stent in the blood vessel is achieved through the difference in degradation rates of the inner and outer layers of fibers.
[0062] During the degradation experiment, when using an electronic balance to measure the mass of the bracket, since the bracket will continue to degrade over time and the mass will decrease accordingly, a transparent cover is needed to place the electronic balance in a fully sealed environment to prevent the surrounding air flow from causing inaccurate measurement results.
[0063] Drug release experiments
[0064] The vascular stent prepared in Example 1 was placed in the same test environment as the degradation experiment. The total mass of rapamycin in the vascular stent is
[0065] Samples were taken from the PBS buffer every 12 hours, and the drug concentration was determined using high performance liquid chromatography (HPLC). The observations were continued for 5 days. The drug release rate and cumulative release amount were evaluated by the measured drug concentration data. The drug release rate and cumulative release amount are shown in Table 2.
[0066] Table 2
[0067]
[0068] The drug release rate was fast when the first few time points were tested. The drug release rate gradually slowed down and the concentration gradually decreased when the next few time points were tested. In the end, it showed that the drug release was nearing the end.
[0069] When the present invention is used, polylactic acid is used to prepare the electrospinning solution of the first radiating fiber, and polylactic acid-glycolic acid copolymer is mixed with immunosuppressive drugs to prepare the electrospinning solution of the second radiating fiber. The hydrogel is used to bond the first radiating fiber to the second radiating fiber.
[0070] A bracket 3D printing device is built, and two groups of spinning nozzles are prepared. One group is a first nozzle 1 at the center, which is used to prepare the first radial fiber; the other group is a plurality of second nozzles 2, which are radially arranged around the first nozzle 1, and are used to prepare the second radial fiber.
[0071] A glue dispensing nozzle 3 is arranged between the first nozzle 1 and the second nozzle 2 for applying hydrogel at the connection between the first radiating fiber and the second radiating fiber.
[0072] The electrospinning solution and the hydrogel solution were loaded into the syringe pumps respectively and connected to the corresponding spinnerets. The spacing between the spinning nozzles was adjusted, and the stent 3D printing was started. The vascular stent was prepared by controlling the movement of the syringe pump and the spinning nozzle.
[0073] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A 3D printed degradable vascular stent, comprising: The first radiating fiber, the second radiating fiber and the immunosuppressive drug are characterized by: The second radial fibers are evenly arranged in a concentric ring manner on the outer wall around the first radial fibers, and both the first radial fibers and the second radial fibers are biocompatible and biodegradable; in the same biological environment, the second radial fibers will be degraded preferentially compared to the first radial fibers, and the immunosuppressive drug is evenly dispersed and mixed in the internal structure of the second radial fibers.
2. A 3D printed degradable vascular stent according to claim 1, characterized in that: The connection between the first radiating fiber and the second radiating fiber uses hydrogel as a connection medium.
3. The 3D printed degradable vascular stent according to claim 1, characterized in that: The first radiating fiber is made of one of polylactic acid and polycaprolactone.
4. The 3D printed degradable vascular stent according to claim 1, characterized in that: The second radiating fiber is made of a mixed solution of polylactic acid-glycolic acid copolymer and immunosuppressive drugs in a mass ratio of 7-8:2-3 through a bracket 3D printing device.
5. The 3D printed degradable vascular stent according to claim 4, characterized in that: The polylactic acid-glycolic acid copolymer is prepared by uniformly mixing lactic acid and glycolic acid in a mass ratio of 4-8:2-6.
6. A method for preparing a 3D printed degradable vascular stent, based on the 3D printed degradable vascular stent according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, preparing electrospinning solutions for preparing the first radiating fiber and the second radiating fiber respectively, and adding immunosuppressive drugs to the electrospinning solution prepared for preparing the second radiating fiber; S2, building a 3D printing device for a bracket and preparing two sets of spinning nozzles, one set of spinning nozzles is located in the center and is used to prepare the first radial fiber; Another group of spinning nozzles has multiple nozzles, and all are arranged radially around the central spinning nozzle, and are used to prepare the second radial fiber; S3, the electrospinning solutions are loaded into the syringe pumps respectively and connected to the corresponding spinnerets, the spacing between the spinning nozzles is adjusted, and the 3D printing of the bracket is started.
7. The method for preparing a 3D printed degradable vascular stent according to claim 6, characterized in that: The two groups of spinning nozzles include a first nozzle, a second nozzle and a dispensing nozzle arranged between the first nozzle and the second nozzle; the first nozzle is connected to an electrospinning solution for preparing a first radiating fiber, the second nozzle is connected to an electrospinning solution for preparing a second radiating fiber, and the dispensing nozzle is connected to a hydrogel solution.
8. The method for preparing a 3D printed degradable vascular stent according to claim 7, characterized in that: The inner wall of the first nozzle is provided with a plurality of grooves corresponding to the second nozzle, and the grooves are used to accommodate the prepared second radiation fibers.
9. The method for preparing a 3D printed degradable vascular stent according to claim 6, characterized in that: The immunosuppressive drug is at least one of rapamycin, paclitaxel, everolimus, atorvastatin, aspirin, clopidogrel, ticagrelor, metoprolol, and Diovan.
10. The method for preparing a 3D printed degradable vascular stent according to claim 6, characterized in that: The inner diameter of the first radiating fiber is 2-4 mm, and the thickness is 200-300 μm; the inner diameter of the second radiating fiber is 1-3 mm, and the thickness is 100-150 μm; the thickness of the hydrogel coating is 30-60 μm.
Citation Information
Cited By
Degradable coronary artery stent and preparation method thereof
CN121987861A