Preparation method of three-dimensional carbon-based composite material for oily wastewater treatment

By forming a layered double metal hydroxide and metal sulfide structure on a three-dimensional carbon-based material, combined with a peristaltic pump flow system, the problem of low separation efficiency of two-dimensional materials is solved, and efficient oil-water separation and catalytic degradation in oily wastewater are achieved. deal with.

CN118807787APending Publication Date: 2024-10-22ZHEJIANG SCI-TECH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410821194.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

When the existing technology treats oily wastewater, the small pore size and short permeability channels of the two-dimensional wetting separation material lead to low separation efficiency, and it is difficult to simultaneously treat insoluble oil pollution and soluble organic pollutants.

Method used

A three-dimensional carbon-based composite material modified with layered bimetallic hydroxide and metal sulfide is used to form a regular layered structure on the surface of the matrix material through hydrothermal reaction. It is combined with a peristaltic pump to build a flow system to achieve oil-water separation and catalytic degradation.

Benefits of technology

It achieves efficient removal of different types of organic pollutants and excellent separation performance of oil-water emulsions, with a separation efficiency of more than 98.0%, a catalytic degradation efficiency of more than 90%, and simultaneous treatment of oil droplets and water-soluble pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807787A_ABST
    Figure CN118807787A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a three-dimensional carbon-based composite material for oil-containing wastewater treatment, which comprises the following steps: firstly, immersing a proper base material into an aqueous solution containing divalent metal salt, trivalent metal salt and alkaline substances, and transferring the mixed solution into a reaction kettle for hydrothermal reaction; the three-dimensional carbon-based composite material loaded with the layered double hydroxides is obtained; immersing the obtained composite material into an aqueous solution containing metal molybdenum salt and a sulfur source, and transferring the mixed solution into a reaction kettle for hydrothermal reaction to obtain the three-dimensional carbon-based composite material. The prepared three-dimensional composite material has the advantages that a good synchronous removal effect on soluble organic pollutants and insoluble oil stains in the oily wastewater can be realized, and meanwhile, the material is in a three-dimensional state, has excellent mechanical properties and can be repeatedly recycled. The method is simple and easy to implement, high in controllability and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inorganic material preparation, and in particular to a method for preparing a three-dimensional carbon-based composite material co-modified by layered double metal hydroxides and metal sulfides for treating oily wastewater. Background Art

[0002] The treatment of oily wastewater has become a research hotspot in the field of environmental remediation. Among them, the permonosulfate (PMS) advanced oxidation technology with advantages such as fast reaction rate and strong oxidation ability is considered to be a promising treatment method for water-soluble organic pollutants in wastewater. In addition, in addition to water-soluble organic matter, oily wastewater usually contains a large amount of insoluble oil. For the separation of insoluble oil in water, superwetting membrane separation technology has been highly valued by many researchers due to its high separation ability, low energy demand, no indirect pollution and wide applicability. However, when treating oily wastewater, the small pore size and short permeation channel of two-dimensional wetting separation materials often cause the separation materials to be severely blocked, significantly affecting their separation efficiency. Therefore, many researchers have turned their attention to three-dimensional special wettability oil-water separation materials with larger pore size and longer permeation channel. Therefore, developing innovative strategies to combine wettability materials with PMS-based advanced oxidation technology to achieve efficient treatment of complex oily wastewater is of great significance in treating complex oily wastewater. The patent with application number CN202310741187.X discloses a method for modifying membrane materials with MXene / Bi2O3 heterojunction microspheres for oily wastewater treatment: Ti3AlC2 is etched and then dispersed to obtain a suspension, and PMMA is added to the suspension to obtain MXene microspheres through reaction, which are dispersed in a solvent system with bismuth salt, and MXene / Bi2O3 heterojunction microspheres are obtained through hydrothermal reaction, and the heterojunction microspheres and tannic acid are dispersed in a solvent to obtain a mixture, which is sprayed onto the membrane surface to obtain a membrane material, wherein the cross-linking and hydrogen bonding interaction between tannic acid and MXene ensures the physical stability and super-wetting properties of the functional layer, and the arrangement of the 3D MXene heterojunction effectively breaks through the limitation of separation flux compared with the traditional physically stacked 2D MXene dense membrane. The patent with application number CN201910849235.0 discloses a method for preparing a super-hydrophilic / underwater super-oleophobic modified substrate material: including preparing a certain concentration of styrene maleic anhydride copolymer solution and polyethyleneimine solution, immersing the substrate material in the styrene maleic anhydride copolymer solution for a certain time, taking it out and draining it, immersing it in the polyethyleneimine solution for a certain time, taking it out and draining it again, washing it with water to obtain a modified substrate material with super-hydrophilic / underwater super-oleophobic properties, which can be effectively used for oil-water mixture separation, and in particular, the modified polymer film has a very good emulsified oil separation effect. However, the above several oil-water separation materials are not significantly improved in the treatment of oily wastewater, and these materials are single for insoluble oil pollution in oily wastewater, and soluble organic pollutants in wastewater cannot be effectively treated. Therefore, it is necessary to develop new oil-water separation materials, while treating oil pollution in wastewater, catalytic degradation of soluble organic pollutants in water.

