Application of Ag2WO4 / CuBi2O4 composite material in ultrasonic catalytic degradation of organic pollutants in wastewater

By using the Ag2WO4/CuBi2O4 composite material as an ultrasonic catalyst to degrade tetracycline in water under ultrasonic conditions, the problem of difficulty in removing tetracycline pollution in the existing technology is solved, and efficient and green wastewater treatment is achieved.

CN118807774AActive Publication Date: 2024-10-22SHENZHEN HONGYUE INFORMATION TECH CO LTD

Patent Information

Application Number
CN202410783661.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-22
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Existing technologies are difficult to effectively remove tetracycline antibiotic pollution in water bodies, and traditional treatment technologies cannot completely remove tetracyclines, resulting in environmental pollution and health risks.

Method used

Ag2WO4/CuBi2O4 composite material is used as an ultrasonic catalyst to degrade tetracycline in wastewater under ultrasonic conditions. By synthesizing the composite material and performing ultrasonic treatment at different mass ratios and addition amounts, the activity and removal efficiency of the catalyst can be improved.

Benefits of technology

Efficient degradation of tetracycline is achieved, with a degradation rate of 87.14%. The preparation method is simple and non-toxic, providing a green and environmentally friendly wastewater treatment solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807774A_ABST
    Figure CN118807774A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solid ultrasonic catalysis, and particularly relates to application of an Ag2WO4 / CuBi2O4 composite material in ultrasonic catalytic degradation of organic pollutants in wastewater. The method comprises the following steps: adding an Ag2WO4 / CuBi2O4 composite material into wastewater containing organic pollutants, and carrying out ultrasonic treatment for 2 hours under the ultrasonic power of 500W. The degradation rate of tetracycline in water can reach 85.05 + / -4.84%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid ultrasonic catalysis, and specifically relates to an Ag 2 WO 4 / CuBi 2 O 4 Application of composite materials in ultrasonic catalytic degradation of organic pollutants in wastewater. Background Art

[0002] At present, the environmental pollution and health risks caused by the abuse of antibiotics have become a hot topic of research in recent years. Tetracycline is a broad-spectrum antibiotic that is widely used in the treatment of diseases in animal husbandry and aquaculture due to its low price. In addition, tetracycline is highly water-soluble and has a long half-life. Its stable nucleus structure makes it impossible to remove tetracycline through traditional treatment technologies. It is often reported that tetracycline can be detected in surface water, groundwater and sediments. In summary, finding a wastewater treatment technology that has a good removal effect on tetracycline and antibiotics is a crucial link. Summary of the invention

[0003] The purpose of the present invention is to provide an efficient and environmentally friendly Ag 2 WO 4 / CuBi 2 O 4 Composite materials, as efficient and environmentally friendly acoustic catalysts that effectively solve water pollution, have broad application potential.

[0004] The technical solution adopted by the present invention is: an Ag 2 WO 4 / CuBi 2 O 4 The composite material is used in ultrasonic catalytic degradation of organic pollutants in wastewater, the method is as follows: Ag is added to the wastewater containing organic pollutants 2 WO 4 / CuBi 2 O 4 The composite material was ultrasonicated at an ultrasonic power of 500 W for 2 h.

[0005] In the above application, the organic pollutant is tetracycline.

[0006] In the above application, the initial concentration of organic pollutants was 40 mg / L.

[0007] In the above applications, among organic pollutants, Ag 2 WO 4 / CuBi 2 O 4The addition amounts of composite materials were 0, 0.5 g / L, 1 g / L, 1.5 g / L, and 2 g / L, respectively.

[0008] For the above applications, Ag 2 WO 4 / CuBi 2 O 4 The preparation method of the composite material comprises the following steps: 2 O 4 AgNO was slowly dripped into the suspension while stirring. 3 The aqueous solution was stirred in the dark and Na 2 WO 4 ·2H 2 O aqueous solution was slowly added to the above mixed solution, and stirring, suction filtration, washing and drying were continued in a dark environment to obtain Ag 2 WO 4 / CuBi 2 O 4 Composite materials.

