Application of alpha brominated fatty acid as collecting agent in flotation separation of lithium chlorite
By using α-bromo fatty acids as collectors in flotation separation, the problem of difficulty in separating lithium chlorite from monohydrate and kaolinite is solved, efficient enrichment of lithium chlorite is achieved, and the collection efficiency is improved. The selectivity and low-temperature performance of the collector are suitable for the development and utilization of clay-type lithium ores.
Patent Information
- Application Number
- CN202411128338.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-22
AI Technical Summary
There is a lack of effective collectors in the existing technology for the flotation separation of lithium chlorite from monohydrate and kaolinite, resulting in low lithium chlorite enrichment efficiency, and commonly used collectors are harmful to lithium chlorite. Its selectivity and low-temperature solubility are poor, which affects the development and utilization of clay-type lithium ores.
Alpha brominated fatty acids are used as collectors, and bromine groups are introduced at the alpha position to enhance the reactivity and steric hindrance of the active sites. Combined with appropriate pH adjustment and stirring conditions, the combination of lithium chlorite and monohydrate, Efficient separation of kaolinite.
It achieves excellent enrichment effect of lithium chlorite, improves the selectivity and low-temperature solubility of the collector, has the advantages of wide range of raw materials, simple synthesis, easy use, and low temperature resistance, and can effectively separate lithium chlorite and monohydrate. Aluminite, kaolinite.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mineral flotation separation, in particular to the application of alpha-brominated fatty acid as a collector in the flotation separation of hectorite. Background Art
[0002] Lithium is an important energy metal and is widely used in high-end fields such as high-energy batteries, aerospace, and nuclear fusion power generation due to its super strong electrochemical activity and ultra-light properties. Lithium resources in nature can generally be divided into three categories: brine type, pegmatite type, and clay type. Among them, brine type and pegmatite type are the main lithium resources currently being developed and utilized. With the high demand for lithium and the discovery of a large number of clay-type lithium mines in recent years, the development and utilization of clay-type lithium mines have received attention. However, clay-type lithium mines generally have the problem of low lithium content. Direct treatment by hydrometallurgy requires a large amount of roasting aids or leaching agents. In addition, roasting aids or leaching agents are usually strong acids and strong alkalis. Large-scale use will cause corrosion to equipment, and leaching residues will also harm the environment. Therefore, it is of great significance to pre-enrich the lithium-containing minerals in clay-type lithium mines by flotation to reduce the amount of ore to be processed in subsequent hydrometallurgy.
[0003] The main lithium-rich mineral in clay-type lithium ore is lithium chlorite, and its associated gangue minerals are mainly kaolinite and gibbsite. Therefore, the flotation separation of lithium chlorite from kaolinite and gibbsite is the basis for the enrichment of clay-type lithium ore. However, there are very few collectors for the flotation separation of lithium chlorite from gibbsite and kaolinite, and the existing reagents have poor selectivity and low-temperature solubility. Therefore, the development of efficient flotation collectors for lithium chlorite and the efficient separation of lithium chlorite from gibbsite and kaolinite are of great significance to the development and utilization of clay-type lithium ore. Summary of the invention
[0004] The purpose of the present invention is to provide an application of α-brominated fatty acid as a collector in the flotation separation of hectorite, so as to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is the use of α-brominated fatty acid as a collector in the flotation separation of lithium chlorite, wherein the chemical formula of the α-brominated fatty acid is BrC n H 2n-1 O 2 , where n=12-16.
[0007] Furthermore, the flotation separation is specifically the flotation separation of lithium chlorite from clay-type lithium ore.
[0008] Furthermore, the clay-type lithium ore is a chlorite-type clay-type lithium ore.
[0009] Furthermore, the mineral components of the clay-type lithium ore include lithium chlorite, kaolinite and gibbsite.
[0010] That is, the essence of technical solution 1 is to provide the application of α-bromo fatty acid as a collector for flotation separation of hectorite from hectorite, kaolinite and gibbsite.
[0011] Furthermore, the α-brominated fatty acid is a straight chain structure or a branched chain structure, and bromine (Br) is connected to the α-carbon of the fatty acid.
