Body flange and production method thereof
Through the modified ductile iron material process, combined with ultrasonic treatment and carbonitriding technology, the strength and air tightness problems of the body flange in high temperature and high pressure environments are solved, its tensile strength and wear resistance are improved, and the high-pressure pipeline is ensured security and performance.
Patent Information
- Application Number
- CN202411053692.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing body flange has low tensile strength, low air tightness, internal blisters and pore defects during processing and use. It cannot be used under high pressure conditions, and there is a risk of leakage.
Using the modification and optimization process of ductile iron materials, combined with smelting and refining, ultrasonic-assisted in-pack spheroidization inoculation, isothermal heat treatment, ultrasonic-assisted casting, carbonitriding and cladding wear-resistant coating processes, we have developed better performance Ductile iron material is used to produce the body flange to improve its strength, toughness and wear performance in high temperature and high pressure environments.
The tensile strength, hardness and wear resistance of the body flange are significantly improved to ensure its performance in high temperature and high pressure pipeline environments and avoid leakage risks and material defects.
Smart Images

Figure CN118808561A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flange production and relates to a body flange and a production method thereof. Background Art
[0002] The body flange is a disc-shaped part, which is mainly used for connecting pipes. It is fixed to one end of the pipe. There are holes on the body flange. Bolts pass through the holes to connect and tighten the two flanges, so that the pipes are connected. Gaskets are used to seal the flanges.
[0003] The traditional production process of the body flange includes casting process and mechanical processing. The body flange currently produced by casting process has the following defects in processing and use: (1) The tensile strength of cast iron materials used for casting is lower than that of steel. The internal structure of cast iron alloy is loose and the air tightness is not high. It is easy to break when the pressure or external force is too large. (2) The body flange produced by casting process has defects such as sand holes and air holes inside, and cannot be used under high pressure conditions, otherwise there will be a risk of leakage.
[0004] Therefore, in order to solve the above technical problems, it is urgent to improve the existing production process of the body flange. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a body flange and a production method thereof. The present invention modifies and optimizes the production process of ductile iron material for the body flange, combines the raw material mixture smelting and refining process, ultrasonic-assisted spheroidizing inoculation process, isothermal heat treatment process, ultrasonic-assisted casting process, carbonitriding process and cladding wear-resistant coating process, to develop and produce ductile iron material with better performance. Using it to produce the body flange can greatly improve the performance of the body flange at room temperature, ensure the good comprehensive mechanical properties of the body flange, and can well meet the requirements of strength, toughness and wear performance of the body flange under the high temperature and high pressure pipeline use environment.
[0006] To achieve this object, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a method for producing a body flange, the method comprising: S1. Alloy smelting: putting the raw material mixture into a smelting furnace, and smelting the raw material mixture to obtain an alloy melt; S2, refining and purification: adjusting the temperature of the alloy melt to the refining temperature, then adding a purifier to the alloy melt, keeping it at the refining temperature for a period of time, then continuously introducing nitrogen into the smelting furnace, removing scum on the liquid surface to obtain a refined melt; S3, spheroidization inoculation: placing a spheroidizer on one side of the bottom dam of the ladle, compacting and tamping to form a spheroidizer layer, evenly spreading a primary inoculant on the surface of the spheroidizer layer, compacting and tamping to form a primary inoculant layer covering the surface of the spheroidizer layer, and sequentially stacking a perlite layer and an iron plate on the surface of the primary inoculant layer; flushing the refined molten metal in the smelting furnace into the ladle from the side of the bottom dam where the spheroidizer layer and the primary inoculant layer are not placed, and adding a secondary inoculant along the flow during the flushing of the refined molten metal; after the refined molten metal in the smelting furnace is completely flushed into the ladle, extending an ultrasonic probe from above the refined molten metal to below the liquid level of the refined molten metal, applying ultrasonic waves to the refined molten metal, and obtaining a casting liquid after ultrasonic treatment; S4, casting: preheating the mold in advance, when the temperature of the casting liquid reaches the casting temperature, injecting the casting liquid in the molten iron ladle into the preheated mold, adding three inoculants during the pouring process of the casting liquid; after the casting liquid is completely injected into the mold, naturally cooling to a first cooling temperature, then adjusting the cooling rate, ultrasonically vibrating the mold after casting, stopping the ultrasonic vibration when the mold is cooled to a second cooling temperature and keeping the temperature for a period of time, then naturally cooling to room temperature, and demolding to obtain a flange casting; S5, quenching and tempering heat treatment: first, the flange casting after casting is heated to the annealing temperature and kept warm for a period of time, then quickly cooled to the first temperature and kept warm for a period of time, then slowly cooled to the second temperature, taken out of the furnace and air-cooled to room temperature, and the annealing treatment is completed; then, the flange casting after annealing is heated to the normalizing temperature and kept warm for a period of time, then taken out of the furnace and air-cooled to room temperature, and the normalizing treatment is completed; then, the flange casting after normalizing is heated to the quenching temperature and kept warm for a period of time, and after the end of the insulation, it is cooled to the third temperature with the furnace, and then the flange casting is taken out and immediately buried in the preheated molten salt, and after a period of time, the surface temperature of the flange casting is reduced to the fourth temperature, and then it is taken out from the molten salt and air-cooled to room temperature, and the quenching treatment is completed; finally, the flange casting after quenching is heated to the tempering temperature and kept warm for a period of time, and air-cooled to room temperature with the furnace, and the tempering treatment is completed to obtain the flange green billet; S6, nitrocarburizing: introducing carbon dioxide into the reaction furnace, placing the flange green body in the reaction furnace, heating the flange green body to the carburizing temperature and keeping it warm for a period of time to perform carburizing treatment; introducing protective gas into the reaction furnace to cool the flange green body, after the flange green body is cooled to the co-carburizing temperature, introducing a mixed gas consisting of ammonia, nitrogen and carbon dioxide into the reaction furnace, keeping it warm for a period of time, completing the nitrocarburizing treatment, and obtaining a rough flange product; S7, sandblasting roughening: sandblasting the rough flange product with a sandblasting device, then placing the rough flange product after sandblasting in a mixed solvent of anhydrous ethanol and acetone for ultrasonic cleaning, and taking it out and drying it after cleaning; S8, coating cladding: anhydrous ethanol and a binder are mixed in proportion to prepare a binder solution, and a cladding material and the binder solution are mixed in proportion to prepare a paste-like cladding slurry, wherein the cladding material includes nickel-based alloy powder, cerium dioxide and tungsten carbide; the cladding slurry is uniformly applied to the surface of the rough flange after sandblasting, and a cladding slurry layer is formed after drying; the cladding slurry layer is laser clad by a laser, and a cladding layer is formed on the surface of the rough flange after cooling to obtain the body flange.
[0007] The present invention optimizes and modifies the production process of ductile iron materials for body flanges, combines the raw material mixture smelting and refining process, ultrasonic-assisted spheroidizing inoculation process, isothermal heat treatment process, ultrasonic-assisted casting process, carbonitriding process and cladding wear-resistant coating process, and develops and produces ductile iron materials with excellent mechanical properties and wear resistance. Using the ductile iron materials for the production of body flanges can greatly improve the performance of the body flanges at room temperature, and can fully meet the requirements for strength, toughness and wear performance of the body flanges in the high-temperature and high-pressure pipeline use environment.
[0008] The present invention applies ultrasonic treatment during both the spheroidization inoculation and the casting process, wherein, during the spheroidization inoculation process, the ultrasonic probe is inserted into the refined molten liquid to directly perform ultrasonic treatment on the refined molten liquid; during the casting process, the ultrasonic probe is contacted with the mold to indirectly perform ultrasonic treatment on the casting liquid. By performing ultrasonic treatment during the spheroidization inoculation process, the number of graphite balls is increased and the matrix structure is refined; by performing ultrasonic treatment during the casting process, the growth morphology of the graphite balls is uniform and the roundness of the graphite balls is improved. Through the synergistic effect of ultrasonic treatment at different production stages, the comprehensive mechanical properties of the flange casting, such as tensile strength and hardness, can be greatly improved.
[0009] The present invention directly performs ultrasonic treatment on the refined molten liquid through an ultrasonic probe during the spheroidization inoculation process. The high ultrasonic energy generates a negative pressure zone in the local micro-region of the refined molten liquid during the propagation process. When the ultrasonic energy exceeds the surface tension of the refined molten liquid, the refined molten liquid is torn apart to generate a large number of small bubbles. As the ultrasonic time passes, the small bubbles gradually accumulate and grow to form large bubbles. When the pressure in the large bubbles reaches the critical point, they will instantly break and split into more small bubbles. The small bubbles after the splitting will continue to accumulate, grow, break and split repeatedly. When the large bubbles break rapidly, instantaneous high pressure will be generated in the large bubbles. At the same time, the refined molten liquid around the large bubbles will also instantly rush into the bubbles, causing the refined molten liquid near the bubbles to produce strong local vibrations. As the small bubbles continue to accumulate, grow, break and split repeatedly, a cyclic cavitation effect is formed. The impact force generated by each bubble break can strongly flush the dendrites, improve the nucleation rate, and is conducive to the formation of equiaxed crystals. At the same time, the spacing of the secondary dendrites is also reduced, so that the carbides are broken, so that the matrix structure of the flange casting can be refined. In addition, the thermal effect of ultrasound causes the temperature of the refined melt near the ultrasonic probe to increase while the cooling rate to decrease. The high-temperature refined melt is conducive to the growth of graphite nodules. Therefore, the present invention significantly increases the number of graphite nodules by ultrasonically treating the refined melt during the spheroidization inoculation process.
[0010] The invention adopts a specially formulated inoculant, and adopts different inoculants in the processes of ladle inoculation, flushing inoculation and casting inoculation to meet the inoculation requirements of different processing stages, so that the processed body flange has higher strength and better wear resistance; during the ladle inoculation, the first inoculant is laid in layers, and the inoculation effect can be improved after the refined solution is flushed into the molten iron ladle; during the inoculation process, ultrasonic vibration is applied to the refined solution, which is beneficial to increase the number of graphite cores and the roundness of graphite balls, thereby improving the strength of the body flange; casting inoculation is performed after the ladle inoculation, so that the inoculation effect can be prolonged.
[0011] The present invention indirectly performs ultrasonic treatment on the casting liquid through an ultrasonic probe during the casting process, and the cooling rate of the casting liquid in the mold is slowed down through the acoustic cavitation effect and thermal effect of the ultrasonic wave, so that the carbon-poor area and the carbon-rich area in the casting liquid can fully diffuse to achieve carbon balance, which is beneficial to reduce the area of the carbon-poor area around the graphite ball. During the cooling and solidification process of the casting liquid, the graphite ball can grow freely in the casting liquid without being constrained and limited by the space of the carbon-poor area. Therefore, the graphite balls in the flange casting finally formed are uniform in size and have a high roundness, which is beneficial to further improve the comprehensive mechanical properties of the flange casting.
[0012] The present invention adopts two-stage cooling in the casting process, which improves the uniformity of the components of the flange casting and is conducive to further improving the comprehensive mechanical properties of the flange casting. When the casting liquid obtained after refining is naturally cooled from the casting temperature to the first cooling temperature, a solid phase begins to be generated in the casting liquid, and the preferential growth of grains begins inside the casting liquid. At this time, adjusting the cooling rate of the mold and performing ultrasonic vibration treatment at the same time can improve the uniformity of the components inside the casting liquid, promote grain refinement, and greatly enhance the fine grain strengthening effect inside the flange casting; when the mold is reduced to the second cooling temperature, the solute inside the flange casting can be fully diffused through long-term heat preservation, reducing the possibility of segregation inside the flange casting, and further enhancing the comprehensive mechanical properties of the flange casting.
[0013] Since the present invention adds nickel, molybdenum, vanadium and other whitening elements to the raw material mixture of the main flange, the whitening elements have the ability to bind carbon atoms during the casting process, which will slow down the diffusion rate of carbon atoms into the graphite balls; and the added nickel element has the function of stabilizing austenite, therefore, the edge of the flange casting obtained after casting has a whitening tendency, and there are a large number of large-sized primary cementites, which leads to the reduction of the comprehensive mechanical properties of the main flange. Therefore, in order to ensure that the main flange has sufficient tensile strength to improve the actual plasticity, obtain high strength and toughness, and at the same time cannot reduce its tensile strength, the present invention heat treats the flange casting to eliminate free cementite as much as possible, and homogenizes the metallographic structure and internal composition of the flange casting. In this way, the mechanical properties of the flange casting are improved.
[0014] The present invention adopts a high-temperature and low-temperature two-stage annealing process to decompose the pearlite in the matrix structure, and transforms the matrix structure composed of ferrite, pearlite, graphite nodules and tiny graphite particles into a matrix structure composed of ferrite, graphite nodules and tiny graphite particles. The two-stage annealing process can change the matrix structure, thereby improving the mechanical properties of the body flange.
[0015] The present invention adopts a gas carbonitriding process, a flange green body is placed in a reaction furnace, a gas medium containing carbon atoms and nitrogen atoms is introduced into the furnace, and during the high-temperature heating process, carbon atoms and nitrogen atoms diffuse on the surface of the flange green body and are absorbed by the surface of the flange green body into the interior, thereby forming a carbonitriding layer with a certain thickness, which can achieve both the carburizing depth and the nitriding hardness, so that many properties of the flange green body, such as toughness, hardness and wear resistance, are significantly improved.