[0003] As a typical two-dimensional material, layered double hydroxides exhibit excellent chemical tolerance and high mechanical stability. The interchangeable metal composition on the layered double hydroxides makes them widely used as catalysts to activate PMS. Metal sulfides have been widely used as co-catalysts to accelerate redox reactions and improve catalytic efficiency due to their good electron transfer efficiency and friendly economic properties. Therefore, preparing a composite structure material co-modified with layered double hydroxides and metal sulfides by a simple method is an important path to achieve continuous activation of PMS and rapid degradation of organic pollutants. In addition, three-dimensional carbon-based materials usually have good chemical stability, suitable separation pore size, long permeation channels, and a π-electron conjugated system on the surface, which is conducive to electron transfer and can promote catalytic reactions. Therefore, three-dimensional carbon-based materials are used as substrates to load layered double hydroxides and metal sulfides to prepare three-dimensional carbon-based wettability composite materials. Their super hydrophilicity and abundant pores can be used for oil-water emulsion separation. At the same time, the composite structure of layered double hydroxides and metal sulfides gives the composite material excellent catalytic properties. Even in complex water environments, the composite material can play a good role in oil-water separation and degradation of harmful soluble organic matter. Summary of the invention

[0004] In view of the shortcomings of the existing oily wastewater treatment methods, the present invention provides a method for preparing a three-dimensional carbon-based composite material co-modified with layered double metal hydroxides and metal sulfides for oily wastewater treatment. The method is simple and easy to implement and suitable for industrial production; when the prepared composite material is used to treat oily wastewater, it has both oil-water separation and catalytic degradation functions, and the catalytic degradation speed in different oil-water emulsions is fast and the effect is good, and it can be reused.

[0005] A method for preparing a layered double metal hydroxide and metal sulfide co-modified three-dimensional carbon-based composite material for oily wastewater treatment, comprising the following steps:

[0006] (1) immersing a suitable matrix material in an aqueous solution containing a divalent metal salt, a trivalent metal salt, or an alkaline substance, and transferring the mixed solution into a reactor for hydrothermal reaction to obtain a three-dimensional carbon-based composite material loaded with a layered double metal hydroxide;

[0007] (2) immersing the composite material obtained in step (1) in an aqueous solution containing a metal salt and a sulfur source, and transferring the mixed solution into a reactor for a hydrothermal reaction to obtain a three-dimensional carbon-based composite material modified with the layered double metal hydroxide and disulfide.

[0008] Preferably, the matrix material in step (1) is one of carbonized melamine sponge, carbonized polyurethane sponge, or activated carbon fiber. More preferably, activated carbon fiber is selected as the base material.