[0009] For the above applications, CuBi 2 O 4 The preparation method comprises the following steps: 3 ) 3 ·5H 2 O dilute nitric acid solution was stirred, and Cu(NO 3 ) 2 ·5H 2 O aqueous solution, and then slowly add NaOH solution to obtain a white-green suspension and continue stirring. After stirring, a hydrothermal reaction is carried out. After the reaction is completed, the solution is filtered, washed, dried, and ground to obtain CuBi 2 O 4 powder.

[0010] In the above application, the hydrothermal reaction conditions are 180°C for 12h.

[0011] For the above application, drying is performed at 60°C for 12 h.

[0012] For the above applications, Ag 2 WO 4 The mass of CuBi added 2 O 4 10%-40% of the mass.

[0013] For the above applications, Ag 2 WO 4 The mass of CuBi added 2 O 4 30% of the mass.

[0014] The beneficial effects of the present invention are: CuBi 2 O 4 It is an emerging bismuth-based catalyst with the characteristics of wide range of light energy utilization and strong photoreaction activity. Constructing heterojunction is an important way to improve CuBi 2 O 4 The effective means of catalytic activity, while Ag 2 WO 4 It has good photocatalytic performance and excellent electrical conductivity. In addition to the excellent performance of silver-based catalysts, Ag 2 WO 4 The preparation process is simple and it is considered to be one of the most effective semiconductors currently. 2 WO 4 / CuBi 2 O 4 Composite material combined with ultrasonic degradation of tetracycline, the results showed that the prepared Ag 2 WO 4 / CuBi 2 O 4 The composite material has the advantages of good degradation effect, simple preparation method and non-toxicity, etc., and provides a new solution for ultrasonic catalytic treatment of organic pollutants in wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The Ag with different composite ratios obtained in Example 1 2 WO 4 / CuBi 2 O 4 XRD patterns of the composite materials.

[0016] Figure 2 It is CuBi 2 O 4 (A), Ag 2 WO 4 (B) and SEM images of the composite ACBO (C).

[0017] Figure 3 Is different Ag 2 WO 4 Image of the change in tetracycline removal rate of ACBO sonocatalytic system under different composite percentages.

[0018] Figure 4 The effect of the dosage of ACBO-30 added on the removal rate of tetracycline.

[0019] Specific example method

[0020] The present invention is described in detail below with reference to the embodiments.

[0021] Example 1

[0022] (A) Ag with different composite ratios 2 WO 4 / CuBi 2 O 4 Preparation of composite materials

[0023] 1) CuBi 2 O 4 Preparation: 784.0 mg Bi(NO 3 ) 3 5H 2 O, dissolve it in 20mL of dilute nitric acid (1mol / L) to inhibit its hydrolysis, and prepare a solution for use. Then use an analytical balance to weigh 241.6mg Cu(NO 3 ) 2 ·3H 2 O, and dissolved it in 20 mL of deionized water to obtain Cu(NO 3 ) 2 ·3H 2 O solution. 3 ) 3 ·5H 2 O solution was placed on a magnetic stirrer and Cu(NO 3 ) 2 ·5H 2 O solution for 30 min. Keep stirring and add Cu(NO 3 ) 2 ·5H 2 O and Bi(NO 3 ) 3 5H 2 Slowly add 20mL of 2mol / L NaOH solution to the mixed solution of O to obtain a white-green suspension and continue stirring for 360min. After stirring, transfer the suspension to a 100mL reactor, put it into the reactor after the oven is preheated to 180°C, and react at 180°C for 12h. After the reaction is completed, wait for the reactor to cool to room temperature, filter out a brown solid, wash it with alcohol and water for 3 times each, and then dry it in a 60°C vacuum oven for 12h. Take out the dried product and grind it to obtain CuBi 2 O 4 powder.

[0024] 2) Ag 2 WO 4 Preparation of composite materials: Weigh 0.02 mol AgNO 3 With 0.01mol Na 2 WO 4 ·2H 2O and dissolved them in 35 mL of deionized water, and stirred thoroughly to obtain AgNO 3 with Na 2 WO 4 ·2H 2 O solution. On a magnetic stirrer, AgNO 3 The solution was added to Na 2 WO 4 ·2H 2 O solution, after stirring and reacting for 60 minutes, filter and wash, dry at 60℃ for 6 hours, take out and grind for later use.