[0016] The present invention forms a cladding layer on the surface of the rough flange product after sandblasting by laser cladding technology. By setting the cladding layer on the surface of the rough flange product, the strength and hardness of the main flange surface can be significantly improved, and the wear resistance of the main flange surface can be improved. The cladding layer includes nickel-based alloy powder, cerium dioxide and tungsten carbide. The laser cladding technology makes the tungsten carbide particles in the cladding layer dispersed in the nickel-based alloy powder without grain boundary segregation. Therefore, by adding tungsten carbide particles of hard phase, the high-temperature wear resistance and hardness of the cladding layer can be significantly improved; in addition, since tungsten carbide has high-temperature stability, it has little effect on the microstructure and metallographic structure of the cladding layer. The addition of cerium dioxide particles can accelerate the dissolution of cerium dioxide particles and promote the improvement of their shape. At the same time, the cerium dioxide particles are dispersed and filled in the nickel-based alloy powder, so that the laser energy can be smoothly transmitted along the nickel-based alloy powder, thereby accelerating the melting rate of the nickel-based alloy powder, so that the nickel-based alloy powder can be quickly melted, solidified and crystallized, which has a refinement effect on the metallographic structure of the cladding layer, can effectively reduce defects such as cracks and holes in the cladding layer, and is conducive to the formation of a cladding layer with a denser metallographic structure, thereby improving the comprehensive mechanical properties of the cladding layer.
[0017] As a preferred technical solution of the present invention, in step S1, the raw material mixture is composed of the following elements in mass fractions, based on the mass fraction of the raw material mixture being 100wt%: Carbon 3.5~3.7wt%, silicon 2~2.5wt%, manganese 0.3~0.6wt%, nickel 0.1~0.2wt%, molybdenum 0.3~0.4wt% and vanadium 0.2~0.5wt%, the balance is iron; wherein the mass fraction of carbon can be 3.5wt%, 3.52wt%, 3.54wt%, 3.56wt%, 3.58wt%, 3.6wt%, 3.62wt%, 3.64wt%, 3.66wt%, 3.68wt% or 3.7wt%; the mass fraction of silicon can be 2.0wt%, 2 The mass fraction of manganese can be 0.05wt%, 2.1wt%, 2.15wt%, 2.2wt%, 2.25wt%, 2.3wt%, 2.35wt%, 2.4wt%, 2.45wt%, or 2.5wt%; the mass fraction of manganese can be 0.3wt%, 0.32wt%, 0.34wt%, 0.36wt%, 0.38wt%, 0.4wt%, 0.42wt%, 0.44wt%, 0.46wt%, 0.48wt%, 0.5wt%, 0.52wt%, 0.54wt%, 0.56wt t%, 0.58wt% or 0.6wt%; the mass fraction of nickel can be 0.1wt%, 0.1wt%, 0.11wt%, 0.12wt%, 0.13wt%, 0.14wt%, 0.15wt%, 0.16wt%, 0.17wt%, 0.18wt%, 0.19wt% or 0.2wt%; the mass fraction of molybdenum can be 0.3wt%, 0.31wt%, 0.32wt%, 0.33wt%, 0.34wt%, 0.35wt%, 0.36wt%, 0.37wt% %, 0.38wt%, 0.39wt% or 0.4wt%; the mass fraction of vanadium can be 0.2wt%, 0.22wt%, 0.24wt%, 0.26wt%, 0.28wt%, 0.3wt%, 0.32wt%, 0.34wt%, 0.36wt%, 0.38wt%, 0.4wt%, 0.42wt%, 0.44wt%, 0.46wt%, 0.48wt% or 0.5wt%, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0018] The present invention specifically limits the carbon content in the raw material mixture to 3.5~3.7wt%. The carbon element has three forms of existence in the matrix structure. One is solid solution into the matrix structure to achieve a solid solution strengthening effect; the second is to form graphite balls. The higher the carbon content, the more graphite balls precipitated in the matrix structure, and the smaller the diameter of the graphite balls, so that the roundness of the graphite balls is improved; the third is to form carbides to achieve a precipitation strengthening effect. Since the formation of graphite balls requires a higher concentration of carbon content, the carbon content in the raw material mixture cannot be less than 3.5wt%. As the carbon content increases, the number of free cementite decreases. When the carbon content reaches 3.5wt%, the cementite disappears. However, when the carbon content exceeds 3.7wt%, it will cause the floating of graphite balls.
[0019] The present invention specifically limits the silicon content in the raw material mixture to 2~2.5wt%. Silicon can not only effectively reduce the tendency of white cast iron, but also has the effect of refining the eutectic group and improving the roundness of graphite spheres. However, silicon element will cause the tough-brittle transition temperature of the matrix to increase, resulting in a decrease in the tensile strength and hardness of the matrix; in addition, when the silicon content exceeds 2.5wt%, the roundness of the graphite spheres will be destroyed, resulting in graphite distortion and the production of fragmented graphite. Therefore, in order to ensure the roundness of the graphite spheres in the body flange without affecting the tensile strength and hardness of the body flange, the present invention specifically limits the silicon content in the raw material mixture to 2~2.5wt%.
[0020] The present invention specifically limits the manganese content in the raw material mixture to 0.3-0.6wt%. As the manganese content increases, the tensile strength of the prepared body flange gradually increases, but the elongation decreases significantly as the manganese content increases. This is because the manganese element can expand the austenite phase region, and the manganese atoms can increase the phase change resistance to prevent the diffusion rate of iron atoms, thereby slowing down the decomposition rate of austenite and increasing the critical supercooling of the eutectoid transformation. However, as the manganese content increases, the manganese atoms easily replace the iron atoms in the matrix and form a network of cementite with carbon, thereby reducing the toughness of the matrix and causing the elongation of the body flange to decrease.
[0021] The present invention specifically limits the nickel content in the raw material mixture to 0.1-0.2wt%. Nickel is a graphitizing element and has no effect on the graphite morphology. Therefore, nickel can reduce the tendency of white cast iron. In addition, nickel can be infinitely dissolved in the casting liquid and does not form carbides with carbon, has a carbon removal effect, and is beneficial to improving the toughness of the matrix. At the same time, nickel is also an austenite forming element, which can reduce the transformation temperature of austenite to ferrite, shift the eutectoid point to the left, and improve the hardenability of the matrix. When the nickel content in the raw material mixture is within the range of 0.1-0.2wt%, as the nickel content increases, the hardenability of the matrix is improved, and austenite is transformed into martensite, so that the hardness of the body flange finally prepared is greatly improved, and there is an appropriate amount of residual austenite, which is beneficial to improve the toughness of the body flange, so that the body flange has both high hardness and high toughness; when the nickel content exceeds 0.2wt%, due to the increase in the content of residual austenite in the cast iron structure, the hardness decreases instead.
[0022] The present invention specifically limits the molybdenum content in the raw material mixture to 0.3-0.4wt%, and the vanadium content to 0.2-0.5wt%. Molybdenum and vanadium are white cast elements in the solidification process of the casting liquid, which are not conducive to the precipitation of carbon in the form of graphite. Part of the molybdenum and vanadium in the casting liquid are dissolved into the matrix structure, and part of them form carbides. Since the precipitation temperature and melting point of the carbides of molybdenum and vanadium are relatively high, the high-temperature stability of the body flange can be improved and the high-temperature hardness of the body flange can be ensured. In addition, molybdenum and vanadium elements can also refine the grain size of the structure, increase the number of graphite balls, reduce the critical cooling rate, improve its hardenability, slow down the softening trend of the body flange at high temperature, and thus improve the high-temperature creep resistance of the body flange. However, the content of molybdenum and vanadium should not be too high. When it exceeds the upper limit of the range defined by the present invention, it will lead to a decrease in the number of graphite balls precipitated in the matrix structure.
[0023] In some optional examples, the smelting temperature is 1450-1460°C, for example, it can be 1450°C, 1451°C, 1452°C, 1453°C, 1454°C, 1455°C, 1456°C, 1457°C, 1458°C, 1459°C or 1460°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] In some optional examples, the smelting time is 1 to 2 hours, for example, it can be 1.0h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h or 2.0h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] As a preferred technical solution of the present invention, in step S2, the refining temperature is 1520-1540°C, for example, it can be 1520°C, 1522°C, 1524°C, 1526°C, 1528°C, 1530°C, 1532°C, 1534°C, 1536°C, 1538°C or 1400°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] In some optional examples, the mass ratio of the purifier to the alloy melt is (0.4~0.6):100, for example, it can be 0.4:100, 0.42:100, 0.44:100, 0.46:100, 0.48:100, 0.5:100, 0.52:100, 0.54:100, 0.56:100, 0.58:100 or 0.6:100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] In some optional examples, the refining temperature is kept for 50 to 60 minutes, for example, 50 minutes, 51 minutes, 52 minutes, 53 minutes, 54 minutes, 55 minutes, 56 minutes, 57 minutes, 58 minutes, 59 minutes or 60 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] In some optional examples, the nitrogen introduction pressure is 1.5~1.8 MPa, for example, it can be 1.5 MPa, 1.52 MPa, 1.54 MPa, 1.56 MPa, 1.58 MPa, 1.6 MPa, 1.62 MPa, 1.64 MPa, 1.66 MPa, 1.68 MPa, 1.7 MPa, 1.72 MPa, 1.74 MPa, 1.76 MPa, 1.78 MPa or 1.8 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] In some optional embodiments, the nitrogen gas flow rate is 100-150 Nm 3 / h, for example, it can be 100Nm 3 / h、105Nm 3 / h、110Nm 3 / h、115Nm 3 / h、120Nm 3 / h、125Nm 3 / h、130Nm 3 / h、135Nm 3 / h、140Nm 3 / h、145Nm 3 / h or 150Nm 3 / h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] In some optional examples, the nitrogen introduction time is 10 to 20 min, for example, it can be 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min or 20 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] As a preferred technical solution of the present invention, in step S3, the mass ratio of the spheroidizing agent to the refined melt is (1.5-2.5):100, for example, it can be 1.5:100, 1.6:100, 1.7:100, 1.8:100, 1.9:100, 2.0:100, 2.1:100, 2.2:100, 2.3:100, 2.4:100 or 2.5:100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] The present invention particularly defines the mass ratio of the spheroidizing agent to the refined melt as (1.5-2.5):100. When the amount of the spheroidizing agent added is lower than the lower limit of the range defined by the present invention, the graphite balls in the obtained cast iron structure will be not round, the periphery will crack, and the graphite balls will be in the form of blooming or pointed protrusions. The diameter of the graphite balls is large and the number is small. This is because the amount of the spheroidizing agent added is too small, resulting in insufficient spheroidizing elements, causing magnesium to be severely burned and oxidized, resulting in poor spheroidization. When the amount of the spheroidizing agent added is within the numerical range defined by the present invention, the spheroidizing effect of the prepared body flange is better, the shape of the graphite balls in the organization is more rounded, the diameter is smaller and the number is larger. This is because the spheroidizing agent has a good absorption effect during the spheroidizing treatment process, the residual amount of magnesium is moderate, and the fine spheroidizing agent particles inhibit the precipitation of cementite, so that graphite is precipitated in large quantities in an instant, so a large number of graphite balls with small size and uniform distribution are obtained, so that the mechanical properties of the body flange are significantly improved. When the amount of the spheroidizing agent added exceeds the upper limit of the range defined in the present invention, agglomerated graphite will appear and the graphite distribution will be uneven. This is because the amount of the spheroidizing agent added is too high, resulting in a poor spheroidizing effect. Although adding spheroidizing elements to the refined melt is a basic condition for producing graphite balls, the spheroidizing elements have surface activity. When the residual amount of the spheroidizing elements is high, the free atom adsorption density will increase, blocking some growth steps, causing the graphite morphology to be distorted, resulting in a graphite morphology similar to that when the amount of the spheroidizing agent added is too low.