[0009] Preferably, the divalent metal ion in the divalent metal salt in step (1) is Co 2+ , Cu 2+ , Fe 2+ 、Ni 2+ Mg 2+ One or two of the metal ions, more preferably, the divalent metal ion in the divalent metal salt is Co 2+ 、Ni 2+ One of the metal ions; the trivalent metal ion in the trivalent metal salt is A1 3+ , Fe 3+ and Cr 3+ One or two of the above, more preferably, the trivalent metal ion in the trivalent metal salt is A1 3+ , Fe 3+ One of the divalent metal salts; the anion of the trivalent metal salt is CO3 2- , Cl - 、NO3 - 、SO4 2- One or two of the above, more preferably, the anion of the divalent metal salt or trivalent metal salt is SO4 2- ; The alkaline substance is urea, ammonia water or sodium hydroxide, and urea is more preferably used.

[0010] Preferably, the total concentration of the divalent metal salt and the trivalent metal salt in step (1) is 0.01-0.2 mol / L; the molar ratio of the divalent metal salt to the trivalent metal salt in the mixed solution of the divalent metal salt and the trivalent metal salt is 0.5-4; the molar mass ratio of the total amount of the divalent metal salt and the trivalent metal salt to the alkaline substance is 1:1-10. More preferably, the total concentration of the divalent metal salt and the trivalent metal salt is 0.024-0.096 mol / L; the molar ratio of the divalent metal salt to the trivalent metal salt is 1-3; the molar mass ratio of the total amount of the divalent metal salt and the trivalent metal salt to the alkaline substance is 1:2-6.

[0011] Preferably, the metal salt in the metal salt described in step (2) is Mo 4+ , W 4+ One of the above, further preferably, the metal salt in the metal salt is Mo 4+ ; Preferably, the sulfur source is one of L-cysteine, thioacetamide and thiourea, and more preferably, the sulfur source is one of L-cysteine ​​and thioacetamide;

[0012] Preferably, the concentration of metal ions in the process of preparing the metal sulfide in step (2) is 0.01-0.2 mol / L; the molar ratio of metal ions in the mixed solution to sulfur in the sulfur source is 0.1-2. More preferably, the concentration of metal ions in the process of preparing the metal sulfide is 0.03-0.18 mol / L; the molar ratio of the metal salt to the total amount of the sulfur source is 0.1-1.

[0013] Preferably, the temperature of the hydrothermal reaction in step (1) is 100°C and the duration is 6 to 18 hours. Further preferably, the temperature of the hydrothermal reaction is 100°C and the duration is 8 to 16 hours. The preferred hydrothermal reaction conditions are conducive to the formation of regular and densely distributed layered double hydroxide microsheets on the surface of the three-dimensional matrix: the hydrothermal time needs to be controlled within an appropriate range. If the hydrothermal time is short, the layered double hydroxide sheets will not grow completely on the surface of the matrix. If the hydrothermal time is long, the layered double hydroxide will agglomerate severely and easily fall off the surface of the matrix.

[0014] Preferably, the temperature of the hydrothermal reaction in step (2) is 200° C., and the duration is 12 to 24 hours. More preferably, the temperature of the hydrothermal reaction is 200° C., and the duration is 14 to 22 hours.

[0015] The three-dimensional carbon-based composite material prepared by the present invention and modified by the layered double metal hydroxide and metal sulfide can effectively remove different types of organic pollutants (drugs, phenols or dyes) when used for catalytic degradation, and the removal rate of water-soluble organic pollutants is nearly 100% within a reaction time of 20 minutes. When used for oil-water separation, it has excellent separation performance for oil-water emulsions stabilized by various surfactants, with a separation efficiency of about 98.0% and a separation flux of 5.7×10 6 L m -2 h -1 bar -1 The above. The peristaltic pump is combined with the flow system to make the oil-water separation process and the catalytic degradation process proceed simultaneously. More than 95% of various oil-water emulsions can be efficiently intercepted within 20 minutes, and the degradation efficiency of organic pollutants can reach more than 90%, achieving the effect of simultaneous treatment of oil droplets and water-soluble pollutants in oily wastewater.

