Production system and method of high-strength single-zero aluminum foil

By analyzing the voltage fluctuation of the tension and straightening cleaning instrument and the deviation of the reflected light intensity on the surface of the aluminum foil, the relationship between the quality of the aluminum foil and the instrument is evaluated, which solves the problem of inaccurate aluminum foil quality assessment in the existing technology and achieves efficient cleaning and quality control of the aluminum foil.

CN118808323AInactive Publication Date: 2024-10-22JIANGSU ZHONGJI LAMINATION MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411082998.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, there is a lack of scientific and quantitative methods for quality assessment of aluminum foil blanks after straightening and cleaning, resulting in inaccurate assessment results and difficulty in quickly locating the correlation between production equipment and product quality.

Method used

By obtaining the real-time voltage fluctuation curve of the tension and straightening cleaning instrument and the deviation value of the reflected light intensity on the blank surface, the analysis parameters are calculated, and the threshold is preset for comparative analysis, to evaluate the relationship between the blank quality and the instrument, and to determine the relationship between quality abnormalities and voltage fluctuations.

Benefits of technology

Achieved quantitative assessment of the quality of aluminum foil after straightening and cleaning, timely discovered problems during the cleaning process, optimized the process, and ensured product quality and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808323A_ABST
    Figure CN118808323A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum foil production, and particularly discloses a high-strength single-zero aluminum foil production system and method.The method comprises the steps that withdrawal, straightening and cleaning detection is conducted on a blank subjected to withdrawal, straightening and cleaning, so that whether the blank subjected to withdrawal, straightening and cleaning is qualified or not is evaluated; analyzing the relationship between the quality of the blank subjected to withdrawal and straightening cleaning and a withdrawal and straightening cleaning instrument; according to the method, by detecting the pulling, straightening and cleaning steps, it is guaranteed that the aluminum coil is subjected to effective pulling, straightening and cleaning, it is guaranteed that the aluminum coil has good surface quality and performance in the subsequent machining and using process, and the problems existing in the cleaning process can be found in time through detection; by calculating and analyzing parameters, the relation between the quality of the blank subjected to withdrawal and straightening cleaning and the voltage fluctuation of the withdrawal and straightening cleaning instrument is evaluated in a quantitative mode, so that a basis is provided for subsequent problem positioning, direction optimization and quality control, and by analyzing the change of the parameters, which link of the withdrawal and straightening cleaning instrument the problem occurs in is judged preliminarily.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum foil production, and in particular to a production system and method for high-strength single-zero aluminum foil. Background Art

[0002] Aluminum foil is a hot stamping material that is directly rolled into a thin sheet with metal aluminum. Its hot stamping effect is similar to that of pure silver foil, so it is also called fake silver foil. Due to the soft texture and good ductility of aluminum, it has a silvery-white luster. If the rolled thin sheet is mounted on offset paper with sodium silicate and other materials to make aluminum foil, it can also be printed. However, aluminum foil itself is easily oxidized and the color becomes darker. It will fade due to friction and touch. Therefore, it is not suitable for hot stamping of book covers that are to be preserved for a long time.

[0003] The Chinese invention patent with publication number CN112899529A discloses a method for manufacturing high-strength aluminum foil for a fresh air system, and its process flow includes melting, casting and rolling, rough rolling, intermediate annealing, rough rolling and trimming, finishing rolling, finished product annealing, straightening and cleaning, slitting, inspection and packaging.

[0004] However, in the prior art, there is often a lack of scientific and quantitative methods for evaluating the quality of blanks after straightening and cleaning. Traditional evaluation methods may rely too much on manual experience or simple visual inspection. This evaluation method is not only highly subjective, but also easily affected by human factors, resulting in inaccurate evaluation results. In addition, in the prior art, the analysis of the correlation between production equipment and product quality is often not in-depth enough. When there is a problem with product quality, companies often find it difficult to quickly locate the source of the problem and are unable to determine whether it is caused by equipment failure, improper operation or other reasons. Summary of the invention

[0005] The object of the present invention is to provide a production system and method of high-strength single-zero aluminum foil to solve the technical problems in the above background.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] In a first aspect, the present invention provides a production system and method for high-strength single-zero aluminum foil, comprising:

[0008] Melting, casting and rolling, first rough rolling, intermediate annealing, second rough rolling, trimming, finishing rolling, finished product annealing, straightening and cleaning, slitting, inspection and packaging;

[0009] Conducting a straightening and cleaning test on the billet after straightening and cleaning, so as to evaluate whether the billet after straightening and cleaning is qualified;

[0010] Analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument. The specific method is:

[0011] Obtain the abnormal fluctuation time period, and according to the abnormal fluctuation time period and the reflected light intensity deviation value Qi of the blank surface sub-area after straightening and cleaning, obtain the analysis parameter, preset the analysis parameter threshold, compare and analyze the analysis parameter with the analysis parameter threshold, and analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument;

[0012] If the analysis parameter is less than the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning has nothing to do with the voltage fluctuation of the straightening and cleaning instrument;

[0013] If the analysis parameter is ≥ the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning is related to the voltage fluctuation of the straightening and cleaning instrument.

[0014] As a further solution of the present invention: the method for obtaining the abnormal fluctuation time period is:

[0015] B1: During the straightening and cleaning process, the straightening and cleaning instrument is tested in real time to obtain the real-time voltage of the straightening and cleaning instrument;

[0016] B2: Based on a two-dimensional coordinate system with time as the X-axis and the voltage of the straightening and cleaning instrument as the Y-axis, a voltage fluctuation curve is obtained according to the real-time voltage of the straightening and cleaning instrument, and a preset range area with a Y-axis value of a preset voltage range and parallel to the X-axis is drawn;

[0017] B3: Obtain abnormal voltage fluctuations according to the voltage fluctuation curve and the preset range area, and record the time of each abnormal voltage fluctuation. The time period of the abnormal voltage fluctuation is the abnormal fluctuation time period.

[0018] As a further solution of the present invention: the method for obtaining abnormal voltage fluctuations is: calculate the area enclosed by the part of the voltage fluctuation curve that exceeds the preset range area and the preset range area, obtain the fluctuation pre-abnormal area, and preset the fluctuation pre-abnormal area threshold, compare and analyze the fluctuation pre-abnormal area with the fluctuation pre-abnormal area threshold, if the fluctuation pre-abnormal area ≥ the fluctuation pre-abnormal area threshold, then mark the part of the voltage fluctuation curve that exceeds the preset range area as abnormal voltage fluctuation.

[0019] As a further solution of the present invention: the method for obtaining the analysis parameters is:

[0020] According to the reflected light intensity deviation value Qi of the sub-area on the surface of the blank after straightening and cleaning, the abnormal time period of straightening and cleaning is obtained, the abnormal time period of straightening and cleaning is compared and analyzed with the abnormal fluctuation time period, and the time overlap between the abnormal time period of straightening and cleaning and the abnormal fluctuation time period is calculated. The ratio of the time overlap to the time overlap threshold is the analysis parameter.

[0021] As a further solution of the present invention: the method for obtaining the abnormal time period of straightening and cleaning is as follows: presetting the reflected light intensity deviation value threshold of the billet surface sub-area after straightening and cleaning as QR, comparing and analyzing the reflected light intensity deviation value Qi of the billet surface sub-area after straightening and cleaning with the reflected light intensity deviation value threshold QR of the billet surface sub-area after straightening and cleaning, marking the billet surface sub-area after straightening and cleaning whose reflected light intensity deviation value Qi of all sub-areas on the billet surface after straightening and cleaning is greater than or equal to the reflected light intensity deviation value threshold QR of the billet surface sub-area after straightening and cleaning as abnormal straightening and cleaning sub-area, and recording the time period when the abnormal straightening and cleaning sub-area is subjected to straightening and cleaning treatment, so as to obtain the abnormal straightening and cleaning time period.

[0022] As a further solution of the present invention: the specific method for evaluating whether the blank after straightening and cleaning is qualified is:

[0023] The billet after straightening and cleaning is tested to obtain test data, and test parameters are calculated based on the test data, so as to evaluate the billet after straightening and cleaning based on the test parameters to determine whether the billet after straightening and cleaning is qualified;

[0024] Among them, the detection data includes: tension, straightening and cleaning characterization value and uniformity characterization value.