[0033] In some optional examples, based on the mass fraction of the spheroidizing agent being 100wt%, it is composed of the following elements in mass fractions:Silicon 40-45wt%, magnesium 7-7.5wt%, manganese 3-4wt%, calcium 2-3wt%, yttrium 1.2-1.5wt%, cerium 0.4-0.5wt%, lanthanum 0.4-0.5wt%, neodymium 0.4-0.5wt%, aluminum 0.1-0.5wt% and titanium 0.1-0.5wt%, and the balance is iron; wherein the mass fraction of silicon can be 40wt%, 40.5wt%, 41wt%, 41.5wt%, 42wt%, 42.5wt%, 43wt%, 43.5wt%, 44wt%, 44.5wt% or 45wt%; the mass fraction of magnesium can be 7.0wt%, 7.05wt%, 7.1wt%, 7.15wt%, 7.2wt%, 7. The mass fraction of manganese can be 3.0wt%, 3.1wt%, 3.2wt%, 3.3wt%, 3.4wt%, 3.5wt%, 3.6wt%, 3.7wt%, 3.8wt%, 3.9wt% or 4.0wt%; the mass fraction of calcium can be 2.0wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt% or 3.0wt%; the mass fraction of yttrium can be 1.2wt%, 1.22wt%, 1.24wt%, 1.2 % or 0.5wt%; the mass fraction of cerium can be 0.4wt%, 0.41wt%, 0.42wt%, 0.43wt%, 0.44wt%, 0.45wt%, 0.46wt%, 0.47wt%, 0.48wt%, 0.49wt% or 0.5wt%; the mass fraction of lanthanum can be 0.4wt%, 0.41wt%, 0.42wt%, 0.43wt%, 0.44wt%, 0.45wt%, 0.46wt%, 0.47wt%, 0.48wt%, 0.49wt% or 0.5wt%; the mass fraction of lanthanum can be 0.4wt%, 0.41wt%, 0.42wt%, 0.43wt%, 0.44wt%, 0.45wt%, 0.46wt%, 0.47wt%, 0.48wt%, 0.49wt% or 0.5wt%. .46wt%, 0.47wt%, 0.48wt%, 0.49wt% or 0.5wt%; the mass fraction of neodymium can be 0.4wt%, 0.41wt%, 0.42wt%, 0.43wt%, 0.44wt%, 0.45wt%, 0.46wt%, 0.47wt%, 0.48wt%, 0.49wt% or 0.5wt%; the mass fraction of aluminum can be 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt% or 0.5wt%; the mass fraction of titanium can be 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt% or 0.5wt%, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0034] Magnesium is the main component of the spheroidizing agent, which can spheroidize graphite in the refining solution of hypoeutectic, eutectic and hypereutectic components, and has good desulfurization and oxygen absorption capabilities. Rare earth elements such as yttrium, cerium, lanthanum, and neodymium have a strong affinity with oxygen, molybdenum, vanadium and other elements that interfere with spheroidization in the refining solution. They can not only purify the refining solution, but also provide a certain heterogeneous core, which is conducive to reducing casting defects such as inclusions and subcutaneous pores, and at the same time, the spheroidizing effect of magnesium is fully exerted, playing a role in spheroidization or indirect spheroidization; however, excessive rare earth residues in the refining solution will lead to the deterioration of graphite morphology and graphite distortion. Therefore, the present invention specifically limits the content of rare earth elements such as yttrium, cerium, lanthanum, neodymium, etc., and adds manganese, calcium, aluminum and titanium at the same time. The four elements can play a synergistic role to delay the decomposition of magnesium, control the absorption and reaction rate of the spheroidizing agent, prevent graphite distortion, increase the number of graphite cores, prolong the spheroidization decay time, promote nucleation, and refine the organization, so that the mechanical properties of the final prepared body flange are significantly improved.
[0035] In some optional examples, the particle size D90 of the spheroidizing agent is 10-15 mm, for example, 10 mm, 10.5 mm, 11 mm, 11.5 mm, 12 mm, 12.5 mm, 13 mm, 13.5 mm, 14 mm, 14.5 mm or 15 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] The present invention adopts an improved flushing method for spheroidization. Since the density of the spheroidizer is relatively small, after it is made into a powdered spheroidizer with a particle size D90 of 10-15 mm, it is easy to float during the reaction process. Considering that the powdered spheroidizer will burn violently in the refining solution and is easy to burn, the present invention covers the spheroidizer with a primary inoculant during the spheroidization process, and then lays perlite and iron plate on the primary inoculant, and then flushes the refined melt into the iron ladle for spheroidization. In this way, it can be ensured that when the powdered spheroidizer is poured into the refined melt, it will not immediately come into contact with the refined solution to react violently, but will start to react after a certain amount of refined solution has been poured in, thereby delaying the initial reaction time of the spheroidizer and the refined solution and slowing down the reaction speed; at the same time, when the refined solution reacts with the spheroidizer, the liquid level of the refined solution is already high, which also prolongs the floating time of the spheroidizer, so that the spheroidizer can be evenly and slowly absorbed in the refined solution, and will not quickly float to the liquid surface of the refined solution to be oxidized and burned.
[0037] The present invention limits the particle size D90 of the spheroidizer to 10-15 mm, the gaps between the powdered spheroidizer particles are small, the refined solution is not easy to penetrate between the spheroidizer particles, and only when the amount of the refined solution in the molten iron ladle is high, the perlite and the iron plate will melt layer by layer, thereby prolonging the detonation time of the spheroidizer; in addition, the spheroidization reaction is started only when the amount of the refined solution in the molten iron ladle is high, so that the floating and melting time of the spheroidizer in the refined solution is prolonged, the probability of magnesium escape is reduced, and the utilization rate of magnesium is increased. In addition, as the particle size of the spheroidizer decreases, the specific surface area of the spheroidizer particles increases, the activity is enhanced, and when the spheroidizer contacts the refined solution, it will quickly react with the anti-spheroidizing elements such as sulfur and oxygen in the refined solution, shortening the free growth time of the graphite ball in the liquid state, so that the spheroidizing elements are completely consumed during the floating process, and the phenomenon of the spheroidizer floating to the surface of the refined solution and burning is avoided. When the particle size D90 of the spheroidizer exceeds 15mm, the gaps between the spheroidizers are larger, and the refining solution can easily penetrate into the gaps between the spheroidizers. At this time, once the refining solution is rushed into the ladle, the spheroidizer will explode. At the same time, since the refining solution can quickly enter the gaps between the spheroidizers, it is easy for part of the spheroidizer to float to the surface of the refining solution to undergo an oxidation reaction, causing the escape of magnesium and reducing the utilization rate of magnesium.
[0038] In some optional examples, the primary inoculant is composed of silicon-calcium-barium alloy and silicon carbide, wherein the mass ratio of the silicon-calcium-barium alloy to the refined melt is (0.2-0.3):100, for example, it can be 0.2:100, 0.21:100, 0.22:100, 0.23:100, 0.24:100, 0.25:100, 0.26:100, 0.27:100, 0.28:100, 0.29:100 or 0.3:10. 0; the mass ratio of the silicon carbide to the refined melt is (0.1-0.2):100, for example, it can be 0.1:100, 0.11:100, 0.12:100, 0.13:100, 0.14:100, 0.15:100, 0.16:100, 0.17:100, 0.18:100, 0.19:100 or 0.2:100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] In some optional examples, based on the mass fraction of the silicon-calcium-barium alloy being 100wt%, it is composed of the following elements in mass fractions: 40-45wt% silicon, 12-15wt% calcium, 10-12wt% barium, 0.3-0.6wt% zirconium and 0.15-0.3wt% antimony, with the remainder being iron; wherein the mass fraction of silicon may be 40wt%, 40.5wt%, 41wt%, 41.5wt%, 42wt%, 42.5wt%, 43wt%, 43.5wt%, 44wt%, 44.5wt% or 45wt%; the mass fraction of calcium may be 12wt%, 12.2wt%, 12.4wt%, 12.6wt%, 12.8wt%, 13wt%, 13.2wt%, 13.4wt%, 13.6wt%, 13.8wt%, 14wt%, 14.2wt%, 14.4wt%, 14.6wt%, 14.8wt% or 15wt%; the mass fraction of barium may be 10wt%, 10.2wt%, 10.4wt%, 10.6wt%, 10.8wt%, 11wt%, 11. % or 0.2wt%; the mass fraction of zirconium can be 0.3wt%, 0.32wt%, 0.34wt%, 0.36wt%, 0.38wt%, 0.4wt%, 0.42wt%, 0.44wt%, 0.46wt%, 0.48wt%, 0.5wt%, 0.52wt%, 0.54wt%, 0.56wt%, 0.58wt% or 0.6wt%; the mass fraction of antimony can be 0.15wt%, 0.16wt%, 0.17wt%, 0.18wt%, 0.19wt%, 0.2wt%, 0.21wt%, 0.22wt%, 0.23wt%, 0.24wt%, 0.25wt%, 0.26wt%, 0.27wt%, 0.28wt%, 0.29wt% or 0.3wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] In some optional examples, the particle size D90 of the primary inoculant is 8 to 10 mm, for example, it can be 8.0 mm, 8.2 mm, 8.4 mm, 8.6 mm, 8.8 mm, 9.0 mm, 9.2 mm, 9.4 mm, 9.6 mm, 9.8 mm or 10.0 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] In some optional examples, the mass ratio of the secondary inoculant to the refined melt is (0.03~0.05):100, for example, it can be 0.03:100, 0.032:100, 0.034:100, 0.036:100, 0.038:100, 0.04:100, 0.042:100, 0.044:100, 0.046:100, 0.048:100 or 0.05:100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] In some optional examples, based on the mass fraction of the secondary inoculant being 100wt%, it is composed of the following elements in mass fractions: 50-60wt% silicon, 8-15wt% barium, 10-20wt% calcium, 2-3wt% aluminum, 6-10wt% cerium and 5-9wt% strontium, and the balance is iron; wherein the mass fraction of silicon can be 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, 55wt%, 56wt%, 57wt%, 58wt%, 59wt% or 60wt%; the mass fraction of barium can be 8.0wt%, 8.5wt%, 9.0wt%, 9.5wt%, 10.0wt%, 10.5wt%, 11.0wt%, 11.5wt%, 12.0wt%, 12.5wt%, 13.0wt%, 13.5wt%, 14.0wt%, 14.5wt% or 15.0wt%; the mass fraction of calcium can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt% %, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%; the mass fraction of aluminum can be 2.0wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt% or 3.0wt%; the mass fraction of cerium can be 6.0wt%, 6.5wt%, 7.0wt%, 7.5wt%, 8.0wt%, 8.5wt%, 9.0wt%, 9.5wt% or 10.0wt%; the mass fraction of strontium can be 5.0wt%, 5.5wt%, 6.0wt%, 6.5wt%, 7.0wt%, 7.5wt%, 8.0wt%, 8.5wt% or 9.0wt%, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0043] The present invention adds elements such as silicon, barium, calcium, aluminum, cerium and strontium to the secondary inoculant, wherein silicon, calcium and aluminum react with oxygen, nitrogen and the like in the refined solution to form compounds with high melting points, becoming the core of graphite crystallization, and can effectively promote the graphitization of carbon; in addition, after adding silicon, calcium and aluminum, local silicon-rich micro-regions, calcium-rich micro-regions and aluminum-rich micro-regions will be formed in the refined solution, which is conducive to the precipitation of graphite. The addition of barium can effectively inhibit the decline of inoculation and ensure the effect of inoculation. The addition of rare earth elements such as cerium and strontium can improve the tensile strength of flange castings and inhibit the whitening of flange castings; in addition, the addition of strontium can assist silicon, calcium and aluminum in graphitizing the refined solution, inhibit the whitening of flange castings, and has a strong graphitization ability.
[0044] In some optional examples, the particle size D90 of the secondary inoculant is 1~3mm, for example, it can be 1mm, 1.2mm, 1.4mm, 1.6mm, 1.8mm, 2.0mm, 2.2mm, 2.4mm, 2.6mm, 2.8mm or 3.0mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0045] In some optional instances, the outlet temperature of the refined molten metal in the smelting furnace before it is rushed into the ladle is controlled at 1500-1520°C, for example, it can be 1500°C, 1502°C, 1504°C, 1506°C, 1508°C, 1510°C, 1512°C, 1514°C, 1516°C, 1518°C or 1520°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0046] In some optional examples, the ultrasonic probe extends to 80 to 100 mm below the liquid surface of the refined melt, for example, it can be 80 mm, 82 mm, 84 mm, 86 mm, 88 mm, 90 mm, 92 mm, 94 mm, 96 mm, 98 mm or 100 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] In some optional instances, the transmission power of the ultrasonic probe is 1000~1200W, for example, it can be 1000W, 1020W, 1040W, 1060W, 1080W, 1100W, 1120W, 1140W, 1160W, 1180W or 1200W, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0048] In some optional instances, the ultrasonic frequency emitted by the ultrasonic probe is 20~30kHz, for example, it can be 20kHz, 21kHz, 22kHz, 23kHz, 24kHz, 25kHz, 26kHz, 27kHz, 28kHz, 29kHz or 30kHz, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] In some optional examples, the ultrasonic treatment time is 1 to 3 minutes, for example, it can be 1.0 min, 1.2 min, 1.4 min, 1.6 min, 1.8 min, 2.0 min, 2.2 min, 2.4 min, 2.6 min, 2.8 min or 3.0 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0050] As a preferred technical solution of the present invention, in step S4, the mold is preheated to 500-600°C, for example, it can be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0051] In some optional instances, the casting temperature is 1380~1400℃, for example, it can be 1380℃, 1382℃, 1384℃, 1386℃, 1388℃, 1390℃, 1392℃, 1394℃, 1396℃, 1398℃ or 1400℃, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0052] In some optional examples, the mass ratio of the tertiary inoculant to the refined melt is (0.1~0.15):100, for example, it can be 0.1:100, 0.105:100, 0.11:100, 0.115:100, 0.12:100, 0.125:100, 0.13:100, 0.135:100, 0.14:100, 0.145:100 or 0.15:100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0053] In some optional examples, based on the mass fraction of the tertiary inoculant being 100wt%, it is composed of the following elements in mass fraction: Silicon 65-75wt%, calcium 10-20wt%, aluminum 2-3wt% and bismuth 0.01-0.015wt%, the balance is iron; wherein the mass fraction of silicon can be 65wt%, 66wt%, 67wt%, 68wt%, 69wt%, 70wt%, 71wt%, 72wt%, 73wt%, 74wt% or 75wt%; the mass fraction of calcium can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%; the mass fraction of aluminum can be 2.0wt% %, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt% or 3.0wt%; the mass fraction of bismuth can be 0.01wt%, 0.0105wt%, 0.011wt%, 0.0115wt%, 0.012wt%, 0.0125wt%, 0.013wt%, 0.0135wt%, 0.014wt%, 0.0145wt% or 0.015wt%, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0054] The present invention adds bismuth element to the tertiary inoculant, which is beneficial to improve the roundness of graphite balls, can reduce the diameter of graphite balls, increase the number of graphite balls, and make the distribution of graphite balls more uniform. This is because, on the one hand, during the solidification and crystallization process of the casting liquid, bismuth can be adsorbed on each crystal face of the graphite crystal to form interface adsorption, reduce the surface free energy of the graphite crystal, inhibit the single growth of the graphite crystal, and make the growth rate of each crystal face of the graphite crystal tend to be consistent, which is conducive to forming a spherical structure with a more rounded shape. At the same time, since bismuth forms an enveloping layer around the graphite crystal, the diffusion of carbon atoms is slowed down, so the diameter of the graphite ball can be reduced. On the other hand, bismuth can play a certain inoculation role, can hinder the diffusion of silicon, thereby strengthening the long-term existence of the carbon-rich zone, can enhance the concentration fluctuations and energy fluctuations of carbon and silicon in the casting liquid, so that the graphite crystals in the casting liquid can be maintained, thereby increasing the tendency of graphite homogeneity and heterogeneous core formation, promoting the formation of graphite heterogeneous nucleation, and reducing the possibility of block graphite formation. However, excessive bismuth will also hinder graphitization. Therefore, the present invention specifically limits the mass fraction of bismuth to 0.01-0.015wt%.