[0016] Compared with the prior art, the present invention has the following advantages:

[0017] 1. The present invention provides a mild growth environment that is conducive to the synthesis of regular and dense flaky layered double hydroxides and flower-like metal sulfides on the surface of the substrate, making full use of the catalytic function of the layered double hydroxides and the co-catalytic function of the metal sulfides, so that the prepared three-dimensional composite material has the ability to quickly catalytically degrade pollutants.

[0018] 2. The present invention utilizes the layered double metal hydroxide grown on the substrate surface to induce the metal sulfide to grow on the modified substrate surface, thereby overcoming the problem of uneven growth of the metal sulfide on the substrate surface.

[0019] 3. Optimize the three-dimensional material substrate, grow a layered double metal hydroxide and metal sulfide composite structure on its surface, give it surface wettability and micro-nano rough structure, overcome the high energy consumption and low efficiency defects in the traditional oily wastewater treatment process, and reduce the inherent oil droplet clogging and hydrophilic surface contamination problems in the oil-water separation process. In addition, combined with a peristaltic pump to build a flow reaction system, the three-dimensional material can achieve excellent simultaneous treatment effects on oil droplets and water-soluble pollutants in oily wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The XRD pattern of the activated carbon fiber modified with layered double hydroxide and metal sulfide prepared in Example 1;

[0021] Figure 2 The SEM images of the activated carbon fibers modified with layered double hydroxide and metal sulfide prepared in Example 1 at different magnifications are shown;

[0022] Figure 3 The three-dimensional carbon-based material prepared in Example 1 shows the degradation effect of atrazine, an organic pollutant in an oil-containing emulsion, in a flow system and a traditional intermittent mode;

[0023] Figure 4 The test photos of the contact angle of the three-dimensional carbon-based material prepared in Example 1 to water and the contact angle to oil under water;

[0024] Figure 5 These are SEM images of activated carbon fibers modified with metal sulfide and layered double hydroxide prepared in Comparative Example 1 at different magnifications. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0026] Embodiment 1:

[0027] Weigh 0.12 g of hydrated iron sulfate (Fe2(SO4)3·xH2O), 0.48 g of hydrated nickel nitrate (NiSO4·6H2O) and 1.30 g of urea and ultrasonically disperse them in 50 mL of deionized water. At the same time, cut the size of the sample into 2.5×2.5 cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0028] Weigh 0.97g of hydrated sodium molybdate (Na2MoO4·2H2O) and ultrasonically disperse it in 50mL of deionized water, then add 1.46g of L-cysteine ​​(C3H7NO2S) to the solution and continue stirring for 30min. Then add the completely dissolved above solution to the previously dried layered double hydroxide-modified activated carbon fiber sample, and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 18h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0029] The XRD spectra of the layered double metal hydroxide and metal sulfide modified activated carbon fiber material prepared in this example are as follows: Figure 1 As shown (including activated carbon fiber material AL modified with single layered double metal hydroxide, activated carbon fiber AM modified with single metal sulfide, activated carbon fiber sample ALM modified with layered double metal hydroxide and metal sulfide). It can be seen that the position of the product diffraction peak is consistent with the typical crystal phase of hydrotalcite and metal sulfide, indicating that layered double metal hydroxide and metal sulfide are synthesized on the surface of activated carbon fiber.

[0030] The SEM photos of the layered double hydroxide and metal sulfide co-modified activated carbon fiber material prepared in this example at different magnifications are shown in FIG. Figure 2 It can be seen that layered double hydroxides and flower-like metal sulfides grow uniformly and densely on the surface of activated carbon fibers.

[0031] The degradation effect of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example on the soluble pollutant atrazine in the oil-containing emulsion is as follows: Figure 3 As shown in Figure 2, 98.5% of the pollutants can be removed within 20 minutes of reaction time. It can be seen that the three-dimensional composite material has an excellent catalytic degradation effect on pollutants.