[0025] As a further solution of the present invention: the method for acquiring the detection data is:

[0026] A1: Divide the surface of the billet after straightening and cleaning into multiple sub-areas evenly;

[0027] A2: A light source of fixed intensity is emitted to the surface of the billet after straightening and cleaning, and the intensity of the reflected light from the surface of the billet after straightening and cleaning is received to obtain the reflected light intensity of each sub-area of ​​the billet surface after straightening and cleaning, and the reflected light intensity of the sub-area of ​​the billet surface after straightening and cleaning is calculated to be different from the reflected light intensity of the preset sub-area, and the absolute value is taken to obtain the reflected light intensity deviation value of the sub-area of ​​the billet surface after straightening and cleaning, and the reflected light intensity deviation value of the sub-area of ​​the billet surface after straightening and cleaning is marked as Qi, where i represents different sub-areas of the billet surface after straightening and cleaning, and i is a positive integer;

[0028] A3: Calculate the mean of the reflected light intensity deviation values ​​Qi of all sub-regions on the surface of the blank after straightening and cleaning to obtain the mean of the reflected light intensity deviation of the sub-regions, calculate the ratio of the mean of the reflected light intensity deviation of the sub-regions to the mean threshold of the reflected light intensity deviation of the sub-regions, and obtain the straightening and cleaning characterization value, which is marked as LQ;

[0029] A4: Calculate the standard deviation based on the reflected light intensity deviation value Qi of all sub-areas on the surface of the blank after straightening and cleaning and the mean value of the reflected light intensity deviation of the sub-areas to obtain the standard deviation of the reflected light intensity deviation of the sub-areas, calculate the ratio of the standard deviation of the reflected light intensity deviation of the sub-areas to the standard deviation threshold of the reflected light intensity deviation of the sub-areas, that is, obtain the uniform characterization value, and mark the uniform characterization value as JY.

[0030] As a further solution of the present invention: the method further comprises:

[0031] The tension and cleaning characterization value LQ and the uniform characterization value JY are processed;

[0032] By formula: The detection parameter JC is obtained by calculation, wherein a1 and a2 are preset proportional factors and are both greater than 0.

[0033] As a further solution of the present invention: the method further comprises:

[0034] The detection parameter threshold is preset as JR, and the detection parameter JC is compared and analyzed with the detection parameter threshold JR;

[0035] If the detection parameter JC is less than the detection parameter threshold JR, the blank after straightening and cleaning is judged to be qualified;

[0036] If the detection parameter JC ≥ the detection parameter threshold JR, the blank after straightening and cleaning is judged to be unqualified.

[0037] In a second aspect, the present invention provides a production system for high-strength single-zero aluminum foil, which implements a method as described in any one of the above methods, including:

[0038] A qualified assessment module, wherein the qualified assessment module is used to perform a straightening and cleaning test on the straightening and cleaning blank, so as to assess whether the straightening and cleaning blank is qualified;

[0039] A relationship analysis module is used to analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument. The specific method is as follows:

[0040] Obtain the abnormal fluctuation time period, and according to the abnormal fluctuation time period and the reflected light intensity deviation value Qi of the blank surface sub-area after straightening and cleaning, obtain the analysis parameter, preset the analysis parameter threshold, compare and analyze the analysis parameter with the analysis parameter threshold, and analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument;

[0041] If the analysis parameter is less than the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning has nothing to do with the voltage fluctuation of the straightening and cleaning instrument;

[0042] If the analysis parameter is ≥ the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning is related to the voltage fluctuation of the straightening and cleaning instrument.

[0043] Beneficial effects of the present invention:

[0044] (1) The present invention ensures that the aluminum coil is effectively straightened and cleaned by detecting the straightening and cleaning steps, and ensures that it has good surface quality and performance during subsequent processing and use. Through detection, problems in the cleaning process, such as incomplete cleaning and residual cleaning agent, can be discovered in time, so as to adjust the cleaning process in time and ensure product quality.

[0045] (2) The present invention evaluates the relationship between the quality of the blank after straightening and cleaning and the voltage fluctuation of the straightening and cleaning instrument in a quantitative manner by calculating and analyzing parameters, thereby providing a basis for subsequent problem location, optimization direction and quality control. By analyzing the changes in parameters, it is helpful to preliminarily determine which link of the straightening and cleaning instrument the problem occurs in, such as whether the voltage fluctuation is caused by unstable voltage supply, aging of instrument components or other factors. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The present invention will be further described below in conjunction with the accompanying drawings.

