Application of CuxFeyAlz multi-element catalyst in transfer hydrogenation reaction of benzene and ethanol
In the transfer hydrogenation reaction of benzene and ethanol, CuxFeyAlz multi-component catalyst is used to prepare highly dispersed Cu nanoparticles by co-precipitation method and synergistically interact with copper and iron to solve the high energy consumption and safety risk problems of the existing benzene hydrogenation process and achieve high efficiency. , Economical cyclohexane synthesis.
Patent Information
- Application Number
- CN202410879650.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-01
AI Technical Summary
The existing benzene hydrogenation process has problems such as high energy consumption, high risk, and low conversion rate. The traditional high-pressure hydrogenation process has high costs, high storage and transportation requirements, and high safety risks, and ethanol is not prone to hydride transfer.
It is prepared by co-precipitation method using CuxFeyAlz multi-component catalyst and is used for the transfer hydrogenation reaction of benzene and ethanol. It utilizes the synergistic effect of highly dispersed Cu nanoparticles, copper and iron to achieve efficient conversion of benzene into cyclohexane.
At 250°C, the conversion rate and selectivity of benzene exceed 99%, providing an economical and green route to synthesize cyclohexane, showing superior catalytic performance and cycle stability.
Smart Images

Figure CN118807748A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of transfer hydrogenation reaction of benzene and ethanol, and particularly relates to Cu x Fe y Al z Application of multi-component catalysts in the transfer hydrogenation of benzene and ethanol. Background Art
[0002] Cyclohexane is widely used in the field of petrochemicals and is an important chemical raw material. Its main economic use is the production of caprolactam and adipic acid, intermediates for the synthesis of nylon; cyclohexane can also be used as a flux and is an excellent flux for resins, asphalt, wax, cellulose ether and rubber. Except for a few cyclohexane obtained by distillation and separation from petroleum fractions, 90% of cyclohexane comes from the benzene hydrogenation process. Therefore, benzene hydrogenation to cyclohexane has a high economic value. The methods commonly used in industry to produce cyclohexane by benzene hydrogenation are mainly gas phase method and liquid phase method. The liquid phase benzene hydrogenation process requires a high pressure and a low conversion rate, so there are problems such as high energy consumption, high process risk and low yield. The gas phase benzene hydrogenation process is evenly mixed and the catalyst and product are easy to separate. Both the gas phase method and the liquid phase method require the use of high-pressure H2 for direct hydrogenation, resulting in high costs, high storage and transportation requirements, safety risks and operating restrictions.
[0003] Catalytic transfer hydrogenation (CTH) is considered to be an effective solution to replace the traditional high-pressure hydrogenation process due to its high efficiency, atom economy and sustainability. Reducing solvents such as methanol, ethanol and isopropanol produced in biorefineries can be used as hydrogen sources. Ethanol is an attractive hydrogen donor due to its abundance, sustainability, non-toxicity and environmental benignity, but ethanol is not prone to hydride transfer because the formed carbon cation is highly unstable. Therefore, it is very important to find a catalyst that can both dehydrogenate ethanol and hydrogenate the benzene ring. Summary of the invention
[0004] Aiming at the problems existing in the current catalytic transfer hydrogenation process for preparing cyclohexane, the present invention provides a Cu x Fe y Al z The multi-component catalyst is used for the transfer hydrogenation reaction of benzene and ethanol. At 250°C, the conversion rate of benzene is >99% (converted into cyclohexane), the selectivity is >99%, and the catalyst exhibits excellent catalytic performance. The catalyst is prepared by a coprecipitation method. Highly dispersed Cu nanoparticles and a relatively high metal copper area as well as the synergistic effect between copper and iron are key factors in improving the transfer hydrogenation yield. The catalyst is used for the transfer hydrogenation reaction of benzene and ethanol.
[0005] The technical solution of the present invention is as follows:
[0006] Cux Fe y Al z Application of a multi-component catalyst in the transfer hydrogenation reaction of benzene and ethanol, wherein x=8, 0<y≤2, 0<z≤2.
[0007] Preferably, the Cu x Fe y Al z The multi-catalyst is prepared by a co-precipitation method.