[0055] In some optional examples, the particle size D90 of the tertiary inoculant is 0.2~0.6mm, for example, it can be 0.2mm, 0.25mm, 0.3mm, 0.35mm, 0.4mm, 0.45mm, 0.5mm, 0.55mm or 0.6mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0056] In some optional instances, the first cooling temperature is 1100~1200℃, for example, it can be 1100℃, 1110℃, 1120℃, 1130℃, 1140℃, 1150℃, 1160℃, 1170℃, 1180℃, 1190℃ or 1200℃, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0057] In some optional instances, after naturally cooling to the first cooling temperature, the cooling rate is adjusted to 1-2°C / min, for example, it can be 1.0°C / min, 1.1°C / min, 1.2°C / min, 1.3°C / min, 1.4°C / min, 1.5°C / min, 1.6°C / min, 1.7°C / min, 1.8°C / min, 1.9°C / min or 2.0°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0058] In some optional instances, the ultrasonic power of the ultrasonic vibration is 700~800W, for example, it can be 700W, 710W, 720W, 730W, 740W, 750W, 760W, 770W, 780W, 790W or 800W, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0059] In some optional instances, the ultrasonic frequency of the ultrasonic vibration is 10~20kHz, for example, it can be 10kHz, 11kHz, 12kHz, 13kHz, 14kHz, 15kHz, 16kHz, 17kHz, 18kHz, 19kHz or 20kHz, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0060] In some optional instances, the second cooling temperature is 950~1050℃, for example, it can be 950℃, 960℃, 970℃, 980℃, 990℃, 1000℃, 1010℃, 1020℃, 1030℃, 1040℃ or 1050℃, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0061] In some optional embodiments, the second cooling temperature is kept warm for 8 to 12 hours, for example, 8 hours, 8.5 hours, 9 hours, 9.5 hours, 10 hours, 10.5 hours, 11 hours, 11.5 hours or 12 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0062] As a preferred technical solution of the present invention, in step S5, the flange casting is heated to the annealing temperature at a heating rate of 20-30°C / min, for example, it can be 20°C / min, 21°C / min, 22°C / min, 23°C / min, 24°C / min, 25°C / min, 26°C / min, 27°C / min, 28°C / min, 29°C / min or 30°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0063] In some optional instances, the annealing temperature is 1000~1050℃, for example, it can be 1000℃, 1005℃, 1010℃, 1015℃, 1020℃, 1025℃, 1030℃, 1035℃, 1040℃, 1045℃ or 1050℃, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0064] In some optional examples, the annealing temperature is kept for 1.5 to 2.5 hours, for example, 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours, 2.0 hours, 2.1 hours, 2.2 hours, 2.3 hours, 2.4 hours or 2.5 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0065] In some optional examples, the annealing temperature is cooled to the first temperature at a cooling rate of 30-40°C / min, for example, 30°C / min, 31°C / min, 32°C / min, 33°C / min, 34°C / min, 35°C / min, 36°C / min, 37°C / min, 38°C / min, 39°C / min or 40°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0066] In some optional instances, the first temperature is 700-750°C, for example, 700°C, 705°C, 710°C, 715°C, 720°C, 725°C, 730°C, 735°C, 740°C, 745°C or 750°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0067] In some optional instances, the first temperature is kept warm for 30 to 40 minutes, for example, 30 minutes, 31 minutes, 32 minutes, 33 minutes, 34 minutes, 35 minutes, 36 minutes, 37 minutes, 38 minutes, 39 minutes or 40 minutes, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0068] In some optional instances, the temperature is cooled from the first temperature to the second temperature at a cooling rate of 10-20°C / min, for example, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min, 15°C / min, 16°C / min, 17°C / min, 18°C / min, 19°C / min or 20°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0069] In some optional instances, the second temperature is 500-600°C, for example, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0070] In some optional instances, the flange casting after annealing is heated to the normalizing temperature at a heating rate of 8-12°C / min, for example, it can be 8.0°C / min, 8.5°C / min, 9.0°C / min, 9.5°C / min, 10.0°C / min, 10.5°C / min, 11.0°C / min, 11.5°C / min or 12.0°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0071] In some optional instances, the normalizing temperature is 880-900°C, for example, it may be 880°C, 882°C, 884°C, 886°C, 888°C, 890°C, 892°C, 894°C, 896°C, 898°C or 900°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0072] The present invention specifically limits the normalizing temperature to 880-900°C. As the normalizing temperature increases, the spheroidization rate of the graphite spheres in the body flange decreases and flocculent graphite appears, resulting in an irregular graphite shape. This is because during the cooling process, the saturation of carbon in austenite decreases, resulting in the enrichment of carbon atoms in austenite to the surface of the graphite spheres. However, due to the short cooling time of the normalizing process, the carbon atoms cannot be completely enriched on the surface of the graphite spheres, resulting in the appearance of flocculent graphite. In addition, the pearlite content in the matrix increases with the increase of the normalizing temperature. This is because during the heating process, as the normalizing temperature increases, the austenitization degree in the matrix increases, and during the cooling process, the austenite undergoes a eutectic transformation and decomposes into a pearlite structure, thereby increasing the pearlite content in the matrix; in addition, as the normalizing temperature increases, the pearlite lamella spacing in the matrix decreases, which is beneficial to improving the tensile strength of the matrix.
[0073] In some optional examples, the normalizing temperature is kept for 1 to 2 hours, for example, 1.0 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h, 1.5 h, 1.6 h, 1.7 h, 1.8 h, 1.9 h or 2.0 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0074] In some optional instances, the flange casting after normalizing is heated to the quenching temperature at a heating rate of 5 to 10°C / min, for example, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min, 7°C / min, 7.5°C / min, 8°C / min, 8.5°C / min, 9°C / min, 9.5°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0075] In some optional instances, the quenching temperature is 840-860°C, for example, it may be 840°C, 842°C, 844°C, 846°C, 848°C, 850°C, 852°C, 854°C, 856°C, 858°C or 860°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0076] In some optional examples, the quenching temperature is kept for 20 to 30 minutes, for example, 20 minutes, 21 minutes, 22 minutes, 23 minutes, 24 minutes, 25 minutes, 26 minutes, 27 minutes, 28 minutes, 29 minutes or 30 minutes, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0077] In some optional instances, the third temperature is 580~600℃, for example, it can be 580℃, 582℃, 584℃, 586℃, 588℃, 590℃, 592℃, 594℃, 596℃, 598℃ or 600℃, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0078] In some optional instances, the preheating temperature of the molten salt is 280-320°C, for example, it can be 282°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C or 320°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0079] In some optional examples, the flange casting is buried in the molten salt for 1 to 2 hours, for example, 1.0h, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2.0, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0080] In some optional instances, the fourth temperature is 260~300℃, for example, it can be 260℃, 265℃, 270℃, 275℃, 280℃, 285℃, 290℃, 295℃ or 300℃, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0081] In some optional instances, the flange casting after quenching is heated to the tempering temperature at a heating rate of 3 to 5°C / min, for example, 3.0°C / min, 3.2°C / min, 3.4°C / min, 3.6°C / min, 3.8°C / min, 4.0°C / min, 4.2°C / min, 4.4°C / min, 4.6°C / min, 4.8°C / min or 5.0°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0082] In some optional instances, the tempering temperature is 530-550°C, for example, it may be 530°C, 532°C, 534°C, 536°C, 538°C, 540°C, 542°C, 544°C, 546°C, 548°C or 550°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0083] In some optional examples, the tempering temperature is kept for 3 to 4 hours, for example, 3.0 hours, 3.1 hours, 3.2 hours, 3.3 hours, 3.4 hours, 3.5 hours, 3.6 hours, 3.7 hours, 3.8 hours, 3.9 hours or 4.0 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0084] As a preferred technical solution of the present invention, in step S6, the carburizing temperature is 800-900°C, for example, it can be 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C or 900°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0085] In some optional examples, the carburizing temperature is kept for 0.5 to 1.5 hours, for example, 0.5 hours, 0.6 hours, 0.7 hours, 0.8 hours, 0.9 hours, 1.0 hours, 1.1 hours, 1.2 hours, 1.3 hours, 1.4 hours or 1.5 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0086] In some optional instances, the co-infiltration temperature is 500~600℃, for example, it can be 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃ or 600℃, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0087] In some optional examples, the mixed gas consists of ammonia, nitrogen and carbon dioxide.
[0088] In some optional examples, taking the total volume fraction of the mixed gas as 100%, the volume fraction of ammonia is 30-40%, for example, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%; the volume fraction of carbon dioxide is 5-8%, and the balance is nitrogen, for example, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8% or 8.0%, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0089] In some optional examples, the amount of the mixed gas introduced is 1000~1500L / h, for example, it can be 1000L / h, 1050L / h, 1100L / h, 1150L / h, 1200L / h, 1250L / h, 1300L / h, 1350L / h, 1400L / h, 1450L / h or 1500L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0090] In some optional instances, the temperature is kept at the co-infiltration temperature for 5 to 8 hours, for example, 5.0h, 5.2h, 5.4h, 5.6h, 5.8h, 6.0h, 6.2h, 6.4h, 6.6h, 6.8h, 7.0h, 7.2h, 7.4h, 7.6h, 7.8h or 8.0h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0091] In some optional instances, the depth of the nitrocarburizing is 10 to 20 μm, for example, it can be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0092] As a preferred technical solution of the present invention, in step S7, the sandblasting medium used in the sandblasting process is brown corundum sand.
[0093] In some optional instances, the particle size D90 of the sandblasting medium is 400-500 μm, for example, 400 μm, 410 μm, 420 μm, 430 μm, 440 μm, 450 μm, 460 μm, 470 μm, 480 μm, 490 μm or 500 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0094] In some optional instances, the blasting pressure of the sandblasting treatment is 0.6~0.8MPa, for example, it can be 0.6MPa, 0.62MPa, 0.64MPa, 0.68MPa, 0.7MPa, 0.72MPa, 0.74MPa, 0.76MPa, 0.78MPa or 0.8MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0095] In some optional examples, the vertical distance between the nozzle and the rough surface of the flange during the sandblasting process is 150~250mm, for example, it can be 150mm, 160mm, 170mm, 180mm, 190mm, 200mm, 210mm, 220mm, 230mm, 240mm or 250mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0096] In some optional instances, the angle between the axis of the nozzle and the rough surface of the flange during the sandblasting process is 20~30°, for example, it can be 20°, 21°, 22°, 23°, 24°, 25°, 26°, 27°, 28°, 29° or 30°, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0097] In some optional instances, the surface roughness of the flange rough product formed after sandblasting is 50~60μm, for example, it can be 50μm, 51μm, 52μm, 53μm, 54μm, 55μm, 56μm, 57μm, 58μm, 59μm or 60μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0098] As a preferred technical solution of the present invention, in step S8, the mass ratio of the anhydrous ethanol to the binder is (10~20):1, for example, it can be 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1 or 20:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0099] In some optional examples, the ratio of the cladding material to the binder solution is 1g:(0.2~0.3)mL, for example, it can be 1g:0.2mL, 1g:0.21mL, 1g:0.22mL, 1g:0.23mL, 1g:0.24mL, 1g:0.25mL, 1g:0.26mL, 1g:0.27mL, 1g:0.28mL, 1g:0.29mL or 1g:0.3mL, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0100] In some optional examples, taking the mass fraction of the cladding material as 100wt%, it is composed of the following components in mass fractions: Cerium dioxide 0.5~1wt%; Tungsten carbide 30~40wt%; The balance is nickel-based alloy powder.