[0012] The second technical solution of the present invention is a method for flotation separation of lithium chlorite using an α-bromo fatty acid collector, comprising the following steps: mixing the α-bromo fatty acid collector with water to obtain a collector solution; crushing and ball-milling the mineral and mixing it with water to obtain a pulp; adjusting the pH of the pulp to 9-11, then adding a calcium chloride solution, adding the collector solution after acting for 2-3 minutes, and flotation scraping after acting for 2-3 minutes; the chemical formula of the α-bromo fatty acid is BrC n H 2n-1 O 2 , where n=12-16.
[0013] Furthermore, the mineral is a clay-type lithium ore; the components of the mineral include lithium chlorite, kaolinite and gibbsite.
[0014] Furthermore, the mass percentage concentration of the collector solution is 0.5-2%.
[0015] Furthermore, the α-bromo fatty acid collector is mixed with water and stirred at a speed of 1000-1200 r / min for 5-10 min to obtain the collector solution.
[0016] Furthermore, the crushing is specifically to crush the mineral to a particle size of less than 2 mm to obtain a crushed mineral.
[0017] Furthermore, the ball milling is specifically to ball mill the crushed mineral until the component with a mass particle size of less than 0.038 mm accounts for 80-90%.
[0018] Furthermore, the mass percentage concentration of the slurry is 3-20%.
[0019] Furthermore, the specific operation of adjusting the pH value of the ore pulp to 9-11 is: adding a NaOH solution with a mass percentage concentration of 0.5-3% to the ore pulp to adjust the pH value of the ore pulp to 9-11, and the slurry adjustment time is 2-3 minutes.
[0020] Furthermore, the mass percentage concentration of the calcium chloride solution is 0.5-1%; the amount of the calcium chloride solution added is 0.02-0.8% of the volume of the slurry.
[0021] Furthermore, the amount of the collector solution added is 0.2-3% of the volume of the slurry.
[0022] Furthermore, the flotation scraping time is 3-5 minutes.
[0023] Lithium chlorite is a clay-type lithium ore with extremely fine crystal size. Unlike other lithium ores, it usually requires fine grinding to dissociate. Clay minerals are prone to swelling and cracking in water, making separation difficult. In addition, its gangue usually contains iron and magnesium impurities with similar properties to the active sites of lithium chlorite, which also increases the difficulty of separation. Therefore, collectors suitable for other common lithium ores such as hard rock lithium-containing minerals are often not suitable for lithium chlorite. The present invention aims at the technical gap of flotation separation of clay-type lithium ore and flotation separation of lithium chlorite and gibbsite and kaolinite, and provides the application of alpha-bromo fatty acid as a collector in flotation separation of lithium chlorite. The carbon number of the alpha-bromo fatty acid collector is 12-16. The collector can produce strong reaction activity with the active sites on the surface of lithium chlorite by introducing a strong electron-withdrawing group Br at the α position, but cannot produce strong effect with gibbsite and kaolinite. At the same time, the larger radius of Br is used to produce a steric effect, thereby enhancing the selectivity of the collector to lithium chlorite. At the same time, the introduction of Br can effectively enhance the low-temperature solubility of the collector. The collector has a wide source of raw materials, a simple synthesis process, is easy to use, has strong capture capacity and selectivity, and has good low-temperature resistance.
[0024] The present invention discloses the following technical effects:
[0025] The present invention uses alpha-brominated fatty acid as a collector for flotation separation of hectorite, which can realize effective separation of hectorite from gibbsite and kaolinite, and achieve excellent hectorite enrichment effect.
[0026] The alpha-bromo fatty acid collector used in the present invention has the advantages of wide raw material source, simple synthesis, convenient use, good low temperature resistance, etc., and strong selectivity for lithium chlorite. DETAILED DESCRIPTION
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0028] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0032] The "room temperature" referred to in the following examples and comparative examples specifically refers to 20-25°C.
