Microwave-assisted hydrothermal induction heterostructure composite material as well as preparation method and application thereof
The metal oxide and biochar composite material prepared by the microwave-assisted hydrothermal induction method solves the problems of high preparation cost and unsatisfactory catalytic effect in the existing technology, and achieves high-efficiency pollutant degradation effect at low cost and low equipment requirements.
Patent Information
- Application Number
- CN202410867740.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-22
AI Technical Summary
Existing biochar modification methods have high preparation costs, high equipment requirements, and unsatisfactory catalytic effects, making it difficult to effectively adsorb heavy metals and organic pollutants.
The microwave-assisted hydrothermal induction method is used to prepare metal oxides such as Fe2O3, CuO, CoO and NiO and biochar composite materials. Sugarcane bagasse or rice husk carbonization products are used to form heterostructure composite materials through ultrasonic treatment and microwave hydrothermal reaction.
Biochar modification with low cost and low equipment requirements is achieved. The material is reusable and has a high catalytic degradation rate. It is suitable for the degradation of a variety of pollutants, including common dyes, pigments and antibiotics.
Smart Images

Figure CN118807747A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biochar composite materials. Background Art
[0002] my country is a country dominated by agriculture, which leads to the generation of a large amount of agricultural solid waste. These agricultural solid wastes occupy a large area and contain a large amount of biomass energy. If they are not handled properly, they will have a bad impact on the environment. Therefore, it is particularly necessary to recycle agricultural solid waste, and preparing it into biochar is an efficient and feasible method.
[0003] As a new type of material with porous loose structure and high specific surface area, biochar has excellent adsorption performance, microbial activity and chemical stability, which makes it have important application prospects in water treatment. The utilization of agricultural waste for biochar resources and its application in various environmental pollution treatment will be a very environmentally friendly and practical field. However, due to the light weight, small powder particles and single composition of biochar, the effect of adsorbing heavy metals and organic pollutants is affected, and the recovery in water and soil is also limited. Modified biochar can make up for some shortcomings of single biochar and improve the adsorption effect.
[0004] At present, there are several main methods for modifying biochar: (1) Oxidation method: Oxidation functional groups (including C=O, -OH and -COOH) are very important for improving the performance of biochar in various applications. For example, when biochar is used as an adsorbent for removing heavy metals, the surface -OH and -COOH groups can greatly improve the adsorption capacity. Among the methods of introducing oxidative functional groups, surface oxidation is one of the most widely used methods. Hydrogen peroxide (H2O2), ozone (O3), potassium permanganate (KMnO4) and nitric acid (HNO3) are generally used for surface oxidation. (2) Amination method: Introducing amino groups into the surface of biochar can greatly improve its performance in applications such as carbon dioxide absorption and pollutant adsorption. (3) Metal loading method: Through the reducibility and porous characteristics of biochar materials, metals are introduced as adsorption active sites or catalytic reaction sites of biochar.
[0005] However, the above methods have high modification temperature requirements (400-600° C.), which leads to high requirements on equipment and high preparation costs, and the catalytic effect of the obtained catalyst is not ideal. Summary of the invention
[0006] The purpose of the present invention is to provide a microwave-assisted hydrothermal induced heterogeneous structure composite material, a preparation method and application thereof. The present invention has the advantages of low preparation cost, can reduce the burden on the ecological environment, has low equipment requirements, can be repeatedly used, and has a wide range of applications.
[0007] The technical solution of the present invention is a microwave-assisted hydrothermal-induced heterogeneous structure composite material, which is composited with biochar and metal oxides, and the metal oxides are one or more of Fe2O3, CuO, CoO and NiO.
[0008] In the aforementioned microwave-assisted hydrothermal-induced heterogeneous structure composite material, the biochar is a carbonized product of sugarcane bagasse or rice husk.
[0009] The above-mentioned method for preparing the microwave-assisted hydrothermal-induced heterogeneous structure composite material comprises the following steps:
[0010] a. Take biomass raw materials, crush them to obtain product A.
[0011] b. Take the nitrate solution and treat it ultrasonically to obtain product B.
[0012] c. Take H2SO4 solution and treat it ultrasonically to obtain product C.
[0013] d. Mix product B and product C and then perform ultrasonic treatment to obtain product D.
[0014] e. After mixing product A and product D, they are first subjected to microwave treatment and then hydrothermal reaction to obtain product E.
[0015] f. Product E is dried, placed in a muffle furnace for calcination, and subjected to pyrolysis reaction to obtain a reaction product, namely, a finished product.