[0008] Preferably, the catalyst also includes CeO2, i.e. Cu x Fe y Al z / CeO2; preferably, the molar ratio of Ce to Al is 1-2:1.
[0009] Preferably, the Cu x Fe y Al z The multi-component catalyst preparation method comprises the following steps:
[0010] (1) Copper salt, iron salt and aluminum salt are mixed uniformly to prepare a precursor solution;
[0011] (2) slowly dripping the precursor solution and the alkaline precipitant solution of step (1) into the reactor simultaneously to react;
[0012] (3) Washing, drying, calcining; reducing gas reduction treatment, directly used in the transfer hydrogenation reaction of benzene and ethanol.
[0013] Furthermore, in step (1), the molar ratio of copper, iron and aluminum in the copper salt, iron salt and aluminum salt is 8:0.5-2:0.5-2.
[0014] Furthermore, the reaction conditions in step (2) are: 70°C-90°C, and the reaction time is more than 12 hours.
[0015] Furthermore, CeO2 is added before the reaction in step (2).
[0016] Furthermore, the washing condition in step (3) is washing with water until the pH of the supernatant is 6-8;
[0017] Furthermore, the calcination conditions in step (3) are calcination at 480° C. for 2-6 h at a heating rate of 2° C. / min;
[0018] Furthermore, in step (3), the reducing gas reduction treatment process is: under a hydrogen atmosphere, the reduction is carried out at a heating rate of 2°C / min for 2 hours, and the reduction temperature is 200°C.
[0019] Beneficial Effects of the Invention
[0020] At present, the catalyst commonly used for ethanol dehydrogenation is mainly based on Cu-based catalysts, and the metals with catalytic activity for benzene hydrogenation include Rh, Pt, W, Ni, Fe, Pd, Co, etc. The present invention prepares a Cu-Fe-Al ternary catalyst by a simple coprecipitation method, and uses it for the transfer hydrogenation reaction of benzene and ethanol. The conversion rate of benzene at 250°C is >99% (converted into cyclohexane), and the selectivity is >99%, showing excellent catalytic performance and cycle stability. The present invention provides an economical and green way for synthesizing cyclohexane by hydrogenation of benzene. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a transmission electron microscope image of the Cu8Fe1Al1 catalyst prepared in Example 1. DETAILED DESCRIPTION
[0022] Example 1
[0023] Weigh 48.3g of Cu(NO3)2·3H2O, 10.1g of Fe(NO3)3·9H2O and 9.38g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water. Ultrasonicate for 15min to dissolve and form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. Slowly drip the metal precursor solution and the precipitant solution into a three-necked flask pre-filled with 400ml and stir magnetically for 30min, heat to 80℃, age for 12h, centrifuge the mixture and wash with deionized water until the pH of the supernatant is about 7, then place it in a vacuum drying oven at 80℃ and dry it for 20h. The obtained solid is calcined at 480℃ in a muffle furnace at a heating rate of 2℃ / min for 3h. The sample was then placed in a hydrogen atmosphere and reduced for 2 hours at a heating rate of 2°C / min at a reduction temperature of 200°C. After reduction, it was directly used as a catalyst. The reduced catalyst was named Cu8Fe1Al1.
[0024] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 350 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 ml / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 ml / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. The conversion rate of benzene at 250°C was 99.7% (converted to cyclohexane) and the selectivity was 99.3%.
[0025] Example 2
[0026] Weigh 48.3g of Cu(NO3)2·3H2O, 10.1g of Fe(NO3)3·9H2O and 9.38g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water. Ultrasonicate for 15min to dissolve and form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. Slowly drip the metal precursor solution and the precipitant solution into a three-necked flask pre-filled with 400ml and stir magnetically for 30min, heat to 80℃, age for 12h, centrifuge the mixture and wash with deionized water until the pH of the supernatant is about 7, then place it in a vacuum drying oven at 80℃ and dry it for 20h. The obtained solid is calcined at 480℃ in a muffle furnace at a heating rate of 2℃ / min for 3h. The sample was then placed in a hydrogen atmosphere and reduced for 2 hours at a heating rate of 2°C / min at a reduction temperature of 200°C. After reduction, it was directly used as a catalyst. The reduced catalyst was named Cu8Fe1Al1.