[0101] Among them, the mass fraction of cerium dioxide can be 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt% or 1wt%; the mass fraction of tungsten carbide can be 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt% or 40wt%, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0102] The present invention specifically limits the addition amount of cerium dioxide to 0.5-1wt%. As the addition amount of cerium dioxide increases, the number of tungsten carbide particles in the cladding layer decreases, and the number of tungsten carbide particles at the edge of the cladding layer also decreases. The tungsten carbide particles are mainly concentrated in the middle of the cladding layer and close to the rough flange. When the addition amount of cerium dioxide is less than 0.5wt%, the tungsten carbide particles in the cladding layer are in a dispersed distribution state. Since the thickness of the edge where the cladding layer and the rough flange meet is thin and the heat dissipation is fast, the tungsten carbide particles gather at the edge of the cladding layer. When the addition amount of cerium dioxide reaches 0.5wt%, the overall number of tungsten carbide particles decreases, and the number of tungsten carbide particles at the edge of the cladding layer also decreases; in addition, with the increase of the addition amount of cerium dioxide, the size of the tungsten carbide particles in the cladding layer also decreases significantly. This is because cerium dioxide is easily concentrated at the grain boundary or phase interface, which reduces the melting point of the alloy system. As a result, the cerium dioxide concentrated at the interface of the tungsten carbide particles accelerates the melting of the tungsten carbide particles and the refinement of the cladding layer, forming fine granular and rod-shaped dendrites, and the distribution of dendrites in the cladding layer is relatively uniform, making the organizational structure of the cladding layer more compact. In addition, after adding cerium dioxide, the number of pores in the cladding layer is significantly reduced, and the crack situation is also improved.
[0103] In some optional examples, based on the mass fraction of the nickel-based alloy powder being 100wt%, it is composed of the following elements in mass fraction: Chromium 15-20wt%, iron 4-6wt%, silicon 3-5wt%, boron 3-4wt% and carbon 0.5-1wt%, the balance is nickel; The mass fraction of chromium can be 15wt%, 15.5wt%, 16wt%, 16.5wt%, 17wt%, 17.5wt%, 18wt%, 18.5wt%, 19wt%, 19.5wt% or 20wt%; the mass fraction of iron can be 4.0wt%, 4.2wt%, 4.4wt%, 4.6wt%, 4.8wt%, 5.0wt%, 5.2wt%, 5.4wt%, 5.6wt%, 5.8wt% or 6.0wt%; the mass fraction of silicon can be 3.0wt%, 3.2wt%, 3.4wt%, 3.6wt%, 3.8wt%, 4.0wt%, 4.2wt%, 4 .4wt%, 4.6wt%, 4.8wt% or 5.0wt%; the mass fraction of boron can be 3.0wt%, 3.1wt%, 3.2wt%, 3.3wt%, 3.4wt%, 3.5wt%, 3.6wt%, 3.7wt%, 3.8wt%, 3.9wt% or 4.0wt%; the mass fraction of carbon can be 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt% or 1wt%, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0104] In some optional instances, the laser spot diameter used in the laser cladding process is 3~4mm, for example, it can be 3.0mm, 3.1mm, 3.2mm, 3.3mm, 3.4mm, 3.5mm, 3.6mm, 3.7mm, 3.8mm, 3.9mm or 4.0mm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0105] In some optional instances, the laser power used in the laser cladding process is 1000~1200W, for example, it can be 1000W, 1020W, 1040W, 1060W, 1080W, 1100W, 1120W, 1140W, 1160W, 1180W or 1200W, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0106] The present invention specifically limits the laser power used in the laser cladding process to 1000~1200W. The structure of the cladding layer tends to become gradually coarser with the increase of laser power. When the laser power exceeds 1200W, the energy obtained by the molten pool is too high and the cooling rate of the molten pool is too low, which leads to a decrease in the supercooling degree of the molten pool and the nucleation rate in the molten pool during crystallization, and the dendrite structure becomes coarse, thereby affecting the mechanical properties and wear resistance of the cladding layer.
[0107] In some optional instances, the laser scanning speed used in the laser cladding process is 2~4mm / s, for example, it can be 2.0mm / s, 2.2mm / s, 2.4mm / s, 2.6mm / s, 2.8mm / s, 3.0mm / s, 3.2mm / s, 3.4mm / s, 3.6mm / s, 3.8mm / s or 4.0mm / s, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0108] The present invention specifically limits the laser scanning speed used in the laser cladding process to 2-4 mm / s. As the scanning speed increases, the energy obtained by the cladding slurry layer during laser cladding decreases, the cooling rate of the molten pool increases, the supercooling degree increases during crystallization, the nucleation rate increases, the number of crystal nuclei in the molten pool increases, the dendrites tend to be small, and the structure of the cladding layer is refined. In addition, as the scanning speed increases, the average wear volume of the cladding layer gradually decreases, and the average wear rate of the cladding layer gradually decreases, which helps to improve the wear resistance of the cladding layer.
[0109] In some optional examples, the thickness of the cladding layer is 0.5~1.5 mm, for example, it can be 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm or 1.5 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0110] In a second aspect, the present invention provides a body flange prepared according to the production method described in the first aspect.
[0111] Compared with the prior art, the present invention has the following beneficial effects: The present invention optimizes and modifies the production process of ductile iron materials for body flanges, combines the raw material mixture smelting and refining process, ultrasonic-assisted spheroidizing inoculation process, isothermal heat treatment process, ultrasonic-assisted casting process, carbonitriding process and cladding wear-resistant coating process, and develops and produces ductile iron materials with excellent mechanical properties and wear resistance. Using the ductile iron materials for the production of body flanges can greatly improve the performance of the body flanges at room temperature, and can fully meet the requirements for strength, toughness and wear performance of the body flanges in the high-temperature and high-pressure pipeline use environment.
[0112] The present invention applies ultrasonic treatment during both the spheroidization inoculation and the casting process, wherein, during the spheroidization inoculation process, the ultrasonic probe is inserted into the refined molten liquid to directly perform ultrasonic treatment on the refined molten liquid; during the casting process, the ultrasonic probe is contacted with the mold to indirectly perform ultrasonic treatment on the casting liquid. By performing ultrasonic treatment during the spheroidization inoculation process, the number of graphite balls is increased and the matrix structure is refined; by performing ultrasonic treatment during the casting process, the growth morphology of the graphite balls is uniform and the roundness of the graphite balls is improved. Through the synergistic effect of ultrasonic treatment at different production stages, the comprehensive mechanical properties of the flange casting, such as tensile strength and hardness, can be greatly improved.
[0113] The present invention directly performs ultrasonic treatment on the refined molten liquid through an ultrasonic probe during the spheroidization inoculation process. The high ultrasonic energy generates a negative pressure zone in the local micro-region of the refined molten liquid during the propagation process. When the ultrasonic energy exceeds the surface tension of the refined molten liquid, the refined molten liquid is torn apart to generate a large number of small bubbles. As the ultrasonic time passes, the small bubbles gradually accumulate and grow to form large bubbles. When the pressure in the large bubbles reaches the critical point, they will instantly break and split into more small bubbles. The small bubbles after the splitting will continue to accumulate, grow, break and split repeatedly. When the large bubbles break rapidly, instantaneous high pressure will be generated in the large bubbles. At the same time, the refined molten liquid around the large bubbles will also instantly rush into the bubbles, causing the refined molten liquid near the bubbles to produce strong local vibrations. As the small bubbles continue to accumulate, grow, break and split repeatedly, a cyclic cavitation effect is formed. The impact force generated by each bubble break can strongly flush the dendrites, improve the nucleation rate, and is conducive to the formation of equiaxed crystals. At the same time, the spacing of the secondary dendrites is also reduced, so that the carbides are broken, so that the matrix structure of the flange casting can be refined. In addition, the thermal effect of ultrasound causes the temperature of the refined melt near the ultrasonic probe to increase while the cooling rate to decrease. The high-temperature refined melt is conducive to the growth of graphite nodules. Therefore, the present invention significantly increases the number of graphite nodules by ultrasonically treating the refined melt during the spheroidization inoculation process.
[0114] The invention adopts a specially formulated inoculant, and adopts different inoculants in the processes of ladle inoculation, flushing inoculation and casting inoculation to meet the inoculation requirements of different processing stages, so that the processed body flange has higher strength and better wear resistance; during the ladle inoculation, the first inoculant is laid in layers, and the inoculation effect can be improved after the refined solution is flushed into the molten iron ladle; during the inoculation process, ultrasonic vibration is applied to the refined solution, which is beneficial to increase the number of graphite cores and the roundness of graphite balls, thereby improving the strength of the body flange; casting inoculation is performed after the ladle inoculation, so that the inoculation effect can be prolonged.
[0115] The present invention indirectly performs ultrasonic treatment on the casting liquid through an ultrasonic probe during the casting process, and the cooling rate of the casting liquid in the mold is slowed down through the acoustic cavitation effect and thermal effect of the ultrasonic wave, so that the carbon-poor area and the carbon-rich area in the casting liquid can fully diffuse to achieve carbon balance, which is beneficial to reduce the area of the carbon-poor area around the graphite ball. During the cooling and solidification process of the casting liquid, the graphite ball can grow freely in the casting liquid without being constrained and limited by the space of the carbon-poor area. Therefore, the graphite balls in the flange casting finally formed are uniform in size and have a high roundness, which is beneficial to further improve the comprehensive mechanical properties of the flange casting.
[0116] The present invention adopts two-stage cooling in the casting process, which improves the uniformity of the components of the flange casting and is conducive to further improving the comprehensive mechanical properties of the flange casting. When the casting liquid obtained after refining is naturally cooled from the casting temperature to the first cooling temperature, a solid phase begins to be generated in the casting liquid, and the preferential growth of grains begins inside the casting liquid. At this time, adjusting the cooling rate of the mold and performing ultrasonic vibration treatment at the same time can improve the uniformity of the components inside the casting liquid, promote grain refinement, and greatly enhance the fine grain strengthening effect inside the flange casting; when the mold is reduced to the second cooling temperature, the solute inside the flange casting can be fully diffused through long-term heat preservation, reducing the possibility of segregation inside the flange casting, and further enhancing the comprehensive mechanical properties of the flange casting.
[0117] Since the present invention adds nickel, molybdenum, vanadium and other whitening elements to the raw material mixture of the main flange, the whitening elements have the ability to bind carbon atoms during the casting process, which will slow down the diffusion rate of carbon atoms into the graphite balls; and the added nickel element has the function of stabilizing austenite, therefore, the edge of the flange casting obtained after casting has a whitening tendency, and there are a large number of large-sized primary cementites, which leads to the reduction of the comprehensive mechanical properties of the main flange. Therefore, in order to ensure that the main flange has sufficient tensile strength to improve the actual plasticity, obtain high strength and toughness, and at the same time cannot reduce its tensile strength, the present invention heat treats the flange casting to eliminate free cementite as much as possible, and homogenizes the metallographic structure and internal composition of the flange casting. In this way, the mechanical properties of the flange casting are improved.
[0118] The present invention adopts a high-temperature and low-temperature two-stage annealing process to decompose the pearlite in the matrix structure, and transforms the matrix structure composed of ferrite, pearlite, graphite nodules and tiny graphite particles into a matrix structure composed of ferrite, graphite nodules and tiny graphite particles. The two-stage annealing process can change the matrix structure, thereby improving the mechanical properties of the body flange.
[0119] The present invention adopts a gas carbonitriding process, a flange green body is placed in a reaction furnace, a gas medium containing carbon atoms and nitrogen atoms is introduced into the furnace, and during the high-temperature heating process, carbon atoms and nitrogen atoms diffuse on the surface of the flange green body and are absorbed by the surface of the flange green body into the interior, thereby forming a carbonitriding layer with a certain thickness, which can achieve both the carburizing depth and the nitriding hardness, so that many properties of the flange green body, such as toughness, hardness and wear resistance, are significantly improved.