[0016] In the aforementioned method for preparing microwave-assisted hydrothermal-induced heterogeneous structure composite materials, in step a, the biomass raw material is bagasse or rice husk, and the biomass raw material is preliminarily crushed, sieved with a 100-mesh sieve, and the retained portion is crushed again and washed to obtain product A.
[0017] In the aforementioned method for preparing microwave-assisted hydrothermal-induced heterogeneous structure composite materials, in step b, the nitrate solution is Fe(NO3)3 solution, Cu(NO3)2 solution, Co(NO3)2 solution or Ni(NO3)2 solution, the concentration of the nitrate solution is 0.2-0.5 mol / L, and the ultrasonic treatment is performed for 5-30 min.
[0018] In the above-mentioned method for preparing the microwave-assisted hydrothermal-induced heterogeneous structure composite material, in the step c, the concentration of the H2SO4 solution is 10-20%, and the ultrasonic treatment is performed for 5-30 minutes.
[0019] In the aforementioned method for preparing the microwave-assisted hydrothermal-induced heterogeneous structure composite material, in the step d, the mixing ratio of product B and product C is 4:1 according to the volume ratio, and the ultrasonic treatment time is 5-30 minutes.
[0020] The aforementioned method for preparing microwave-assisted hydrothermal-induced heterogeneous structure composite materials, the step e, is to mix product A and product D, microwave treat them for 5-30 minutes, and then transfer them to a hydrothermal kettle to carry out hydrothermal reaction in an oven, the hydrothermal reaction temperature is 100-120°C, and the hydrothermal reaction time is 24-48 hours.
[0021] In the above-mentioned microwave-assisted hydrothermal induced heterogeneous structure composite material preparation method, in the step f, the heating rate of calcination should be 4-5°C·min -1 The final temperature of calcination is 200-400℃, and the calcination time is 1-3h.
[0022] The aforementioned microwave-assisted hydrothermal-induced heterogeneous structure composite material is applied in wastewater treatment.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] (1) The main materials can be obtained from agricultural waste, with low preparation cost, which effectively implements the concept of agricultural waste resource utilization and reduces the burden on the ecological environment.
[0025] (2) The preparation temperature does not exceed 120°C, so the equipment requirements are low, and household microwave ovens can also be used, further reducing the preparation cost.
[0026] (3) The obtained composite material has good morphology, is not easy to lose, and can be reused many times, thereby reducing the cost of sewage treatment. After three reuses, the degradation efficiency can still reach 90%, and the catalytic effect is good.
[0027] (4) It has a wide range of applications and can degrade a variety of pollutants, including common dyes, pigments, antibiotics, etc.
[0028] In summary, the present invention has the advantages of low preparation cost, reducing the burden on the ecological environment, low equipment requirements, repeated use, and a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the SEM electron microscope photo of Fe2O3 / BCMW in Example 1.
[0030] Figure 2 This is a diagram of the recycling and degradation effect of Fe2O3 / BCMW in Example 1 of the present invention.
[0031] Figure 3 This is a diagram showing the degradation effect of Fe2O3 / BCMW on different pollutants in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0033] Embodiment 1 (optimal embodiment): A method for preparing a microwave-assisted hydrothermal-induced heterogeneous structure composite material. It comprises the following steps: grinding and crushing bagasse through a 100-mesh sieve to remove impurities, and then crushing and cleaning the retained portion of the sieve to obtain product A. A 0.2 mol / L Fe(NO3)3 solution is prepared, and ultrasonicated for 10 minutes to obtain product B. A 10% concentration H2SO4 solution is prepared, and ultrasonicated for 10 minutes to obtain product C. According to the volume ratio, products B and C are prepared in a ratio of 4:1, and the prepared solution is ultrasonicated for 10 minutes to obtain product D. Take 1g of product A and 50mL of product D, put them into a reaction container and mix them thoroughly, and then place them under a microwave at a power of 20 for 5 minutes to obtain product E1. Product E1 is transferred to a hydrothermal kettle and subjected to a hydrothermal reaction at 120°C for 24 hours to obtain product E. Product E is filtered and cleaned, dried, and then placed in a muffle furnace for calcination to carry out a pyrolysis reaction. The heating rate is set to 5°C·min during calcination. -1 , the temperature is raised to 250℃, and the reaction time is 2h. After the reaction is completed, the finished composite material is obtained, named Fe2O3 / BM MW The experimental results show that the photo-Fenton catalytic degradation rate of this sample is 97%, and it has good degradation ability for organic dyes and antibiotics.