[0027] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). 100 mg of the catalyst was weighed and pretreated for 2 h under a H2 gas flow at 350 ° C. After the pretreatment, argon was purged for 30 min at a flow rate of 36 ml / min to remove the residual hydrogen in the pipeline. Then the reactants (mixed solution of ethanol and benzene) were pumped into the reactor using a micro-injection pump. The reactant flow rate was 0.04 ml / min, and the space velocity (WHSV) was 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. The conversion rate of benzene at 250°C was 89.6% (converted to cyclohexane) and the selectivity was 91.2%.
[0028] Example 3
[0029] Weigh 48.3g of Cu(NO3)2·3H2O, 10.1g of Fe(NO3)3·9H2O and 9.38g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water, and dissolve them by ultrasonic for 15min to form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. The metal precursor solution and the precipitant solution were slowly dripped into a three-necked flask pre-filled with 400 ml and magnetically stirred for 30 minutes. 4.3 g of CeO2 was added to the above solution, and magnetically stirred for 15 minutes to obtain a uniform suspension. The mixture was heated to 80°C and aged for 12 hours. The mixture was centrifuged and washed with deionized water until the pH of the supernatant was about 7, and then placed in a vacuum drying oven at 80°C for 20 hours. The obtained solid was calcined at 480°C in a muffle furnace at a heating rate of 2°C / min for 3 hours. The sample was then placed in a hydrogen atmosphere and reduced at a heating rate of 2°C / min for 2 hours. The reduction temperature was 200°C. After reduction, it was directly used as a catalyst. The reduced catalyst was named Cu8Fe1Al1 / CeO2 (Ce:Al=1:1).
[0030] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 200 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 mL / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 mL / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400 °C, and the sample was injected and analyzed after stabilization at 50 °C for 15 minutes. The conversion rate of benzene at 250 °C was 85.2% (converted to cyclohexane), and the selectivity was 96.1%.
[0031] Example 4
[0032] Weigh 48.3g of Cu(NO3)2·3H2O, 10.1g of Fe(NO3)3·9H2O and 9.38g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water, and dissolve them by ultrasonic for 15min to form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. The metal precursor solution and the precipitant solution were slowly dripped into a three-necked flask pre-filled with 400 ml and magnetically stirred for 30 minutes. 8.6 g of CeO2 was added to the above solution, and magnetically stirred for 15 minutes to obtain a uniform suspension. The mixture was heated to 80°C and aged for 12 hours. The mixture was centrifuged and washed with deionized water until the pH of the supernatant was about 7, and then placed in a vacuum drying oven at 80°C for 20 hours. The obtained solid was calcined at 480°C in a muffle furnace at a heating rate of 2°C / min for 3 hours. The sample was then placed in a hydrogen atmosphere and reduced at a heating rate of 2°C / min for 2 hours. The reduction temperature was 200°C. After reduction, it was directly used as a catalyst. The reduced catalyst was named Cu8Fe1Al1 / CeO2 (Ce:Al=2:1).
[0033] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 200 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 mL / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 mL / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. The conversion rate of benzene at 250°C was 89.3% (converted to cyclohexane) and the selectivity was 98.1%.
[0034] Example 5
[0035] Weigh 48.3g of Cu(NO3)2·3H2O, 20.2g of Fe(NO3)3·9H2O and 9.38g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water. Ultrasonicate for 15min to dissolve and form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. Slowly drip the metal precursor solution and the precipitant solution into a three-necked flask pre-filled with 400ml and stir magnetically for 30min, heat to 80℃, age for 12h, centrifuge the mixture and wash with deionized water until the pH of the supernatant is about 7, then place it in a vacuum drying oven at 80℃ and dry it for 20h. The obtained solid is calcined at 480℃ in a muffle furnace at a heating rate of 2℃ / min for 3h. The sample was then placed in a hydrogen atmosphere and reduced at a heating rate of 2°C / min for 2h at a reduction temperature of 200°C. After reduction, it was directly used as a catalyst. The reduced catalyst was named Cu8Fe2Al1.
[0036] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 350 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 ml / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 ml / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. The conversion rate of benzene at 250°C was 88.6% (converted to cyclohexane) and the selectivity was 90.7%.