[0025] 3) Ag 2 WO 4 / CuBi 2 O 4 Preparation of composite materials: Accurately weigh 500 mg CuBi 2 O 4 The powder was placed in 20 mL of deionized water and ultrasonically dispersed in an ultrasonic cleaner for 30 min. 3 Dissolve in 20 mL of deionized water and stir thoroughly to obtain AgNO 3 Solution. 2 O 4 The suspension was placed on a magnetic stirrer and AgNO was slowly added while stirring. 3 The solution was placed in a dark environment and stirred for 60 min. 2 WO 4 ·2H 2 O was dissolved in deionized water and 20 mL of Na 2 WO 4 ·2H 2 O solution, Na 2 WO 4 ·2H 2 O solution was slowly added to the mixed solution, and stirring was continued for 60 min in a dark environment. After stirring, the mixed solution of the above three was filtered, washed repeatedly with anhydrous ethanol and deionized water, and then placed in a 60°C vacuum drying oven for 12 h. The obtained dry product Ag 2 WO 4 / CuBi 2 O 4 Grind and mark for later use.

[0026] According to Ag 2 WO 4 The theoretical yield is 500mg CuBi 2 O 4 The compound is named according to the proportion of 2WO 4 The theoretical yield is 50 mg, then Ag 2 WO 4 / CuBi 2 O 4 The complex was named ACBO-10. ACBO-10, ACBO-20, ACBO-30 and ACBO-40 were synthesized according to the same method.

[0027] (ii) Ag 2 WO 4 / CuBi 2 O 4 Characterization of composite materials

[0028] Figure 1 The Ag with different composite ratios is obtained 2 WO 4 / CuBi 2 O 4 XRD spectrum of the composite material. Figure 1 It can be seen that from the prepared pure CuBi 2 O 4 The results show that by using CuBi 2 O 4 By comparing with the standard card (NO.71-1774), it can be seen that the diffraction peaks observed in the figure can be compared with CuBi 2 O 4 The (200), (211), (002), (130), (202), (141), (123), and (521) crystal planes have good attribution and good crystallinity. 2 WO 4 Significant diffraction peaks were observed at 2θ=18.4°, 30.1°, 32.2°, 44.6°, 56.1°, 57.5°, and 59.2° in the diffraction spectrum, which correspond to Ag, 2 WO 4 The above results show that pure CuBi without impurities was synthesized in this experiment. 2 O 4 And pure Ag 2 WO 4 Sample material. Next, it can be seen from the XRD spectrum results of different composites in the figure that when Ag 2 WO 4 When the recombination percentage increases from 10% to 40%, in addition to the CuBi 2 O 4In addition to the diffraction peaks corresponding to the substrate, the corresponding Ag 2 WO 4 The diffraction peak intensity increases with the increase of the composite ratio. This result shows that this experiment successfully deposited CuBi 2 O 4 Surface composited with Ag 2 WO 4 .

[0029] Figure 2 It is CuBi 2 O 4 (A), Ag 2 WO 4 (B) and SEM images of the composite ACBO (C). Figure 2 It can be seen that CuBi synthesized by hydrothermal method 2 O 4 It has a spherical shape and a smooth surface. Its diameter is about 5μm. Ag synthesized by precipitation method 2 WO 4 The ACBO composite synthesized by the two-step method presents a spherical CuBi 2 O 4 The surface is covered with several cubic particles, similar to CuBi 2 O 4 This result shows that Ag 2 WO 4 Successfully attached to CuBi 2 O 4 surface.

[0030] Example 2Ag 2 WO 4 / CuBi 2 O 4 Degradation of tetracycline by composite materials in collaboration with ultrasound

[0031] (A) Ag with different composite ratios 2 WO 4 / CuBi 2 O 4 Method for removing tetracycline by stirring adsorption of composite materials:

[0032] Weigh 20 mg CuBi using an analytical balance 2 O 4 , at this time Ag 2 WO 4The composite ratio is regarded as 0%, and it is added to a 250mL conical flask, and 20mL of a 40mg / L tetracycline solution is added to the flask. The conical flask is placed on a magnetic stirrer and stirred for 30 minutes in the dark. After stirring, the sample is centrifuged, and the supernatant is taken and its absorbance is detected by a UV-visible spectrophotometer to calculate CuBi. 2 O 4 The efficiency of tetracycline removal by composite materials was determined by the same method. The adsorption removal rates of tetracycline by ACBO-10, ACBO-20, ACBO-30 and ACBO-40 were compared. 2 WO 4 / CuBi 2 O 4 Response of composite materials.