[0032] The contact angle of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example to water and the contact angle test photos to oil under water are shown in the figure. Figure 4 As shown, it can be seen that the three-dimensional carbon-based composite material has good hydrophilicity and underwater oleophobicity, and its separation efficiency for oil-water emulsion is 99.5%.

[0033] Embodiment 2:

[0034] Weigh 0.06g Fe2(SO4)3·xH2O, 0.24g NiSO4·6H2O and 0.65g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0035] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 1.46g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 18h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0036] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1 The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 Similarly, layered double hydroxides and metal sulfides grow uniformly and densely on the surface of activated carbon fibers. The activated carbon fiber material modified with layered double hydroxides and metal sulfides prepared in this embodiment has a removal rate of 84.3% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this embodiment are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 97.3%.

[0037] Embodiment 3:

[0038] Weigh 0.24g Fe2(SO4)3·xH2O, 0.96g NiSO4·6H2O and 2.6g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0039] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 1.46g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 18h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0040] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1 The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 Similarly, layered double hydroxides and metal sulfides grow uniformly and densely on the surface of activated carbon fibers. The activated carbon fiber material modified with layered double hydroxides and metal sulfides prepared in this embodiment has a removal rate of 94.5% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this embodiment are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 98.2%.

[0041] Embodiment 4:

[0042] Weigh 0.12g Fe2(SO4)3·xH2O, 0.48g NiSO4·6H2O and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0043] Weigh 0.48g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 0.73g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 18h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0044] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 The activated carbon fiber material modified by layered double metal hydroxide and metal sulfide prepared in this example has a removal rate of 82.5% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this example are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 97.8%.

[0045] Embodiment 5:

[0046] Weigh 0.12g Fe2(SO4)3·xH2O, 0.48g NiSO4·6H2O and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0047] Weigh 1.94g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 2.92g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide modified activated carbon fiber sample, transfer it to a 100mL polytetrafluoroethylene reactor, and hydrothermally heat it at 200℃ for 18h. After the reaction is completed, take out the sample and wash and dry it to obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0048] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1 The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 Similarly, layered double hydroxides and metal sulfides grow uniformly and densely on the surface of activated carbon fibers. The activated carbon fiber material modified with layered double hydroxides and metal sulfides prepared in this embodiment has a removal rate of 93.8% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this embodiment are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 98.1%.

[0049] Embodiment 6:

[0050] Weigh 0.12g Fe2(SO4)3·xH2O, 0.48g NiSO4·6H2O and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 8 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0051] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 1.46g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 18h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0052] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1 The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 The activated carbon fiber material modified by layered double hydroxide and metal sulfide prepared in this example has a removal rate of 79.5% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this example are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 96.5%.

[0053] Embodiment 7:

[0054] Weigh 0.12g Fe2(SO4)3·xH2O, 0.48g NiSO4·6H2O and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 16 hours. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0055] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 1.46g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 18h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0056] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1 The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 Similarly, layered double hydroxides and metal sulfides grow uniformly and densely on the surface of activated carbon fibers. The activated carbon fiber material modified with layered double hydroxides and metal sulfides prepared in this embodiment has a removal rate of 94.2% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this embodiment are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 98.6%.

[0057] Embodiment 8:

[0058] Weigh 0.12g Fe2(SO4)3·xH2O, 0.48g NiSO4·6H2O and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0059] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 1.46g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 14h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0060] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 The activated carbon fiber material modified by layered double hydroxide and metal sulfide prepared in this example has a removal rate of 81.9% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this example are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 95.8%.

[0061] Embodiment 9:

[0062] Weigh 0.12g Fe2(SO4)3·xH2O, 0.48g NiSO4·6H2O and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0063] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 1.46g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 22h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0064] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1 The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 Similarly, layered double hydroxides and metal sulfides grow uniformly and densely on the surface of activated carbon fibers. The activated carbon fiber material modified with layered double hydroxides and metal sulfides prepared in this embodiment has a removal rate of 93.7% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this embodiment are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 98.1%.