[0047] Figure 1 is a flow chart of the method of the present invention;

[0048] Figure 2 It is a flow chart of the method for evaluating whether the blank after drawing, straightening and cleaning is qualified in the present invention;

[0049] Figure 3 It is a flow chart of the method for analyzing the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument in the present invention;

[0050] Figure 4 It is a schematic diagram of the system of the present invention. DETAILED DESCRIPTION

[0051] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] Embodiment 1:

[0053] See also Figure 1 , Figure 2 As shown, a method for producing a high-strength single-zero aluminum foil according to an embodiment of the present invention comprises:

[0054] Melting and casting: DS309 alloy is melted and cast-rolled into cast-rolled aluminum coils; the temperature is controlled for melting, and after melt refining, it is poured into a static furnace for static insulation;

[0055] First rough rolling: rough rolling the billet;

[0056] Intermediate annealing: The rough rolled billet is subjected to two temperature-raising annealing treatments;

[0057] Second rough rolling and trimming: The annealed billet is rough rolled again and trimmed after cooling;

[0058] Finish rolling: Finish rolling is performed on semi-finished products to achieve the thickness required for finished products and control the processing rate;

[0059] Finished product annealing: The finished product annealing is carried out on the billet after finish rolling, and the heating speed and holding time are controlled;

[0060] Straightening and cleaning: the blank after annealing is straightened and cleaned with a high-temperature degreasing agent, and the straightening and cleaning test is performed on the blank after straightening and cleaning, so as to evaluate whether the blank after straightening and cleaning is qualified, and analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument;

[0061] Among them, the tensioning and cleaning equipment includes: tensioning and straightening machine, cleaning equipment;

[0062] Slitting, inspection and packaging: the billets after straightening and cleaning are cut into finished product widths, and various inspections are carried out before packaging;

[0063] The embodiment of the present invention is conceived as follows: straightening and cleaning can significantly improve the shape and straightness of the aluminum coil. The shape and surface quality of the aluminum coil that has been straightened and cleaned are significantly improved, which provides a good foundation for subsequent processing. In the links of finishing rolling, slitting, packaging, etc., the flat and clean aluminum coil is easier to operate, reducing the processing difficulty and defective rate caused by poor shape or surface contamination. Straightening and cleaning detection is an important link to ensure the quality and performance of aluminum coil products. Only aluminum coils that have been effectively cleaned can ensure good surface quality and performance during subsequent processing and use. Through detection, problems in the cleaning process can be discovered in time, such as incomplete cleaning, residual cleaning agent, etc., so as to adjust the cleaning process in time to ensure product quality.

[0064] Embodiment 2:

[0065] Based on Example 1, please refer to Figure 1 , Figure 2 As shown, the production method of a high-strength single-zero aluminum foil according to an embodiment of the present invention also includes a method for evaluating whether the blank after straightening and cleaning is qualified:

[0066] The billet after straightening and cleaning is tested to obtain test data, and test parameters are calculated based on the test data, so as to evaluate the billet after straightening and cleaning based on the test parameters to determine whether the billet after straightening and cleaning is qualified;

[0067] Among them, the test data include: tension, straightening and cleaning characterization value, uniformity characterization value;

[0068] Specifically, the method for acquiring the detection data is:

[0069] A1: Divide the surface of the billet after straightening and cleaning into multiple sub-areas evenly;

[0070] A2: Use a laser transmitter to emit a light source of fixed intensity to the surface of the billet after straightening and cleaning, and use a laser receiver to receive the intensity of the reflected light on the surface of the billet after straightening and cleaning, obtain the reflected light intensity of each sub-area on the surface of the billet after straightening and cleaning, calculate the difference between the reflected light intensity of the sub-area on the surface of the billet after straightening and cleaning and the reflected light intensity of the preset sub-area, and take the absolute value to obtain the reflected light intensity deviation value of the sub-area on the surface of the billet after straightening and cleaning, and mark the reflected light intensity deviation value of the sub-area on the surface of the billet after straightening and cleaning as Qi, where i represents different sub-areas on the surface of the billet after straightening and cleaning, and i is a positive integer;