[0120] The present invention forms a cladding layer on the surface of the rough flange product after sandblasting by laser cladding technology. By setting the cladding layer on the surface of the rough flange product, the strength and hardness of the main flange surface can be significantly improved, and the wear resistance of the main flange surface can be improved. The cladding layer includes nickel-based alloy powder, cerium dioxide and tungsten carbide. The laser cladding technology makes the tungsten carbide particles in the cladding layer dispersed in the nickel-based alloy powder without grain boundary segregation. Therefore, by adding tungsten carbide particles of hard phase, the high-temperature wear resistance and hardness of the cladding layer can be significantly improved; in addition, since tungsten carbide has high-temperature stability, it has little effect on the microstructure and metallographic structure of the cladding layer. The addition of cerium dioxide particles can accelerate the dissolution of cerium dioxide particles and promote the improvement of their shape. At the same time, the cerium dioxide particles are dispersed and filled in the nickel-based alloy powder, so that the laser energy can be smoothly transmitted along the nickel-based alloy powder, thereby accelerating the melting rate of the nickel-based alloy powder, so that the nickel-based alloy powder can be quickly melted, solidified and crystallized, which has a refinement effect on the metallographic structure of the cladding layer, can effectively reduce defects such as cracks and holes in the cladding layer, and is conducive to the formation of a cladding layer with a denser metallographic structure, thereby improving the comprehensive mechanical properties of the cladding layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0121] Figure 1 A production process flow chart of a body flange provided in Example 11 of the embodiment of the present invention; Figure 2 This is a metallographic micrograph of the flange green body prepared in Example 1 of the present invention; Figure 3 This is a graphite metallographic micrograph of the flange green body prepared in Example 1 of the present invention; Figure 4 This is a metallographic micrograph of the base of the flange green body prepared in Comparative Example 1 of the present invention; Figure 5 This is a graphite metallographic micrograph of the flange green body prepared in Comparative Example 1 of the present invention; Figure 6 This is a metallographic micrograph of the flange green body prepared in Comparative Example 2 of the present invention; Figure 7 This is a graphite metallographic micrograph of the flange green body prepared in Comparative Example 2 of the present invention; Figure 8 This is a metallographic micrograph of the base of the flange green body prepared in Comparative Example 3 of the present invention; Fig. 9 This is a graphite metallographic micrograph of the flange green body prepared in Comparative Example 3 of the present invention; Fig.10 This is an optical micrograph of the cladding layer on the surface of the body flange prepared in Example 1 of the present invention; Fig.11 This is an optical micrograph of the cladding layer on the surface of the body flange prepared in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0122] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and their accompanying drawings. The embodiments recorded herein are specific embodiments of the present invention, which are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limitations on the embodiments of the present invention and the scope of protection of the present invention. In addition to the embodiments recorded herein, those skilled in the art can also adopt other obvious technical solutions based on the contents disclosed in the claims of this application and its specification, including technical solutions that adopt any obvious replacements and modifications to the embodiments recorded herein.
[0123] Example 1 This embodiment provides a method for producing a body flange, such as Figure 1 As shown, the production method specifically comprises the following steps: S1. Alloy smelting: putting the raw material mixture into a smelting furnace, heating the raw material mixture to 1450°C and keeping it warm for 2 hours to obtain an alloy melt; The raw material mixture is composed of the following elements in the following mass fractions, based on the mass fraction of the raw material mixture being 100wt%: 3.5wt% carbon, 2.5wt% silicon, 0.3wt% manganese, 0.2wt% nickel, 0.3wt% molybdenum and 0.5wt% vanadium, with the remainder being iron; S2. Refining and purification: The temperature of the alloy melt is adjusted to 1520°C, and a purifier is added to the alloy melt. The purifier is composed of calcium oxide and aluminum oxide in a mass ratio of 1:1, and the mass ratio of the purifier to the alloy melt is 0.4:100. The temperature is kept for 60 minutes to complete the refining and purification. Then, 1.5MPa nitrogen is continuously introduced into the smelting furnace, and the nitrogen introduction amount is 100Nm 3 / h, the feeding time is 20min, and the refined melt is obtained after removing the scum on the liquid surface; S3, spheroidizing inoculation: placing a spheroidizing agent with a particle size D90 of 10 mm on one side of the bottom dam of the ladle, and compacting and tamping to form a spheroidizing agent layer; wherein the mass ratio of the spheroidizing agent to the refined molten metal is 1.5:100; and based on the mass fraction of the spheroidizing agent being 100wt%, it is composed of the following mass fractions of each element: 40wt% of silicon, 7.5wt% of magnesium, 4wt% of manganese, 2wt% of calcium, 1.2wt% of yttrium, 0.4wt% of cerium, 0.5wt% of lanthanum, 0.4wt% of neodymium, 0.1wt% of aluminum and 0.5wt% of titanium, and the balance is iron; A primary inoculant composed of silicon-calcium-barium alloy and silicon carbide is evenly spread on the surface of the spheroidizer layer, and after compaction, a primary inoculant layer covering the surface of the spheroidizer layer is formed; wherein the particle size D90 of the silicon-calcium-barium alloy and the silicon carbide are both 8 mm, the mass ratio of the silicon-calcium-barium alloy to the refined melt is 0.2:100, and the mass ratio of the silicon carbide to the refined melt is 0.2:100; based on the mass fraction of the silicon-calcium-barium alloy being 100wt%, it is composed of the following mass fractions of the elements: 40wt% silicon, 15wt% calcium, 12wt% barium, 0.3wt% zirconium and 0.3wt% antimony, and the balance is iron; Perlite and iron plates are sequentially stacked on the surface of the primary inoculant layer, the outlet temperature of the refined molten metal in the smelting furnace is controlled at 1500°C, and then the refined molten metal is poured into the ladle from the side of the bottom dam of the ladle where the spheroidizer layer and the primary inoculant layer are not placed; in the process of pouring the refined molten metal, a secondary inoculant with a particle size D90 of 1 mm is added along the flow, and the mass ratio of the secondary inoculant to the refined molten metal is 0.03:100; based on the mass fraction of the secondary inoculant being 100wt%, it is composed of the following mass fractions of each element: 50wt% of silicon, 15wt% of barium, 10wt% of calcium, 2wt% of aluminum, 10wt% of cerium and 5wt% of strontium, and the balance is iron; After all the refined molten metal in the smelting furnace is flushed into the ladle, an ultrasonic probe is extended from above the refined molten metal to 80 mm below the liquid surface of the refined molten metal, and 1000 W ultrasonic waves are applied to the refined molten metal. The ultrasonic frequency is 20 kHz, and the ultrasonic treatment time is 3 min. After ultrasonic treatment, a casting liquid is obtained; S4, casting: preheat the mold to 500°C in advance, when the temperature of the casting liquid reaches 1380°C, inject the casting liquid in the molten iron ladle into the preheated mold, add a tertiary inoculant with a particle size D90 of 0.2 mm during the pouring of the casting liquid, and the mass ratio of the tertiary inoculant to the refined molten liquid is 0.1:100; Taking the mass fraction of the tertiary inoculant as 100wt%, it is composed of the following elements in mass fractions: 65wt% silicon, 20wt% calcium, 2wt% aluminum and 0.01wt% bismuth, and the balance is iron; After all the casting liquid is injected into the mold, it is naturally cooled to 1100°C, and then the cooling rate is adjusted to 1°C / min. The mold after casting is subjected to ultrasonic vibration, and the ultrasonic power used is 700W and the ultrasonic frequency is 10kHz. When the mold is cooled to 950°C, the ultrasonic vibration is stopped and kept warm for 12 hours, and then naturally cooled to room temperature. After demolding, the flange casting is obtained; S5. Quenching and tempering heat treatment: the flange casting after casting is subjected to annealing, normalizing, quenching and tempering treatments in sequence; First, the flange casting after casting was heated to 1000℃ at a heating rate of 20℃ / min and kept at this temperature for 2.5h, then quickly cooled to 700℃ at a cooling rate of 30℃ / min and kept at this temperature for 40min, then slowly cooled to 500℃ at a cooling rate of 10℃ / min, and air-cooled to room temperature after being taken out of the furnace to complete the annealing treatment; Then, the flange casting after annealing treatment was heated to 880°C at a heating rate of 8°C / min and kept at this temperature for 2h, and then taken out of the furnace and air-cooled to room temperature to complete the normalizing treatment; Then, the flange casting after normalizing treatment is heated to 840°C at a heating rate of 5°C / min and kept warm for 30 minutes. After the end of the heat preservation, it is cooled to 580°C with the furnace. Then, the flange casting is taken out and immediately buried in molten salt at 280°C. It is kept warm in the molten salt for 2 hours. When the surface temperature of the flange casting drops to 260°C, the flange casting is taken out from the molten salt and air-cooled to room temperature to complete the quenching treatment. Finally, the flange casting after quenching treatment was heated to 530°C at a heating rate of 3°C / min and kept at this temperature for 4 hours, and then air-cooled to room temperature in the furnace to complete the tempering treatment and obtain the flange green body; S6. Nitrocarburizing: carbon dioxide is introduced into the reactor, the flange green body is placed in the reactor, the flange green body is heated to 800°C and kept warm for 1.5 hours for carburizing treatment; argon is introduced into the reactor to cool the flange green body, and after the flange green body is cooled to 500°C, a mixed gas consisting of ammonia, nitrogen and carbon dioxide is introduced into the reactor, and the amount of the mixed gas introduced is 1000L / h; based on the total volume fraction of the mixed gas being 100%, the volume fraction of ammonia is 30%, the volume fraction of carbon dioxide is 5%, and the remainder is nitrogen; after keeping warm for 5 hours, the nitrocarburizing treatment is completed, the depth of nitrocarburizing is 10μm, and a flange rough product is obtained; S7, sandblasting roughening: the flange rough product is sandblasted with brown corundum sand with a particle size D90 of 400 μm, the sandblasting pressure is 0.6 MPa, the vertical distance between the nozzle and the surface of the flange rough product is 150 mm, the angle between the axis of the nozzle and the surface of the flange rough product is 20°, and the surface roughness of the flange rough product formed after sandblasting is 50 μm; then the flange rough product after sandblasting is placed in a mixed solvent of anhydrous ethanol and acetone for ultrasonic cleaning, and taken out and dried after cleaning; S8, coating cladding: anhydrous ethanol and a binder are mixed in a mass ratio of 10:1 to prepare a binder solution, and the cladding material and the binder solution are mixed in a ratio of 1g:0.2mL to prepare a paste-like cladding slurry; Taking the mass fraction of the cladding material as 100wt%, it is composed of the following components in mass fractions: 0.5wt% cerium dioxide, 30wt% tungsten carbide, and the balance nickel-based alloy powder; The nickel-based alloy powder is composed of the following elements in the following mass fractions, based on a mass fraction of 100wt%: 15wt% chromium, 6wt% iron, 3wt% silicon, 4wt% boron and 0.5wt% carbon, with the remainder being nickel; The cladding slurry is evenly coated on the rough surface of the flange after sandblasting, and a cladding slurry layer is formed after drying; the cladding slurry layer is laser clad by a laser, and the process parameters of the laser cladding are: the laser spot diameter is 3mm, the laser power is 1000W, and the laser scanning speed is 2mm / s. After cooling, a cladding layer with a thickness of 0.5mm is formed on the surface of the rough flange to obtain the main body flange.
[0124] The graphite metallographic structure and matrix metallographic structure of the flange green body prepared in this embodiment were observed using a metallographic microscope, and the following results were obtained: Figure 1 and Figure 2 From the metallographic micrograph shown, it can be seen that the number of graphite nodules in the flange green body is large and the size is small.
[0125] The cladding layer on the surface of the body flange prepared in this embodiment was observed using an optical microscope, and the following results were obtained: Fig.10 As shown in the optical micrograph, it can be seen that there are almost no defects such as cracks and holes in the cladding layer.