[0065] Embodiment 10:

[0066] Weigh 0.12g Fe2(SO4)3·xH2O, 0.48g NiSO4·6H2O and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0067] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 0.91g C2H5NS to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide modified activated carbon fiber sample, transfer it to a 100mL polytetrafluoroethylene reactor, and hydrothermal it at 200℃ for 18h. After the reaction is completed, take out the sample and wash and dry it to obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0068] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1 The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 Similarly, layered double hydroxides and metal sulfides grow uniformly and densely on the surface of activated carbon fibers. The activated carbon fiber material modified by layered double hydroxides and metal sulfides prepared in this embodiment has a removal rate of 92.8% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this embodiment are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 93.8%.

[0069] Embodiment 11:

[0070] Weigh 0.11g Al2(SO4)3, 0.48g NiSO4·6H2O and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0071] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 1.46g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 18h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0072] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1 The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 The activated carbon fiber material modified by layered double hydroxide and metal sulfide prepared in this example has a removal rate of 82.8% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this example are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 94.7%.

[0073] Embodiment 12:

[0074] Weigh 0.12g Fe2(SO4)3·xH2O, 0.28g CoSO4 and 1.3g urea and ultrasonically disperse them in 50mL deionized water. At the same time, cut the size of the sample into 2.5×2.5cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor for hydrothermal reaction at 100 ° C for 12 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a layered double metal hydroxide modified activated carbon fiber material.

[0075] Weigh 0.97g Na2MoO4·2H2O and ultrasonically disperse it in 50mL deionized water, then add 1.46g C3H7NO2S to the solution and continue stirring for 30min. Then add the completely dissolved solution to the previously dried layered double hydroxide-modified activated carbon fiber sample and transfer it to a 100mL polytetrafluoroethylene reactor, hydrothermally heat it at 200℃ for 18h, take out the sample after the reaction is completed, wash and dry it, and obtain an activated carbon fiber material modified with layered double hydroxide and metal sulfide.

[0076] The XRD spectrum of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example is similar to that of Figure 1The SEM images of the activated carbon fiber material modified with layered double hydroxide and metal sulfide prepared in this example are similar to Figure 2 The activated carbon fiber material modified by layered double hydroxide and metal sulfide prepared in this example has a removal rate of 88.9% for the pollutant atrazine within 20 minutes. The hydrophilicity and oleophobicity of the three-dimensional carbon-based composite material prepared in this example are similar to Figure 4 Similarly, its separation efficiency for oil-water emulsion is 96.1%.

[0077] Comparative Example 1:

[0078] Weigh 0.97 g Na2MoO4·2H2O and ultrasonically disperse it in 50 mL deionized water, then add 1.46 g C3H7NO2S to the solution and continue stirring for 30 min. At the same time, cut the size of the sample into 2.5×2.5 cm 2 The activated carbon fiber was immersed in the above solution and transferred to a 100 mL polytetrafluoroethylene reactor and hydroheated at 200 °C for 18 h. After the reaction was completed, the sample was taken out and washed and dried to obtain a metal sulfide-modified activated carbon fiber material.

[0079] Weigh 0.12g Fe2(SO4)3·xH2O, 0.48g NiSO4·6H2O and 1.30g urea and ultrasonically disperse them in 50mL deionized water. Then add the completely dissolved solution to the previously dried metal sulfide-modified activated carbon fiber sample, and move it to a 100mL polytetrafluoroethylene reactor for hydrothermal reaction at 100℃ for 12h. After the reaction is completed, take out the sample and wash and dry it to obtain an activated carbon fiber material modified with metal sulfide and layered double metal hydroxide.