[0033] (II) Ag with different composite ratios 2 WO 4 / CuBi 2 O 4 Method for degradation of tetracycline by composite materials in collaboration with ultrasonic catalysis:

[0034] Weigh 20 mg CuBi using an analytical balance 2 O 4 , at this time Ag 2 WO 4 The composite ratio is regarded as 0%, and it is added to a 250mL conical flask, and 20mL of a 40mg / L tetracycline solution is added to the flask. The above conical flask is placed on an ultrasonic cleaner using an iron stand so that the water surface in the instrument is just in contact with the bottom of the conical flask. A black plastic bag is used to provide a dark environment for the reaction to remove interference from the light source. Ultrasonicate for 120 minutes at an ultrasonic power of 500W. The reacted solution is extracted with a syringe, and the supernatant is obtained by filtering the membrane. The absorbance is measured by a UV spectrophotometer to calculate CuBi. 2 O 4 The efficiency of ultrasonic degradation of tetracycline by composite materials was determined by the same method. The efficiency of ACBO-10, ACBO-20, ACBO-30, and ACBO-40 in synergistic ultrasonic catalytic degradation of tetracycline was compared. 2 WO 4 / CuBi 2 O 4 Response of composite materials.

[0035] (III) Different addition amounts of Ag 2 WO 4 / CuBi 2 O 4 Method for removing tetracycline by stirring adsorption of composite materials:

[0036] Weigh 10 mg ACBO-30 accurately on a balance and add it to a 250 mL conical flask. Add 40 mg / L tetracycline solution to the conical flask and place the conical flask on a magnetic stirrer for 30 minutes in the dark. After stirring, centrifuge and collect the supernatant sample. Calculate the adsorption removal rate of tetracycline by ACBO-30 by measuring the absorbance. Similarly, change the input amount of ACBO-30 to 0 mg, 20 mg, 30 mg, and 40 mg and measure the adsorption removal rate at different addition amounts.

[0037] (IV) Different addition amounts of Ag 2 WO 4 / CuBi 2 O 4 Method for degradation of tetracycline by composite materials in collaboration with ultrasonic catalysis:

[0038] Use a balance to accurately weigh 10 mg ACBO-30 and add it to a 250 mL conical flask, add 40 mg / L tetracycline solution to the conical flask, and place the conical flask accurately above the ultrasonic site. Cover with a black plastic bag to create a dark environment, and sonicate for 120 minutes at 500 W power. Collect the supernatant sample, and calculate the ultrasonic degradation rate of tetracycline by ACBO-30 synergistically with ultrasound by measuring the absorbance. Similarly, the amount of ACBO-30 added was changed to 0 mg, 20 mg, 30 mg, and 40 mg, and the ultrasonic degradation rates at different addition amounts were measured respectively.

[0039] (V) Testing

[0040] Figure 3 Ag with different composite ratios 2 WO 4 / CuBi 2 O 4 Comparison of tetracycline removal efficiency by composite material adsorption and synergistic ultrasonic catalytic degradation of tetracycline. Figure 3 As shown, CuBi 2 O 4 The adsorption removal rates of tetracycline hydrochloride by ACBO-10, ACBO-20, ACBO-30 and ACBO-40 were 15.97 (±2.46)%, 34.80 (±1.64)%, 31.62 (±0.21)%, 27.28 (±4.16)% and 27.44 (±5.26)%, respectively, and the ultrasonic degradation rates of tetracycline hydrochloride were 60.69 (±6.90)%, 70.18 (±10.59)%, 80.83 (±4.74)%, 87.14 (±3.88)% and 57.67 (±9.23)%, respectively. When Ag 2 WO 4 Composite with CuBi2 O 4 After that, the removal rate of tetracycline by ACBO sonocatalytic system showed a trend of first increasing and then decreasing, and reached the maximum removal rate when the composite ratio was 30%. 2 WO 4 The increase in removal rate when the composite ratio increases from 10% to 30% can be considered to be due to the increase in Ag 2 WO 4 The addition of CuBi 2 O 4 After the surface is formed, the specific surface area and active sites of the catalyst material are increased, and the excess Ag 2 WO 4 Covering up CuBi 2 O 4 The original reactive active sites are removed, resulting in a decrease in the ultrasonic degradation rate of tetracycline.