[0126] Example 2 This embodiment provides a method for producing a body flange, such as Figure 1 As shown, the production method specifically comprises the following steps: S1. Alloy smelting: putting the raw material mixture into a smelting furnace, heating the raw material mixture to 1452°C and keeping it warm for 1.8 hours to obtain an alloy melt; Based on the mass fraction of the raw material mixture being 100wt%, it is composed of the following elements in mass fractions: 3.55wt% carbon, 2.3wt% silicon, 0.4wt% manganese, 0.18wt% nickel, 0.32wt% molybdenum and 0.4wt% vanadium, and the balance being iron; S2, refining and purification: the temperature of the alloy melt is adjusted to 1525 ° C, and a purifier is added to the alloy melt, the purifier is composed of calcium oxide and aluminum oxide in a mass ratio of 1:1, and the mass ratio of the purifier to the alloy melt is 0.45:100, and the temperature is kept for 58 minutes to complete the refining and purification; then, 1.6MPa nitrogen is continuously introduced into the smelting furnace, and the nitrogen introduction amount is 110Nm 3 / h, the feeding time is 18min, and the refined melt is obtained after removing the scum on the liquid surface; S3. Spheroidizing inoculation: placing a spheroidizing agent with a particle size D90 of 11 mm on one side of the bottom dam of the ladle, and compacting and tamping to form a spheroidizing agent layer; wherein the mass ratio of the spheroidizing agent to the refined molten metal is 1.8:100; and based on the mass fraction of the spheroidizing agent being 100wt%, it is composed of the following mass fractions of each element: 41wt% of silicon, 7.4wt% of magnesium, 3.8wt% of manganese, 2.2wt% of calcium, 1.3wt% of yttrium, 0.42wt% of cerium, 0.48wt% of lanthanum, 0.42wt% of neodymium, 0.2wt% of aluminum and 0.4wt% of titanium, and the balance is iron; A primary inoculant composed of silicon-calcium-barium alloy and silicon carbide is evenly spread on the surface of the spheroidizer layer, and after compaction, a primary inoculant layer covering the surface of the spheroidizer layer is formed; wherein the particle sizes D90 of the silicon-calcium-barium alloy and silicon carbide are both 8.5 mm, the mass ratio of the silicon-calcium-barium alloy to the refined melt is 0.22:100, and the mass ratio of silicon carbide to the refined melt is 0.18:100; based on the mass fraction of the silicon-calcium-barium alloy being 100wt%, it is composed of the following elements in mass fractions: 41wt% silicon, 14wt% calcium, 11.2wt% barium, 0.4wt% zirconium and 0.25wt% antimony, and the balance is iron; Perlite and iron plates are sequentially stacked on the surface of the primary inoculant layer, the outlet temperature of the refined molten metal in the smelting furnace is controlled at 1505°C, and then the refined molten metal is poured into the ladle from the side of the bottom dam of the ladle where the spheroidizing agent layer and the primary inoculant layer are not placed; in the process of pouring the refined molten metal, a secondary inoculant with a particle size D90 of 1.5 mm is added along the flow, and the mass ratio of the secondary inoculant to the refined molten metal is 0.035:100; based on the mass fraction of the secondary inoculant being 100wt%, it is composed of the following mass fractions of the elements: 52wt% of silicon, 14wt% of barium, 12wt% of calcium, 2.2wt% of aluminum, 9wt% of cerium and 6wt% of strontium, and the balance is iron; After all the refined molten metal in the smelting furnace is flushed into the ladle, an ultrasonic probe is extended from above the refined molten metal to 85 mm below the liquid surface of the refined molten metal, and 1050 W ultrasonic waves are applied to the refined molten metal. The ultrasonic frequency is 22 kHz, and the ultrasonic treatment time is 2.5 min. After ultrasonic treatment, a casting liquid is obtained; S4, casting: preheat the mold to 520°C in advance, when the temperature of the casting liquid reaches 1385°C, inject the casting liquid in the molten iron ladle into the preheated mold, add a tertiary inoculant with a particle size D90 of 0.3 mm during the pouring of the casting liquid, and the mass ratio of the tertiary inoculant to the refined melt is 0.11:100; Taking the mass fraction of the tertiary inoculant as 100wt%, it is composed of the following elements in mass fractions: 68wt% silicon, 18wt% calcium, 2.2wt% aluminum and 0.011wt% bismuth, and the balance is iron; After all the casting liquid is injected into the mold, it is naturally cooled to 1102°C, and then the cooling rate is adjusted to 1.2°C / min. The mold after casting is subjected to ultrasonic vibration, and the ultrasonic power used is 720W and the ultrasonic frequency is 12kHz. When the mold is cooled to 980°C, the ultrasonic vibration is stopped and kept warm for 11 hours, and then it is naturally cooled to room temperature. After demolding, the flange casting is obtained; S5. Quenching and tempering heat treatment: the flange casting after casting is subjected to annealing, normalizing, quenching and tempering treatments in sequence; First, the flange casting after casting was heated to 1010℃ at a heating rate of 22℃ / min and kept at this temperature for 2.2h, then quickly cooled to 710℃ at a cooling rate of 32℃ / min and kept at this temperature for 38min, then slowly cooled to 520℃ at a cooling rate of 12℃ / min, and air-cooled to room temperature after being taken out of the furnace to complete the annealing treatment; Then, the flange casting after annealing treatment was heated to 882°C at a heating rate of 9°C / min and kept at this temperature for 1.8h, and then taken out of the furnace and air-cooled to room temperature to complete the normalizing treatment; Then, the flange casting after normalizing treatment was heated to 845°C at a heating rate of 6°C / min and kept at this temperature for 28 minutes. After the end of the heat preservation, it was cooled to 585°C with the furnace. Then, the flange casting was taken out and immediately buried in molten salt at 290°C. It was kept in the molten salt for 1.8 hours. When the surface temperature of the flange casting dropped to 270°C, the flange casting was taken out from the molten salt and air-cooled to room temperature to complete the quenching treatment. Finally, the flange casting after quenching treatment was heated to 535°C at a heating rate of 3.5°C / min and kept at this temperature for 3.8h, and then air-cooled to room temperature in the furnace to complete the tempering treatment and obtain the flange green body; S6. Nitrocarburizing: carbon dioxide is introduced into the reactor, the flange green body is placed in the reactor, the flange green body is heated to 820°C and kept warm for 1.2 hours for carburizing treatment; argon is introduced into the reactor to cool the flange green body, and after the flange green body is cooled to 520°C, a mixed gas consisting of ammonia, nitrogen and carbon dioxide is introduced into the reactor, and the amount of the mixed gas introduced is 1100L / h; based on the total volume fraction of the mixed gas being 100%, the volume fraction of ammonia is 32%, the volume fraction of carbon dioxide is 6%, and the remainder is nitrogen; after keeping warm for 6 hours, the nitrocarburizing treatment is completed, the depth of nitrocarburizing is 12μm, and a flange rough product is obtained; S7, sandblasting roughening: the flange rough product is sandblasted with brown corundum sand with a particle size D90 of 420 μm, the sandblasting pressure is 0.65 MPa, the vertical distance between the nozzle and the surface of the flange rough product is 180 mm, the angle between the axis of the nozzle and the surface of the flange rough product is 22°, and the surface roughness of the flange rough product formed after sandblasting is 52 μm; then the flange rough product after sandblasting is placed in a mixed solvent of anhydrous ethanol and acetone for ultrasonic cleaning, and after cleaning, it is taken out and dried; S8, coating cladding: anhydrous ethanol and a binder are mixed in a mass ratio of 12:1 to prepare a binder solution, and the cladding material and the binder solution are mixed in a ratio of 1g:0.22mL to prepare a paste-like cladding slurry; Taking the mass fraction of the cladding material as 100wt%, it is composed of the following components in mass fractions: 0.6wt% of cerium dioxide, 32wt% of tungsten carbide, and the balance of nickel-based alloy powder; The nickel-based alloy powder is composed of the following elements in the following mass fractions, based on a mass fraction of 100 wt %: 16 wt % of chromium, 5.5 wt % of iron, 3.5 wt % of silicon, 3.8 wt % of boron, and 0.6 wt % of carbon, with the remainder being nickel. The cladding slurry is evenly coated on the rough surface of the flange after sandblasting, and a cladding slurry layer is formed after drying; the cladding slurry layer is laser clad by a laser, and the process parameters of the laser cladding are: the laser spot diameter is 3.2 mm, the laser power is 1050 W, and the laser scanning speed is 2.5 mm / s. After cooling, a cladding layer with a thickness of 0.8 mm is formed on the surface of the rough flange to obtain the main body flange.
[0127] Example 3 This embodiment provides a method for producing a body flange, such as Figure 1 As shown, the production method specifically comprises the following steps: S1. Alloy smelting: putting the raw material mixture into a smelting furnace, heating the raw material mixture to 1455°C and keeping it warm for 1.5 hours to obtain an alloy melt; Based on the mass fraction of the raw material mixture being 100wt%, it is composed of the following mass fractions of each element: 3.6wt% carbon, 2.2wt% silicon, 0.45wt% manganese, 0.15wt% nickel, 0.35wt% molybdenum and 0.3wt% vanadium, and the balance being iron; S2, refining and purification: the temperature of the alloy melt is adjusted to 1530 ° C, and a purifier is added to the alloy melt, the purifier is composed of calcium oxide and aluminum oxide in a mass ratio of 1:1, and the mass ratio of the purifier to the alloy melt is 0.5:100, and the temperature is kept for 55 minutes to complete the refining and purification; then, 1.6MPa nitrogen is continuously introduced into the smelting furnace, and the nitrogen introduction amount is 120Nm 3 / h, the feeding time is 15min, and the refined melt is obtained after removing the scum on the liquid surface; S3. Spheroidizing inoculation: placing a spheroidizing agent with a particle size D90 of 12 mm on one side of the bottom dam of the ladle, and compacting and tamping to form a spheroidizing agent layer; wherein the mass ratio of the spheroidizing agent to the refined molten metal is 2:100; and based on the mass fraction of the spheroidizing agent being 100wt%, it is composed of the following mass fractions of each element: 42wt% of silicon, 7.3wt% of magnesium, 3.5wt% of manganese, 2.5wt% of calcium, 1.3wt% of yttrium, 0.45wt% of cerium, 0.45wt% of lanthanum, 0.45wt% of neodymium, 0.3wt% of aluminum and 0.3wt% of titanium, and the balance being iron; A primary inoculant composed of silicon-calcium-barium alloy and silicon carbide is evenly spread on the surface of the spheroidizer layer, and after compaction, a primary inoculant layer covering the surface of the spheroidizer layer is formed; wherein the particle size D90 of the silicon-calcium-barium alloy and the silicon carbide are both 9 mm, the mass ratio of the silicon-calcium-barium alloy to the refined melt is 0.25:100, and the mass ratio of the silicon carbide to the refined melt is 0.15:100; based on the mass fraction of the silicon-calcium-barium alloy being 100wt%, it is composed of the following mass fractions of the elements: 42wt% silicon, 13wt% calcium, 11wt% barium, 0.4wt% zirconium and 0.2wt% antimony, and the balance is iron; Perlite and iron plates are sequentially stacked on the surface of the primary inoculant layer, the outlet temperature of the refined molten metal in the smelting furnace is controlled at 1510°C, and then the refined molten metal is poured into the ladle from the side of the bottom dam of the ladle where the spheroidizer layer and the primary inoculant layer are not placed; in the process of pouring the refined molten metal, a secondary inoculant with a particle size D90 of 2 mm is added along the flow, and the mass ratio of the secondary inoculant to the refined molten metal is 0.04:100; based on the mass fraction of the secondary inoculant being 100wt%, it is composed of the following mass fractions of each element: 55wt% of silicon, 12wt% of barium, 15wt% of calcium, 2.5wt% of aluminum, 8wt% of cerium and 7wt% of strontium, and the balance is iron; After all the refined molten metal in the smelting furnace is flushed into the ladle, an ultrasonic probe is extended from above the refined molten metal to 90 mm below the liquid surface of the refined molten metal, and 1100 W ultrasonic waves are applied to the refined molten metal. The ultrasonic frequency is 25 kHz, and the ultrasonic treatment time is 2 min. After ultrasonic treatment, a casting liquid is obtained; S4, casting: preheat the mold to 550°C in advance, when the temperature of the casting liquid reaches 1390°C, inject the casting liquid in the molten iron ladle into the preheated mold, add a tertiary inoculant with a particle size D90 of 0.4 mm during the pouring of the casting liquid, and the mass ratio of the tertiary inoculant to the refined melt is 0.12:100; Taking the mass fraction of the tertiary inoculant as 100wt%, it is composed of the following elements in mass fractions: 70wt% silicon, 15wt% calcium, 2.5wt% aluminum and 0.012wt% bismuth, and the balance is iron; After all the casting liquid is injected into the mold, it is naturally cooled to 1105°C, and then the cooling rate is adjusted to 1.5°C / min. The mold after casting is subjected to ultrasonic vibration, and the ultrasonic power used is 750W and the ultrasonic frequency is 15kHz. When the mold is cooled to 1000°C, the ultrasonic vibration is stopped and kept warm for 10 hours, and then naturally cooled to room temperature. After demolding, the flange casting is obtained; S5. Quenching and tempering heat treatment: the flange casting after casting is subjected to annealing, normalizing, quenching and tempering treatments in sequence; First, the flange casting after casting was heated to 1020℃ at a heating rate of 25℃ / min and kept at this temperature for 2h, then quickly cooled to 720℃ at a cooling rate of 35℃ / min and kept at this temperature for 35min, then slowly cooled to 550℃ at a cooling rate of 15℃ / min, and air-cooled to room temperature after being taken out of the furnace to complete the annealing treatment; Then, the flange casting after annealing treatment was heated to 885°C at a heating rate of 10°C / min and kept at this temperature for 1.5h, and then taken out of the furnace and air-cooled to room temperature to complete the normalizing treatment; Then, the flange casting after normalizing treatment is heated to 850°C at a heating rate of 7°C / min and kept at this temperature for 25 minutes. After the end of the heat preservation, it is cooled to 590°C with the furnace. Then, the flange casting is taken out and immediately buried in 300°C molten salt, and kept in the molten salt for 1.5 hours. When the surface temperature of the flange casting drops to 280°C, the flange casting is taken out from the molten salt and air-cooled to room temperature to complete the quenching treatment; Finally, the flange casting after quenching treatment was heated to 540°C at a heating rate of 4°C / min and kept at this temperature for 3.5h, and then air-cooled to room temperature in the furnace to complete the tempering treatment and obtain the flange green body; S6. Nitrocarburizing: carbon dioxide is introduced into the reactor, the flange green body is placed in the reactor, the flange green body is heated to 850°C and kept warm for 1 hour for carburizing treatment; argon is introduced into the reactor to cool the flange green body, and after the flange green body is cooled to 550°C, a mixed gas consisting of ammonia, nitrogen and carbon dioxide is introduced into the reactor, and the amount of the mixed gas introduced is 1200L / h; based on the total volume fraction of the mixed gas being 100%, the volume fraction of ammonia is 35%, the volume fraction of carbon dioxide is 7%, and the remainder is nitrogen; after keeping warm for 7 hours, the nitrocarburizing treatment is completed, the depth of nitrocarburizing is 15μm, and a flange rough product is obtained; S7, sandblasting roughening: the flange rough product is sandblasted with brown corundum sand with a particle size D90 of 450 μm, the sandblasting pressure is 0.7 MPa, the vertical distance between the nozzle and the surface of the flange rough product is 200 mm, the angle between the axis of the nozzle and the surface of the flange rough product is 25°, and the surface roughness of the flange rough product formed after sandblasting is 55 μm; then the flange rough product after sandblasting is placed in a mixed solvent of anhydrous ethanol and acetone for ultrasonic cleaning, and taken out and dried after cleaning; S8, coating cladding: anhydrous ethanol and a binder are mixed in a mass ratio of 15:1 to prepare a binder solution, and the cladding material and the binder solution are mixed in a ratio of 1g:0.25mL to prepare a paste-like cladding slurry; Taking the mass fraction of the cladding material as 100wt%, it is composed of the following components in mass fractions: 0.7wt% cerium dioxide, 35wt% tungsten carbide, and the balance nickel-based alloy powder; The nickel-based alloy powder is composed of the following elements in the following mass fractions, based on a mass fraction of 100 wt %: 17 wt % of chromium, 5 wt % of iron, 4 wt % of silicon, 3.5 wt % of boron, and 0.7 wt % of carbon, with the remainder being nickel. The cladding slurry is evenly coated on the rough surface of the flange after sandblasting, and a cladding slurry layer is formed after drying; the cladding slurry layer is laser clad by a laser, and the process parameters of the laser cladding are: the laser spot diameter is 3.5 mm, the laser power is 1100 W, and the laser scanning speed is 3 mm / s. After cooling, a cladding layer with a thickness of 1 mm is formed on the surface of the rough flange to obtain the main body flange.