[0034] Example 2: Compared with Example 1, the difference is that the Fe(NO3)3 solution is replaced by a Cu(NO3)2 solution of the same concentration, and the resulting product is named CuO / BM MW The results of the experiment showed that the sample had a photo-Fenton catalytic degradation rate of 90% and had good degradation ability for organic dyes and antibiotics.
[0035] Experimental Example 3: Compared with Example 1, the difference is that the Fe(NO3)3 solution is replaced by the Co(NO3)2 solution of the same concentration, and the obtained product is named CoO / BM MW The experimental results show that the photo-Fenton catalytic degradation rate of this sample is 92%, and it has good degradation ability for organic dyes and antibiotics.
[0036] Experimental Example 4: Compared with Example 1, the difference is that the Fe(NO3)3 solution is replaced by a Ni(NO3)2 solution of the same concentration, and the resulting product is named NiO / BM MW The experimental results show that the photo-Fenton catalytic degradation rate of this sample is 87%, and it has good degradation ability for organic dyes and antibiotics.
[0037] Example 5: Compared with Example 1, the difference is that sugarcane bagasse is replaced with rice husk, and the obtained product is named Fe(NO3)3 / BM. It can be measured through experiments that this sample has a photo-Fenton catalytic degradation rate of 89%, and has good degradation ability for organic dyes and antibiotics.
[0038] Example 6: Compared with Example 1, the difference is that the concentration of Fe(NO3)3 solution is adjusted to 0.5 mol / L, and the obtained product is named Fe2O3 / BM MW 0.5mol / L. The experiment showed that the photo-Fenton catalytic degradation rate of this sample was 87%, and it had good degradation ability for organic dyes and antibiotics.
[0039] Example 7: Compared with Example 1, the difference is that the concentration of Fe(NO3)3 solution is adjusted to 0.4 mol / L, and the obtained product is named Fe2O3 / BM MW 40%. Through experiments, it can be measured that the photo-Fenton catalytic degradation rate of this sample is 79%, and it has good degradation ability for organic dyes and antibiotics.
[0040] Example 8: Compared with Example 1, the difference is that the ratio of product B to product C is changed from 4:1 to 1:1. The finished product is named Fe2O3 / BM MW 1:1. Experiments have shown that this sample has a photo-Fenton catalytic degradation rate of 80%, and has good degradation capabilities for organic dyes and antibiotics.
[0041] Example 9: Compared with Example 1, the difference is that after the A product and the D product are put into the reaction container and mixed thoroughly, they are placed under microwave for 30 minutes. The finished product is named Fe2O3 / BM MW 30min. The experiment showed that the sample had a photo-Fenton catalytic degradation rate of 82%, and had good degradation ability for organic dyes and antibiotics.
[0042] Example 10: Compared with Example 1, the difference is that product E1 is transferred to a hydrothermal reactor for hydrothermal reaction at 100°C. The obtained product is named Fe2O3 / BM MW 100℃. The experiment shows that the sample has a photo-Fenton catalytic degradation rate of 87%, and has good degradation ability for organic dyes and antibiotics.
[0043] Example 11: Compared with Example 1, the difference is that the time for transferring product E1 to the hydrothermal reactor for hydrothermal reaction is 48 hours. The obtained finished product is named Fe2O3 / BM MW 48h. The experiment showed that the photo-Fenton catalytic degradation rate of this sample was 83%, and it had good degradation ability for organic dyes and antibiotics.
[0044] Example 12: Compared with Example 1, the difference is that the temperature of product E is raised to 200°C during calcination. The obtained finished product is named Fe2O3 / BM MW200℃. The experiment shows that the sample has a photo-Fenton catalytic degradation rate of 76%, and has good degradation ability for organic dyes and antibiotics.
[0045] Example 13: Compared with Example 1, the difference is that the heating rate of E product is set at 4℃·min during calcination. -1 The finished product is named Fe2O3 / BM MW 4℃·min -1 Through experiments, it can be measured that the photo-Fenton catalytic degradation rate of this sample is 77%, and it has good degradation ability for organic dyes and antibiotics.
[0046] Example 14: Compared with Example 1, the difference is that the temperature of product E is raised to 400°C during calcination. The finished product is named Fe2O3 / BM MW 400℃. The experiment shows that the sample has a photo-Fenton catalytic degradation rate of 75%, and has good degradation ability for organic dyes and antibiotics.