[0033] The specific information of the brominated fatty acids (including α-brominated fatty acids and non-α-brominated fatty acids) used in the following examples and comparative examples is shown in Table 1:
[0034] Table 1
[0035] Chemical formula Structural formula CAS number or manufacturer <![CDATA[α-bromo fatty acid BrC 12 H 23 O 2 > <![CDATA[CH 3 (CH 2 ) 9 CHBrCOOH]]> 111-56-8 <![CDATA[α-bromo fatty acid BrC 14 H 27 O 2 > <![CDATA[CH 3 (CH 2 ) 11 CHBrCOOH]]> 10520-81-7 <![CDATA[α-bromo fatty acid BrC 16 H 31 O 2 > <![CDATA[CH 3 (CH 2 ) 13 CHBrCOOH]]> 18263-25-7
[0036] In the following examples and comparative examples, mineral recovery rate = mass of foam product / mass of total minerals × 100%;
[0037] The floatation difference is the difference in the recovery rates of different mineral components.
[0038] Example 1
[0039] (1) Preparation of α-bromo fatty acid collector solution:
[0040] The chemical formula of the α-bromo fatty acid collector used in this example is BrC 12H 23 O 2 (The structural formula is shown in Table 1), that is, n=12. The α-bromo fatty acid collector was mixed with water at a mass ratio of 0.5:100 at room temperature, and stirred at a speed of 1000 r / min for 5 minutes to obtain a collector solution with a mass percentage concentration of 0.5%.
[0041] (2) Flotation separation of minerals
[0042] 1) A disc crusher is used to crush the mineral (pure mineral lithium chlorite, pure mineral diaspore or pure mineral kaolinite) to a particle size of less than 2 mm, and then a ceramic ball mill is used to ball-mill the crushed mineral until the component with a mass particle size of less than 0.038 mm accounts for 90%.
[0043] 2) Mix the ball-milled mineral (pure mineral lithium chlorite, pure mineral gibbsite or pure mineral kaolinite) with water at room temperature to prepare 60 mL of 3% mass percent slurry, then add 0.5% mass percent NaOH solution to the slurry to adjust the pH of the slurry to 11, the slurry adjustment time is 3 minutes, then add 0.3 mL of 1% mass percent calcium chloride solution to the slurry, act for 3 minutes, then add 1.6 mL of the above collector solution, act for 3 minutes, and then flotation and scraping for 3 minutes to obtain the product in the flotation tank and the foam product. After drying the foam product, calculate the recovery rate of each mineral and the floating difference between different mineral components. The floating difference (difference in recovery rate) of lithium chlorite (recovery rate is 98%), gibbsite (recovery rate is 5%), and kaolinite (recovery rate is 23%) is 93% and 75%, respectively. The efficient separation of lithium chlorite from gibbsite and kaolinite can be achieved.
[0044] Example 2
[0045] (1) Preparation of α-bromo fatty acid collector solution:
[0046] The chemical formula of the α-bromo fatty acid collector used in this example is BrC 14 H 27 O 2 (The structural formula is shown in Table 1), that is, n=14. The α-bromo fatty acid collector was mixed with water at a mass ratio of 0.5:100 at room temperature, and stirred at a speed of 1000 r / min for 10 minutes to obtain a collector solution with a mass percentage concentration of 0.5%.
[0047] (2) Flotation separation of minerals
[0048] 1) A disc crusher is used to crush the mineral (pure mineral lithium chlorite, pure mineral diaspore or pure mineral kaolinite) to a particle size of less than 2 mm, and then a ceramic ball mill is used to ball-mill the crushed mineral until the component with a mass particle size of less than 0.038 mm accounts for 90%.
[0049] 2) Mix the ball-milled mineral (pure mineral lithium chlorite, pure mineral gibbsite or pure mineral kaolinite) with water at room temperature to prepare 60 mL of 5% mass percent slurry, then add 0.5% mass percent NaOH solution to the slurry to adjust the pH of the slurry to 11, the slurry adjustment time is 5 minutes, then add 0.48 mL of 0.5% mass percent calcium chloride solution to the slurry for 3 minutes, then add 0.7 mL of the above collector solution, after 5 minutes of action, flotation and scraping for 3 minutes to obtain the product in the flotation tank and the foam product. After drying the foam product, calculate the recovery rate of each mineral and the floating difference between different mineral components. The floating differences of lithium chlorite (recovery rate is 96%), gibbsite (recovery rate is 1%) and kaolinite (recovery rate is 24%) are 95% and 72%, respectively. The efficient separation of lithium chlorite from gibbsite and kaolinite can be achieved.