[0080] The SEM photos of the activated carbon fiber materials modified with metal sulfide and layered double metal hydroxide prepared in this comparative example are shown in FIG. Figure 5 , MoS2 nanosheets are sparsely accumulated on the surface of the matrix, and there is agglomeration phenomenon, and the layered double hydroxides grown on the surface are sparsely distributed in rod-like and a small amount of flake-like morphology, which indicates that the metal sulfides grown on the surface of the matrix cannot better induce the layered double hydroxides to grow on the fiber surface, which is not conducive to the successful preparation of three-dimensional composite materials with stable surfaces.

Claims

1. A method for preparing a three-dimensional carbon-based composite material for oily wastewater treatment, characterized in that: The steps include: (1) immersing a substrate material in an aqueous solution containing a divalent metal salt, a trivalent metal salt, or an alkaline substance, and transferring the mixed solution into a reactor for hydrothermal reaction to obtain a three-dimensional carbon-based composite material loaded with a layered double metal hydroxide; the substrate material is one of carbonized melamine sponge, carbonized polyurethane sponge, or activated carbon fiber; (2) immersing the composite material obtained in step (1) in an aqueous solution containing a metal salt and a sulfur source, and transferring the mixed solution into a reactor for a hydrothermal reaction to obtain a three-dimensional carbon-based composite material modified with the layered double metal hydroxide and the metal sulfide.

2. The method for preparing a three-dimensional carbon-based composite material for oily wastewater treatment according to claim 1, characterized in that: In step (1), the mixed solution is transferred into a reaction vessel for hydrothermal reaction at a temperature of 100° C. for a time of 6 to 18 hours.

3. The method for preparing a three-dimensional carbon-based composite material for oily wastewater treatment according to claim 1, characterized in that: The divalent metal ion in the divalent metal salt described in step (1) is Co 2+ , Cu 2+ , Fe 2+ 、Ni 2+ , or Mg 2+ One or two of the metal ions; the trivalent metal ion in the trivalent metal salt is A1 3+ , Fe 3+ , or Cr 3+ One or two of the following; the anions of the divalent metal salt and the trivalent metal salt are CO3 2- , Cl - 、NO3 - , or SO4 2- One or two of the following: the alkaline substance is urea, ammonia water, or sodium hydroxide.

4. The method for preparing a three-dimensional carbon-based composite material for oily wastewater treatment according to claim 3, characterized in that: The total concentration of the divalent metal salt and the trivalent metal salt is 0.01-0.2 mol / L; in the mixed solution of the divalent metal salt and the trivalent metal salt, the molar ratio of the divalent metal salt to the trivalent metal salt is 0.5-4; the molar mass ratio of the total amount of the divalent metal salt and the trivalent metal salt to the alkaline substance is 1:1-10.

5. The method for preparing a three-dimensional carbon-based composite material for oily wastewater treatment according to claim 1, characterized in that: In step (2), the mixed solution is transferred into a reaction vessel for hydrothermal reaction at a temperature of 200° C. for a time of 12 to 24 hours.

6. The method for preparing a three-dimensional carbon-based composite material for oily wastewater treatment according to claim 1, characterized in that: The sulfur source in step (2) is one of L-cysteine, thioacetamide, or thiourea; the metal ion in the metal salt is W 4+ , or Mo 4+ One of them.

7. The method for preparing a three-dimensional carbon-based composite material for oily wastewater treatment according to claim 1, characterized in that: In step (2), the molar ratio of the metal ions in the mixed solution to the sulfur element in the sulfur source is 0.1-2; and the concentration of the metal ions in the mixed solution is 0.01-0.2 mol / L.

Citation Information

Patent Citations

  • Method for preparing superhydrophilic / subaqueous superoleophobic modified substrate material

    CN110512423A

  • MXene / Bi2O3 heterojunction microsphere, membrane material containing MXene / Bi2O3 heterojunction microsphere and application of membrane material in oily wastewater

    CN116966846A

  • Compound photocatalyst and preparing method and application thereof

    CN105642364A

  • Preparation method of three-dimensional composite material for oily wastewater treatment

    CN114130417A