[0071] The preset sub-region reflected light intensity is the reflected light intensity of the sub-region on the surface of the blank after straightening and cleaning under ideal conditions;

[0072] A3: Calculate the mean of the reflected light intensity deviation values ​​Qi of all sub-regions on the surface of the blank after straightening and cleaning to obtain the mean of the reflected light intensity deviation of the sub-regions, calculate the ratio of the mean of the reflected light intensity deviation of the sub-regions to the mean threshold of the reflected light intensity deviation of the sub-regions, and obtain the straightening and cleaning characterization value, which is marked as LQ;

[0073] A4: Calculate the standard deviation of the reflected light intensity deviation value Qi of all sub-regions on the surface of the blank after straightening and cleaning and the mean value of the reflected light intensity deviation of the sub-region to obtain the standard deviation of the reflected light intensity deviation of the sub-region, calculate the ratio of the standard deviation of the reflected light intensity deviation of the sub-region to the standard deviation threshold of the reflected light intensity deviation of the sub-region, that is, obtain the uniform characterization value, and mark the uniform characterization value as JY;

[0074] Specifically, the calculation method of the detection parameters is:

[0075] The tension and cleaning characterization value LQ and the uniform characterization value JY are processed;

[0076] By formula: Calculate and obtain the detection parameter JC, where a1 and a2 are preset proportional factors and are both greater than 0;

[0077] Specifically, the evaluation method for evaluating whether the blank after straightening and cleaning is qualified is:

[0078] The detection parameter threshold is preset as JR, and the detection parameter JC is compared and analyzed with the detection parameter threshold JR;

[0079] If the detection parameter JC is less than the detection parameter threshold JR, the blank after straightening and cleaning is judged to be qualified;

[0080] If the detection parameter JC ≥ the detection parameter threshold JR, the blank after straightening and cleaning is judged to be unqualified;

[0081] The embodiment of the present invention is conceived as follows: the straightening cleaning characterization value LQ is expressed as: quantitatively evaluating the overall cleanliness of the blank surface after straightening cleaning; by comparing the deviation between the actual reflected light intensity and the ideal reflected light intensity, and calculating the ratio of the mean value to the preset threshold value, the straightening cleaning characterization value LQ can intuitively reflect the quality of the cleaning effect. The lower the straightening cleaning characterization value LQ, the better the cleaning effect, and the surface stains and impurities are effectively removed; the higher the straightening cleaning characterization value LQ, it may mean that the cleaning is not thorough or there are other problems;

[0082] The main purpose of the uniformity characterization value JY is to evaluate the uniformity of the reflected light intensity on the surface of the blank after drawing, straightening and cleaning; by calculating the standard deviation of the reflected light intensity deviation in the sub-area and comparing it with the preset threshold, the uniformity characterization value JY can reflect the consistency of the surface quality. The lower the uniformity characterization value JY, the more uniform the distribution of the reflected light intensity on the surface, that is, the more stable the surface quality and the smoother the surface; the higher the uniformity characterization value JY, it may mean that there are uneven stains, damage or other quality problems on the surface.

[0083] Embodiment three:

[0084] Based on the first and second embodiments, please refer to Figure 1 , Figure 3 As shown, a method for producing a high-strength single-zero aluminum foil according to an embodiment of the present invention further includes a method for analyzing the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument:

[0085] Obtain the abnormal fluctuation time period, and obtain the analysis parameters according to the abnormal fluctuation time period and the reflected light intensity deviation value Qi of the surface sub-area of ​​the blank after straightening and cleaning, and compare and analyze the analysis parameters, so as to analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument;

[0086] Specifically, the method for obtaining the abnormal fluctuation time period is:

[0087] B1: During the straightening and cleaning process, the straightening and cleaning instrument is tested in real time to obtain the real-time voltage of the straightening and cleaning instrument;

[0088] B2: Based on a two-dimensional coordinate system with time as the X-axis and the voltage of the straightening and cleaning instrument as the Y-axis, a voltage fluctuation curve is obtained according to the real-time voltage of the straightening and cleaning instrument, and a preset range area with a Y-axis value of a preset voltage range and parallel to the X-axis is drawn;