[0050] Example 3
[0051] The same as Example 1, the only difference is that the flotation temperature is 15° C. In this example, the floating differences of hectorite (recovery rate is 94%), gibbsite (recovery rate is 4%), and kaolinite (recovery rate is 22%) are 90% and 72%, respectively, and efficient separation can still be achieved.
[0052] Comparative Example 1
[0053] The same as Example 1, except that the collector used in step (1) is replaced by dodecylamine, a collector commonly used for hard rock type lithium-containing mineral lepidolite. In this comparative example, the floating differences of lithium chlorite (recovery rate 39%), gibbsite (recovery rate 36%), and kaolinite (recovery rate 64%) are reduced to 3% and 25%, respectively, and separation cannot be achieved.
[0054] Comparative Example 2
[0055] The same as Example 1, except that the collector used in step (1) is replaced with sodium oleate, a fatty acid collector commonly used in hard rock type lithium-containing mineral spodumene. In this comparative example, the floating differences of spodumene chlorite (recovery rate 25%), gibbsite (recovery rate 87%), and kaolinite (recovery rate 65%) are reduced to 62% and 40%, respectively, and efficient separation cannot be achieved.
[0056] Comparative Example 3
[0057] The same as Example 1, except that the flotation pH in step (2) is changed to 7 (i.e., the pH of the pulp is adjusted to 7 before adding the calcium chloride solution and the collector solution). In this comparative example, the floating differences of hectorite (recovery rate is 96%), gibbsite (recovery rate is 65%), and kaolinite (recovery rate is 83%) are reduced to 31% and 13%, respectively, and efficient separation cannot be achieved.
[0058] Comparative Example 4
[0059] The same as Example 1, except that the addition of calcium chloride solution is omitted in step (2). In this comparative example, the floating differences of lithium chlorite (recovery rate is 63%), gibbsite (recovery rate is 33%), and kaolinite (recovery rate is 1%) are reduced to 30% and 62%, respectively, and efficient separation cannot be achieved.
[0060] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. The use of α-brominated fatty acid as a collector in the flotation separation of lithium chlorite, characterized in that: The chemical formula of the α-bromo fatty acid is BrC n H 2n-1 O2, where n = 12-16.
2. The use according to claim 1, characterized in that The flotation separation of lithium chlorite specifically involves the flotation separation of lithium chlorite from clay-type lithium ore.
3. A method for flotation separation of lithium chlorite using α-bromo fatty acid collector, characterized in that: The following steps are involved: The α-bromo fatty acid collector is mixed with water to obtain a collector solution; the mineral is crushed, ball-milled and mixed with water to obtain a pulp; the pH of the pulp is adjusted to 9-11, and then a calcium chloride solution is added, and after the calcium chloride solution is added, the collector solution is added, and after the calcium chloride solution is added, the flotation is performed after the calcium chloride solution is added for 2-3 minutes; the chemical formula of the α-bromo fatty acid is BrC n H 2n-1 O2, where n = 12-16.
4. The method according to claim 3, characterized in that The mineral is a clay-type lithium ore; the components of the mineral include lithium chlorite, kaolinite and diaspore.
5. The method according to claim 3, characterized in that The mass percentage concentration of the collector solution is 0.5-2%.
6. The method according to claim 3, characterized in that The crushing specifically includes crushing the mineral to a particle size of less than 2 mm to obtain a crushed mineral.
7. The method according to claim 6, characterized in that The ball milling is specifically to ball mill the crushed mineral until the component with a mass particle size of less than 0.038 mm accounts for 80-90%.
8. The method according to claim 3, characterized in that The mass percentage concentration of the ore pulp is 3-20%.
9. The method according to claim 3, characterized in that The mass percentage concentration of the calcium chloride solution is 0.5-1%; the added amount of the calcium chloride solution is 0.02-0.8% of the volume of the ore pulp.
10. The method according to claim 3, characterized in that The amount of the collector solution added is 0.2-3% of the volume of the ore pulp.
Citation Information
Cited By
Method for floating fluorite, oxidized ores
CN122999389A