[0037] Example 6
[0038] Weigh 48.3g of Cu(NO3)2·3H2O, 5.05g of Fe(NO3)3·9H2O and 9.38g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water. Ultrasonicate for 15min to dissolve and form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. Slowly drip the metal precursor solution and the precipitant solution into a three-necked flask pre-filled with 400ml and stir magnetically for 30min, heat to 80℃, age for 12h, centrifuge the mixture and wash with deionized water until the pH of the supernatant is about 7, then place it in a vacuum drying oven at 80℃ and dry it for 20h. The obtained solid is calcined at 480℃ in a muffle furnace at a heating rate of 2℃ / min for 3h. The sample was then placed in a hydrogen atmosphere and reduced at a heating rate of 2°C / min for 2h at a reduction temperature of 200°C. After reduction, it was used directly as a catalyst. The reduced catalyst was named Cu8Fe 0.5 Al1.
[0039] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 350 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 ml / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 ml / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. The conversion rate of benzene at 250°C was 91.3% (converted to cyclohexane) and the selectivity was 94.5%.
[0040] Example 7
[0041] Weigh 48.3g of Cu(NO3)2·3H2O, 10.1g of Fe(NO3)3·9H2O and 18.76g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water. Ultrasonicate for 15min to dissolve and form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. Slowly drip the metal precursor solution and the precipitant solution into a three-necked flask pre-filled with 400ml and stir magnetically for 30min, heat to 80℃, age for 12h, centrifuge the mixture and wash with deionized water until the pH of the supernatant is about 7, then place it in a vacuum drying oven at 80℃ and dry it for 20h. The obtained solid is calcined at 480℃ in a muffle furnace at a heating rate of 2℃ / min for 3h. The sample was then placed in a hydrogen atmosphere and reduced for 2 hours at a heating rate of 2°C / min at a reduction temperature of 200°C. After reduction, it was directly used as a catalyst. The reduced catalyst was named Cu8Fe1Al2.
[0042] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 350 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 ml / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 ml / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. The conversion rate of benzene at 250°C was 89.4% (converted to cyclohexane), and the selectivity was 73.6%.
[0043] Example 8
[0044] Weigh 48.3g of Cu(NO3)2·3H2O, 10.1g of Fe(NO3)3·9H2O and 4.69g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water. Ultrasonicate for 15min to dissolve and form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. Slowly drip the metal precursor solution and the precipitant solution into a three-necked flask pre-filled with 400ml and stir magnetically for 30min, heat to 80℃, age for 12h, centrifuge the mixture and wash with deionized water until the pH of the supernatant is about 7, then place it in a vacuum drying oven at 80℃ and dry it for 20h. The obtained solid is calcined at 480℃ in a muffle furnace at a heating rate of 2℃ / min for 3h. The sample was then placed in a hydrogen atmosphere and reduced at a heating rate of 2°C / min for 2h at a reduction temperature of 200°C. After reduction, it was used directly as a catalyst. The reduced catalyst was named Cu8Fe1Al 0.5 .
[0045] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 350 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 ml / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 ml / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. The conversion rate of benzene at 250°C was 91.2% (converted to cyclohexane) and the selectivity was 88.3%.
[0046] Comparative Example 1
[0047] Weigh 48.3g of Cu(NO3)2·3H2O and 9.38g of Al(NO3)3·9H2O and dissolve them in 400ml of deionized water. Ultrasonicate for 15min to dissolve and form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. Slowly drip the metal precursor solution and the precipitant solution into a three-necked flask pre-filled with 400ml and stir magnetically for 30min, heat to 80℃, age for 12h, centrifuge the mixture and wash with deionized water until the pH of the supernatant is about 7, then place it in a vacuum drying oven at 80℃ and dry it for 20h. The obtained solid is calcined at 480℃ in a muffle furnace at a heating rate of 2℃ / min for 3h. Then place the sample in a hydrogen atmosphere and reduce it at a heating rate of 2℃ / min for 2h. The reduction temperature is 200℃. After reduction, it is directly used as a catalyst. The reduced catalyst was named Cu8Fe0Al1.
[0048] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 350 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 ml / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 ml / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. The conversion rate of benzene at 250°C was 66.7% (converted to cyclohexane), and the selectivity was 86.8%.