[0089] B3: Obtain abnormal voltage fluctuations according to the voltage fluctuation curve and the preset range area, and record the time of each abnormal voltage fluctuation. The time period of the abnormal voltage fluctuation is the abnormal fluctuation time period;

[0090] The method for obtaining abnormal voltage fluctuation is as follows: calculating the area enclosed by the portion of the voltage fluctuation curve that exceeds the preset range and the preset range to obtain the fluctuation pre-abnormal area, and presetting the fluctuation pre-abnormal area threshold, comparing and analyzing the fluctuation pre-abnormal area with the fluctuation pre-abnormal area threshold, and if the fluctuation pre-abnormal area ≥ the fluctuation pre-abnormal area threshold, marking the portion of the voltage fluctuation curve that exceeds the preset range as abnormal voltage fluctuation;

[0091] Specifically, the method for obtaining the analysis parameters is:

[0092] According to the reflected light intensity deviation value Qi of the sub-area on the surface of the blank after straightening and cleaning, the straightening and cleaning abnormal time period is obtained, the straightening and cleaning abnormal time period is compared and analyzed with the abnormal fluctuation time period, and the time overlap between the straightening and cleaning abnormal time period and the abnormal fluctuation time period is calculated. The ratio of the time overlap to the time overlap threshold is the analysis parameter;

[0093] Among them, the method for obtaining the abnormal time period of straightening and cleaning is as follows: presetting the reflected light intensity deviation value threshold of the billet surface sub-region after straightening and cleaning as QR, comparing and analyzing the reflected light intensity deviation value Qi of the billet surface sub-region after straightening and cleaning with the reflected light intensity deviation value threshold QR of the billet surface sub-region after straightening and cleaning, marking the billet surface sub-region after straightening and cleaning whose reflected light intensity deviation value Qi of all the billet surface sub-regions after straightening and cleaning is greater than or equal to the reflected light intensity deviation value threshold QR of the billet surface sub-region after straightening and cleaning as the abnormal straightening and cleaning sub-region, and recording the time period when the abnormal straightening and cleaning sub-region is straightening and cleaning, that is, obtaining the abnormal straightening and cleaning time period;

[0094] Specifically, the method for analyzing the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument is as follows:

[0095] Preset the analysis parameter threshold, and compare and analyze the analysis parameter with the analysis parameter threshold;

[0096] If the analysis parameter is less than the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning has nothing to do with the voltage fluctuation of the straightening and cleaning instrument;

[0097] If the analysis parameter is ≥ the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning is related to the voltage fluctuation of the straightening and cleaning instrument.

[0098] Embodiment 4:

[0099] Based on the first, second and third embodiments, please refer to Figure 4 As shown, a production system of a high-strength single-zero aluminum foil according to an embodiment of the present invention comprises:

[0100] The qualified assessment module is used to detect the billet after drawing, straightening and cleaning, obtain the test data, and calculate the test parameters according to the test data, so as to evaluate the billet after drawing, straightening and cleaning according to the test parameters to evaluate whether the billet after drawing, straightening and cleaning is qualified;

[0101] The relationship analysis module is used to obtain the abnormal fluctuation time period, and according to the abnormal fluctuation time period and the reflected light intensity deviation value Qi of the sub-area on the surface of the blank after straightening and cleaning, obtain the analysis parameters, preset the analysis parameter threshold, compare and analyze the analysis parameters with the analysis parameter threshold, and analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument.

[0102] The above thresholds are set for the convenience of comparison. The thresholds depend on the amount of sample data and the number of bases set by technicians in this field for each set of sample data.

[0103] The above formulas are obtained by collecting a large amount of data and performing software simulation to select a formula close to the actual value. The factors in the formula are set by technicians in this field according to actual conditions; for example: Formula A technician in this field collects multiple groups of test data and sets corresponding test parameters for each group of test data; substitutes the set test parameters and the collected test data into the formula, any three formulas constitute a three-variable linear equation system, and the calculated factors are screened and averaged to obtain the values ​​of a1 and a2, which are 2.45 and 2.23 respectively;

[0104] The size of the factor is to quantify each parameter to obtain a specific value for subsequent comparison. The size of the factor depends on the amount of test data and the preliminary setting of corresponding test parameters for each set of test data by technical personnel in this field; as long as it does not affect the proportional relationship between the parameter and the quantized value, such as the test parameter is proportional to the value of the straightening and cleaning characterization value.