[0041] Figure 4 The different amounts of Ag added 2 WO 4 / CuBi 2 O 4 Comparison of the efficiency of tetracycline removal by composite material adsorption and synergistic ultrasonic catalytic degradation of tetracycline. Figure 4 As shown, the adsorption removal rates of tetracycline by ACBO-30 with addition amounts of 0.5 g / L, 1 g / L, 1.5 g / L, and 2 g / L were 15.28 (±1.89)%, 15.96 (±4.97)%, 21.28 (±2.07)%, and 24.62 (±1.99)%, respectively; the ultrasonic degradation rates of tetracycline by ACBO-30 with addition amounts of 0, 0.5 g / L, 1 g / L, 1.5 g / L, and 2 g / L were 12.16 (±3.72)%, 79.36 (±3.89)%, 85.05 (±4.84)%, 77.79 (±10.04)%, and 74.86 (±10.68)%, respectively. It can be seen that when the amount of catalyst ACBO-30 added increases from 0.5g / L to 2.0g / L, the ultrasonic degradation rate of tetracycline first increases and then decreases. This is because the amount of catalyst added provides more active sites for adsorption and oxidation, which to a certain extent affects the number of "cavitation bubbles" formed in the solution due to heterogeneous nucleation, thereby increasing the ultrasonic degradation rate of tetracycline. However, once the ideal catalyst dosage is exceeded, the excess catalyst will hinder the penetration of ultrasound and "sonoluminescence".

Claims

1. Application of Ag2WO4 / CuBi2O4 composite material in ultrasonic catalytic degradation of organic pollutants in wastewater, characterized in that: The method is as follows: add Ag2WO4 / CuBi2O4 composite material to wastewater containing organic pollutants, and ultrasonicate for 2 hours at an ultrasonic power of 500W.

2. The use according to claim 1, characterized in that: The organic pollutant is tetracycline.

3. The use according to claim 1, characterized in that: The initial concentration of organic pollutants was 40 mg / L.

4. The use according to claim 1, characterized in that: Among the organic pollutants, the addition amounts of Ag2WO4 / CuBi2O4 composite materials were 0, 0.5 g / L, 1 g / L, 1.5 g / L, and 2 g / L, respectively.

5. The use according to claim 1, characterized in that: The preparation method of the Ag2WO4 / CuBi2O4 composite material comprises the following steps: slowly dripping an AgNO3 aqueous solution into a CuBi2O4 suspension while stirring, stirring in the dark, slowly adding an Na2WO4·2H2O aqueous solution into the mixed solution, and continuing to stir in the dark, filtering, washing and drying to obtain an Ag2WO4 / CuBi2O4 composite material.

6. The use according to claim 5, characterized in that: The preparation method of CuBi2O4 includes the following steps: stirring a dilute nitric acid solution of Bi(NO3)3·5H2O, pouring a Cu(NO3)2·5H2O aqueous solution therein while stirring, and then slowly adding a NaOH solution to obtain a white-green suspension and continuing to stir, and after the stirring is completed, performing a hydrothermal reaction, and after the reaction is completed, filtering, washing, drying, and grinding to obtain CuBi2O4 powder.

7. The use according to claim 6, characterized in that: The hydrothermal reaction was carried out at 180°C for 12 h.

8. The use according to claim 5 or 6, characterized in that: Drying was carried out at 60°C for 12 h.

9. The use according to claim 5, characterized in that: The mass of Ag2WO4 accounts for 10%-40% of the mass of the added CuBi2O4.

10. The use according to claim 8, characterized in that: The mass of Ag2WO4 accounts for 30% of the mass of the added CuBi2O4.

Citation Information

Patent Citations

  • Photocatalyst CuBi2O4 / Bi2WO6 nanospheres with visible-light response synthesized by one-pot process and application thereof

    CN108246306A

  • Copper tungstate / copper bismuthate composite photocatalyst and preparation method thereof

    CN112337476A

Cited By

  • Application of Bi2WO6 / CuBi2O4 composite material in ultrasonic catalytic degradation of antibiotics in wastewater

    CN121288830A