[0049] Comparative Example 2
[0050] Weigh 48.3g of Cu(NO3)2·3H2O and 10.1g of Fe(NO3)3·9H2O and dissolve them in 400ml of deionized water. Ultrasonicate for 15min to dissolve and form a uniform metal ion precursor solution. Then weigh 16g of NaOH and 5.3g of Na2CO3 and dissolve them in 400ml of deionized water to prepare a precipitant solution. Slowly drip the metal precursor solution and the precipitant solution into a three-necked flask pre-filled with 400ml and stir magnetically for 30min, heat to 80℃, age for 12h, centrifuge the mixture and wash with deionized water until the pH of the supernatant is about 7, then place it in a vacuum drying oven at 80℃ and dry it for 20h. The obtained solid is calcined at 480℃ in a muffle furnace at a heating rate of 2℃ / min for 3h. The sample is then placed in a hydrogen atmosphere and reduced at a heating rate of 2℃ / min for 2h. The reduction temperature is 200℃. After reduction, it is directly used as a catalyst. The reduced catalyst was named Cu8Fe1Al0.
[0051] The transfer hydrogenation reaction was carried out in a fixed bed reactor (quartz reaction tube, ID = 8 mm). Weigh 200 mg of the catalyst and pretreat it under H2 gas flow at 350 ° C for 2 h. After the pretreatment, purge with argon at a flow rate of 36 ml / min for 30 min to remove the residual hydrogen in the pipeline. Then use a micro-injection pump to pump the reactants (mixed solution of ethanol and benzene) into the reactor. The reactant flow rate is 0.04 ml / min, and the space velocity (WHSV) is 13.67 h -1 The product analysis was measured by online gas chromatograph. The catalyst performance was tested between 200 and 400°C, and the sample was injected and analyzed after stabilization at 50°C for 15 minutes. At 250°C, the conversion rate of benzene was 72.1% (converted to cyclohexane) and the selectivity was 65.4%.
Claims
1. Cu x Fe y Al z The application of a multi-component catalyst in the transfer hydrogenation reaction of benzene and ethanol is characterized in that: in: x=8, 0<y≤2, 0<z≤2.
2. The use according to claim 1, characterized in that: The Cu x Fe y Al z The multi-catalyst is prepared by a co-precipitation method.
3. The use according to claim 1 or 2, characterized in that: The catalyst also includes CeO2, i.e. Cu x Fe y Al z / CeO2; preferably, the molar ratio of Ce to Al is 1:
1.
4. The use according to claim 1 or 2, characterized in that: The Cu x Fe y Al z The multi-component catalyst preparation method comprises the following steps: (1) Copper salt, iron salt and aluminum salt are mixed uniformly to prepare a precursor solution; (2) slowly dripping the precursor solution and the alkaline precipitant solution of step (1) into the reactor simultaneously to react; (3) Washing, drying, calcining; reducing gas reduction treatment, directly used in the transfer hydrogenation reaction of benzene and ethanol.
5. The use according to claim 4, characterized in that: The molar ratio of copper, iron and aluminum in the copper salt, iron salt and aluminum salt in step (1) is 8:1:
1.
6. The use according to claim 4, characterized in that: The reaction conditions in step (2) are: 70° C.-90° C., and the reaction time is more than 12 hours.
7. The use according to claim 4, characterized in that: In step (2), CeO2 is added before the reaction.
8. The use according to claim 4, characterized in that: The washing condition in step (3) is to wash with high-purity water until the pH of the supernatant is 6-8.
9. The use according to claim 4, characterized in that: The calcination conditions in step (3) are calcination at 480° C. for 2-6 h at a heating rate of 2° C. / min.
10. The use according to claim 4, characterized in that: The reducing gas reduction treatment process in step (3) is: reduction is carried out under a hydrogen atmosphere at a heating rate of 2°C / min for 2h, and the reduction temperature is 200°C.
Citation Information
Patent Citations
Preparation method and application of easy-to-recover high-selectivity furfural hydrogenation catalyst
CN112892537A
Metal oxide promoted copper-based catalyst with hydrogen transfer hydrogenation activity and preparation and application thereof
CN115814805A
A process for the manufacture of cyclohexane by catalytic hydrogenation of benzene in the vapour phase
GB623425A
catalyst
US20060199981A1