[0105] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for producing high-strength single-zero aluminum foil, characterized in that: include: Melting, casting and rolling, first rough rolling, intermediate annealing, second rough rolling, trimming, finishing rolling, finished product annealing, straightening and cleaning, slitting, inspection and packaging; Conducting a straightening and cleaning test on the billet after straightening and cleaning, so as to evaluate whether the billet after straightening and cleaning is qualified; Analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument. The specific method is: Obtain the abnormal fluctuation time period, and according to the abnormal fluctuation time period and the reflected light intensity deviation value Qi of the blank surface sub-area after straightening and cleaning, obtain the analysis parameter, preset the analysis parameter threshold, compare and analyze the analysis parameter with the analysis parameter threshold, and analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument; If the analysis parameter is less than the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning has nothing to do with the voltage fluctuation of the straightening and cleaning instrument; If the analysis parameter is ≥ the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning is related to the voltage fluctuation of the straightening and cleaning instrument.

2. The method for producing a high-strength single-zero aluminum foil according to claim 1, characterized in that: The method for obtaining the abnormal fluctuation time period is: B1: During the straightening and cleaning process, the straightening and cleaning instrument is tested in real time to obtain the real-time voltage of the straightening and cleaning instrument; B2: Based on a two-dimensional coordinate system with time as the X-axis and the voltage of the straightening and cleaning instrument as the Y-axis, a voltage fluctuation curve is obtained according to the real-time voltage of the straightening and cleaning instrument, and a preset range area with a Y-axis value of a preset voltage range and parallel to the X-axis is drawn; B3: Obtain abnormal voltage fluctuations according to the voltage fluctuation curve and the preset range area, and record the time of each abnormal voltage fluctuation. The time period of the abnormal voltage fluctuation is the abnormal fluctuation time period.

3. The method for producing a high-strength single-zero aluminum foil according to claim 2, characterized in that: The method for obtaining the abnormal voltage fluctuation is as follows: calculate the area enclosed by the part of the voltage fluctuation curve that exceeds the preset range area and the preset range area, obtain the fluctuation pre-abnormal area, and preset a fluctuation pre-abnormal area threshold, compare and analyze the fluctuation pre-abnormal area with the fluctuation pre-abnormal area threshold, if the fluctuation pre-abnormal area ≥ the fluctuation pre-abnormal area threshold, then mark the part of the voltage fluctuation curve that exceeds the preset range area as abnormal voltage fluctuation.

4. The method for producing a high-strength single-zero aluminum foil according to claim 1, characterized in that: The method for obtaining the analysis parameters is: According to the reflected light intensity deviation value Qi of the sub-area on the surface of the blank after straightening and cleaning, the abnormal time period of straightening and cleaning is obtained, the abnormal time period of straightening and cleaning is compared and analyzed with the abnormal fluctuation time period, and the time overlap between the abnormal time period of straightening and cleaning and the abnormal fluctuation time period is calculated. The ratio of the time overlap to the time overlap threshold is the analysis parameter.

5. The method for producing a high-strength single-zero aluminum foil according to claim 4, characterized in that: The method for obtaining the abnormal time period of straightening and cleaning is as follows: presetting the reflected light intensity deviation value threshold of the billet surface sub-area after straightening and cleaning as QR, comparing and analyzing the reflected light intensity deviation value Qi of the billet surface sub-area after straightening and cleaning with the reflected light intensity deviation value threshold QR of the billet surface sub-area after straightening and cleaning, marking the billet surface sub-area after straightening and cleaning whose reflected light intensity deviation value Qi of all sub-areas on the billet surface after straightening and cleaning is greater than or equal to the reflected light intensity deviation value threshold QR of the billet surface sub-area after straightening and cleaning as the abnormal sub-area of ​​straightening and cleaning, and recording the time period when the abnormal sub-area of ​​straightening and cleaning is subjected to straightening and cleaning treatment, so as to obtain the abnormal time period of straightening and cleaning.