[0047] Example 15: Compared with Example 1, the difference is that the reaction time of calcination of product E is 1 hour. The finished product is named Fe2O3 / BM MW 1h. The experiment showed that the sample had a photo-Fenton catalytic degradation rate of 72%, and had good degradation ability for organic dyes and antibiotics.
[0048] Example 16: Compared with Example 1, the difference is that the reaction time of calcination of product E is 3h. The finished product is named Fe2O3 / BM MW 3h. The experiment showed that the sample had a photo-Fenton catalytic degradation rate of 70% and had good degradation ability for organic dyes and antibiotics.
[0049] The finished product obtained by the above preparation method was used as a catalyst for dye degradation test, and the results in Table 1 were obtained.
[0050] Table 1
[0051]
[0052]
[0053] Example 17. Use of the finished product obtained by any one of the preparation methods in Examples 1 to 16 as a catalyst in sewage treatment, wherein the sewage is sewage containing organic molecular pollutants such as pigments and / or antibiotics, and the treatment comprises the following steps:
[0054] 1) Measure and adjust the target wastewater pH value to 3-7.
[0055] 2) Pour the catalyst into the contaminated aqueous solution and shake to disperse it. The amount of catalyst added is 0.05g / L-0.2g / L.
[0056] 3) Add an appropriate amount of H2O2 solution as an oxidant according to the sewage concentration, turn on the light source, which is about 10 cm away from the liquid surface, and start the reaction.
Claims
1. A microwave-assisted hydrothermal-induced heterogeneous structure composite material, characterized in that: It is composed of biochar and metal oxides, and the metal oxides are one or more of Fe2O3, CuO, CoO and NiO.
2. The method for preparing the microwave-assisted hydrothermal-induced heterogeneous structure composite material according to claim 1, characterized in that: The biochar is a carbonized product of sugarcane bagasse or rice husk.
3. The method for preparing the microwave-assisted hydrothermal-induced heterogeneous structure composite material according to claim 1 or 2, characterized in that: The following steps are included: a. Take biomass raw materials, crush them to obtain product A. b. Take the nitrate solution and treat it ultrasonically to obtain product B. c. Take H2SO4 solution and treat it ultrasonically to obtain product C. d. Mix product B and product C and then perform ultrasonic treatment to obtain product D. e. After mixing product A and product D, they are first subjected to microwave treatment and then hydrothermal reaction to obtain product E. f. Product E is dried, placed in a muffle furnace for calcination, and subjected to pyrolysis reaction to obtain a reaction product, namely, a finished product.
4. The preparation method according to claim 3, characterized in that: In the step a, the biomass raw material is bagasse or rice husk, and the biomass raw material is preliminarily crushed, sieved with a 100-mesh sieve, and the intercepted part is crushed again and washed to obtain product A.
5. The preparation method according to claim 3, characterized in that: In the step b, the nitrate solution is Fe(NO3)3 solution, Cu(NO3)2 solution, Co(NO3)2 solution or Ni(NO3)2 solution, the concentration of the nitrate solution is 0.2-0.5 mol / L, and the ultrasonic treatment is performed for 5-30 min.
6. The preparation method according to claim 3, characterized in that: In the step c, the concentration of the H2SO4 solution is 10-20%, and the ultrasonic treatment is performed for 5-30 minutes.
7. The preparation method according to claim 3, characterized in that: In the step d, the mixing ratio of product B and product C is 4:1 according to the volume ratio, and the ultrasonic treatment time is 5-30 minutes.
8. The preparation method according to claim 3, characterized in that: The step e is to mix product A and product D, perform microwave treatment for 5-30 minutes, transfer them to a hydrothermal kettle, and perform hydrothermal reaction in an oven. The hydrothermal reaction temperature is 100-120° C. and the hydrothermal reaction time is 24-48 hours.
9. The preparation method according to claim 3, characterized in that: In step f, the heating rate of calcination should be 4-5°C·min -1 The final temperature of calcination is 200-400℃, and the calcination time is 1-3h.
10. Use of the composite material according to claim 1 or 2 in sewage treatment.
Citation Information
Patent Citations
Biochar-supported magnetic substance composite adsorption material, and preparation method and application method thereof
CN106799208A
Preparation method of biochar-supported cobaltosic oxide catalytic material
CN111013590A
CuFeO2 / biochar composite magnetic material and preparation method thereof
CN111389351A
Method for preparing kitchen waste anaerobic biogas residue biochar through ultrasonic-assisted hydrothermal carbonization
CN111908753A
Preparation method of bagasse-based Ni < 2 + > and Co < 2 + > ion doped biochar material