6. The method for producing a high-strength single-zero aluminum foil according to claim 1, characterized in that: The specific method for evaluating whether the blank after straightening and cleaning is qualified is: The billet after straightening and cleaning is tested to obtain test data, and test parameters are calculated based on the test data, so as to evaluate the billet after straightening and cleaning based on the test parameters to determine whether the billet after straightening and cleaning is qualified; Among them, the detection data includes: tension, straightening and cleaning characterization value and uniformity characterization value.

7. The method for producing a high-strength single-zero aluminum foil according to claim 6, characterized in that: The method for acquiring the detection data is: A1: Divide the surface of the billet after straightening and cleaning into multiple sub-areas evenly; A2: A light source of fixed intensity is emitted to the surface of the billet after straightening and cleaning, and the intensity of the reflected light from the surface of the billet after straightening and cleaning is received to obtain the reflected light intensity of each sub-area of ​​the billet surface after straightening and cleaning, and the reflected light intensity of the sub-area of ​​the billet surface after straightening and cleaning is calculated to be different from the reflected light intensity of the preset sub-area, and the absolute value is taken to obtain the reflected light intensity deviation value of the sub-area of ​​the billet surface after straightening and cleaning, and the reflected light intensity deviation value of the sub-area of ​​the billet surface after straightening and cleaning is marked as Qi, where i represents different sub-areas of the billet surface after straightening and cleaning, and i is a positive integer; A3: Calculate the mean of the reflected light intensity deviation values ​​Qi of all sub-regions on the surface of the blank after straightening and cleaning to obtain the mean of the reflected light intensity deviation of the sub-regions, calculate the ratio of the mean of the reflected light intensity deviation of the sub-regions to the mean threshold of the reflected light intensity deviation of the sub-regions, and obtain the straightening and cleaning characterization value, which is marked as LQ; A4: Calculate the standard deviation based on the reflected light intensity deviation value Qi of all sub-areas on the surface of the blank after straightening and cleaning and the mean value of the reflected light intensity deviation of the sub-areas to obtain the standard deviation of the reflected light intensity deviation of the sub-areas, calculate the ratio of the standard deviation of the reflected light intensity deviation of the sub-areas to the standard deviation threshold of the reflected light intensity deviation of the sub-areas, that is, obtain the uniform characterization value, and mark the uniform characterization value as JY.

8. The method for producing a high-strength single-zero aluminum foil according to claim 7, characterized in that: The method further comprises: The tension and cleaning characterization value LQ and the uniform characterization value JY are processed; By formula: The detection parameter JC is obtained by calculation, wherein a1 and a2 are preset proportional factors and are both greater than 0.

9. The method for producing a high-strength single-zero aluminum foil according to claim 1, characterized in that: The method further comprises: The detection parameter threshold is preset as JR, and the detection parameter JC is compared and analyzed with the detection parameter threshold JR; If the detection parameter JC is less than the detection parameter threshold JR, the blank after straightening and cleaning is judged to be qualified; If the detection parameter JC ≥ the detection parameter threshold JR, the blank after straightening and cleaning is judged to be unqualified.

10. A production system of high-strength single-zero aluminum foil used in the production method of high-strength single-zero aluminum foil according to any one of claims 1 to 9, characterized in that: include: A qualified assessment module, wherein the qualified assessment module is used to perform a straightening and cleaning test on the straightening and cleaning blank, so as to assess whether the straightening and cleaning blank is qualified; A relationship analysis module is used to analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument. The specific method is as follows: Obtain the abnormal fluctuation time period, and according to the abnormal fluctuation time period and the reflected light intensity deviation value Qi of the blank surface sub-area after straightening and cleaning, obtain the analysis parameter, preset the analysis parameter threshold, compare and analyze the analysis parameter with the analysis parameter threshold, and analyze the relationship between the quality of the blank after straightening and cleaning and the straightening and cleaning instrument; If the analysis parameter is less than the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning has nothing to do with the voltage fluctuation of the straightening and cleaning instrument; If the analysis parameter is ≥ the analysis parameter threshold, it is determined that the abnormal quality of the blank after straightening and cleaning is related to the voltage fluctuation of the straightening and cleaning instrument.