[0128] Example 4 This embodiment provides a method for producing a body flange, such as Figure 1 As shown, the production method specifically comprises the following steps: S1. Alloy smelting: putting the raw material mixture into a smelting furnace, heating the raw material mixture to 1458°C and keeping it warm for 1.1 hours to obtain an alloy melt; Based on the mass fraction of the raw material mixture being 100wt%, it is composed of the following elements in mass fractions: 3.65wt% carbon, 2.2wt% silicon, 0.5wt% manganese, 0.12wt% nickel, 0.38wt% molybdenum and 0.3wt% vanadium, and the balance being iron; S2, refining and purification: the temperature of the alloy melt is adjusted to 1535 ° C, and a purifier is added to the alloy melt, the purifier is composed of calcium oxide and aluminum oxide in a mass ratio of 1:1, and the mass ratio of the purifier to the alloy melt is 0.55:100, and the temperature is kept for 52 minutes to complete the refining and purification; then, 1.7MPa nitrogen is continuously introduced into the smelting furnace, and the nitrogen introduction amount is 130Nm 3 / h, the feeding time is 12min, and the refined melt is obtained after removing the scum on the liquid surface; S3. Spheroidizing inoculation: placing a spheroidizing agent with a particle size D90 of 13 mm on one side of the bottom dam of the ladle, and compacting and tamping to form a spheroidizing agent layer; wherein the mass ratio of the spheroidizing agent to the refined molten metal is 2.3:100; and based on the mass fraction of the spheroidizing agent being 100wt%, it is composed of the following mass fractions of each element: 44wt% silicon, 7.2wt% magnesium, 3.2wt% manganese, 2.8wt% calcium, 1.4wt% yttrium, 0.48wt% cerium, 0.42wt% lanthanum, 0.48wt% neodymium, 0.4wt% aluminum and 0.2wt% titanium, and the balance is iron; A primary inoculant composed of silicon-calcium-barium alloy and silicon carbide is evenly spread on the surface of the spheroidizer layer, and after compaction, a primary inoculant layer covering the surface of the spheroidizer layer is formed; wherein the particle size D90 of the silicon-calcium-barium alloy and the silicon carbide are both 9.5 mm, the mass ratio of the silicon-calcium-barium alloy to the refined melt is 0.28:100, and the mass ratio of the silicon carbide to the refined melt is 0.12:100; based on the mass fraction of the silicon-calcium-barium alloy being 100wt%, it is composed of the following mass fractions of the elements: 43wt% silicon, 13wt% calcium, 10.5wt% barium, 0.5wt% zirconium and 0.18wt% antimony, and the balance is iron; Perlite and iron plates are sequentially stacked on the surface of the primary inoculant layer, the outlet temperature of the refined molten metal in the smelting furnace is controlled at 1515°C, and then the refined molten metal is poured into the ladle from the side of the bottom dam of the ladle where the spheroidizer layer and the primary inoculant layer are not placed; in the process of pouring the refined molten metal, a secondary inoculant with a particle size D90 of 2.5 mm is added along the flow, and the mass ratio of the secondary inoculant to the refined molten metal is 0.045:100; based on the mass fraction of the secondary inoculant being 100wt%, it is composed of the following mass fractions of the elements: 58wt% of silicon, 10wt% of barium, 18wt% of calcium, 2.8wt% of aluminum, 7wt% of cerium and 8wt% of strontium, and the balance is iron; After all the refined molten metal in the smelting furnace is flushed into the ladle, an ultrasonic probe is extended from above the refined molten metal to 95 mm below the liquid surface of the refined molten metal, and 1150 W ultrasonic waves are applied to the refined molten metal. The ultrasonic frequency is 28 kHz, and the ultrasonic treatment time is 1.5 min. After ultrasonic treatment, a casting liquid is obtained; S4, casting: preheat the mold to 580°C in advance, when the temperature of the casting liquid reaches 1395°C, inject the casting liquid in the molten iron ladle into the preheated mold, add a tertiary inoculant with a particle size D90 of 0.5 mm during the pouring of the casting liquid, and the mass ratio of the tertiary inoculant to the refined melt is 0.13:100; Taking the mass fraction of the tertiary inoculant as 100wt%, it is composed of the following elements in mass fractions: 72wt% silicon, 12wt% calcium, 2.8wt% aluminum and 0.013wt% bismuth, and the balance is iron; After all the casting liquid is injected into the mold, it is naturally cooled to 1108°C, and then the cooling rate is adjusted to 1.8°C / min. The mold after casting is subjected to ultrasonic vibration, and the ultrasonic power used is 780W and the ultrasonic frequency is 18kHz. When the mold is cooled to 1020°C, the ultrasonic vibration is stopped and kept warm for 9 hours, and then naturally cooled to room temperature. After demolding, the flange casting is obtained; S5. Quenching and tempering heat treatment: the flange casting after casting is subjected to annealing, normalizing, quenching and tempering treatments in sequence; First, the flange casting after casting was heated to 1030℃ at a heating rate of 28℃ / min and kept at this temperature for 1.8h, then quickly cooled to 730℃ at a cooling rate of 38℃ / min and kept at this temperature for 32min, then slowly cooled to 580℃ at a cooling rate of 18℃ / min, and air-cooled to room temperature after being taken out of the furnace to complete the annealing treatment; Then, the flange casting after annealing treatment was heated to 888°C at a heating rate of 11°C / min and kept at this temperature for 1.2h, and then taken out of the furnace and air-cooled to room temperature to complete the normalizing treatment; Then, the flange casting after normalizing treatment was heated to 855°C at a heating rate of 8°C / min and kept at this temperature for 22 minutes. After the end of the heat preservation, it was cooled to 595°C with the furnace. Then, the flange casting was taken out and immediately buried in 310°C molten salt, and kept in the molten salt for 1.2 hours. When the surface temperature of the flange casting dropped to 290°C, the flange casting was taken out from the molten salt and air-cooled to room temperature to complete the quenching treatment. Finally, the flange casting after quenching treatment was heated to 545°C at a heating rate of 4.5°C / min and kept at this temperature for 3.2h, and then air-cooled to room temperature in the furnace to complete the tempering treatment and obtain the flange green body; S6. Nitrocarburizing: carbon dioxide is introduced into the reactor, the flange green body is placed in the reactor, the flange green body is heated to 880°C and kept warm for 0.8h for carburizing treatment; argon is introduced into the reactor to cool the flange green body, and after the flange green body is cooled to 580°C, a mixed gas consisting of ammonia, nitrogen and carbon dioxide is introduced into the reactor, and the amount of the mixed gas introduced is 1300L / h; based on the total volume fraction of the mixed gas being 100%, the volume fraction of ammonia is 38%, the volume fraction of carbon dioxide is 7%, and the remainder is nitrogen; after keeping warm for 7h, the nitrocarburizing treatment is completed, the depth of nitrocarburizing is 18μm, and a flange rough product is obtained; S7, sandblasting roughening: the flange rough product is sandblasted with brown corundum sand with a particle size D90 of 480 μm, the sandblasting pressure is 0.75 MPa, the vertical distance between the nozzle and the surface of the flange rough product is 220 mm, the angle between the axis of the nozzle and the surface of the flange rough product is 28°, and the surface roughness of the flange rough product formed after sandblasting is 58 μm; then the flange rough product after sandblasting is placed in a mixed solvent of anhydrous ethanol and acetone for ultrasonic cleaning, and after cleaning, it is taken out and dried; S8, coating cladding: anhydrous ethanol and a binder are mixed in a mass ratio of 18:1 to prepare a binder solution, and the cladding material and the binder solution are mixed in a ratio of 1g:0.28mL to prepare a paste-like cladding slurry; Taking the mass fraction of the cladding material as 100wt%, it is composed of the following components in mass fractions: 0.8wt% cerium dioxide, 38wt% tungsten carbide, and the balance nickel-based alloy powder; The nickel-based alloy powder is composed of the following elements in the following mass fractions, based on a mass fraction of 100 wt %: 18 wt % of chromium, 4.5 wt % of iron, 4.5 wt % of silicon, 3.2 wt % of boron, and 0.8 wt % of carbon, with the remainder being nickel. The cladding slurry is evenly coated on the rough surface of the flange after sandblasting, and a cladding slurry layer is formed after drying; the cladding slurry layer is laser clad by a laser, and the process parameters of the laser cladding are: the laser spot diameter is 3.8 mm, the laser power is 1150 W, and the laser scanning speed is 3.5 mm / s. After cooling, a cladding layer with a thickness of 1.2 mm is formed on the surface of the rough flange to obtain the main body flange.
[0129] Example 5 This embodiment provides a method for producing a body flange, such as Figure 1 As shown, the production method specifically comprises the following steps: S1. Alloy smelting: putting the raw material mixture into a smelting furnace, heating the raw material mixture to 1460°C and keeping the temperature for 1 hour to obtain an alloy melt; Taking the mass fraction of the raw material mixture as 100wt%, it is composed of the following elements in mass fractions: 3.7wt% carbon, 2wt% silicon, 0.6wt% manganese, 0.1wt% nickel, 0.4wt% molybdenum and 0.2wt% vanadium, and the balance is iron; S2, refining and purification: the temperature of the alloy melt is adjusted to 1540 ° C, and a purifier is added to the alloy melt, the purifier is composed of calcium oxide and aluminum oxide in a mass ratio of 1:1, and the mass ratio of the purifier to the alloy melt is 0.6:100, and the temperature is kept for 50 minutes to complete the refining and purification; then, 1.8MPa nitrogen is continuously introduced into the smelting furnace, and the nitrogen introduction amount is 150Nm 3 / h, the feeding time is 10min, and the refined melt is obtained after removing the scum on the liquid surface; S3. Spheroidizing inoculation: placing a spheroidizing agent with a particle size D90 of 15 mm on one side of the bottom dam of the ladle, and compacting and tamping to form a spheroidizing agent layer; wherein the mass ratio of the spheroidizing agent to the refined molten metal is 2.5:100; and based on the mass fraction of the spheroidizing agent being 100wt%, it is composed of the following mass fractions of each element: 45wt% of silicon, 7wt% of magnesium, 3wt% of manganese, 3wt% of calcium, 1.5wt% of yttrium, 0.5wt% of cerium, 0.4wt% of lanthanum, 0.5wt% of neodymium, 0.5wt% of aluminum and 0.1wt% of titanium, and the balance is iron; A primary inoculant composed of silicon-calcium-barium alloy and silicon carbide is evenly spread on the surface of the spheroidizer layer, and after compaction, a primary inoculant layer covering the surface of the spheroidizer layer is formed; wherein the particle size D90 of the silicon-calcium-barium alloy and the silicon carbide are both 10 mm, the mass ratio of the silicon-calcium-barium alloy to the refined melt is 0.3:100, and the mass ratio of the silicon carbide to the refined melt is 0.1:100; based on the mass fraction of the silicon-calcium-barium alloy being 100wt%, it is composed of the following mass fractions of the elements: 45wt% silicon, 12wt% calcium, 10wt% barium, 0.6wt% zirconium and 0.15wt% antimony, and the balance is iron; Perlite and iron plates are sequentially stacked on the surface of the primary inoculant layer, the outlet temperature of the refined molten metal in the smelting furnace is controlled at 1520°C, and then the refined molten metal is poured into the ladle from the side of the bottom dam of the ladle where the spheroidizer layer and the primary inoculant layer are not placed; in the process of pouring the refined molten metal, a secondary inoculant with a particle size D90 of 3 mm is added along the flow, and the mass ratio of the secondary inoculant to the refined molten metal is 0.05:100; based on the mass fraction of the secondary inoculant being 100wt%, it is composed of the following mass fractions of each element: 60wt% of silicon, 8wt% of barium, 20wt% of calcium, 3wt% of aluminum, 6wt% of cerium and 9wt% of strontium, and the balance is iron; After all the refined molten metal in the smelting furnace is flushed into the ladle, an ultrasonic probe is extended from above the refined molten metal to 100 mm below the liquid surface of the refined molten metal, and 1200 W ultrasonic waves are applied to the refined molten metal. The ultrasonic frequency is 30 kHz, and the ultrasonic treatment time is 1 min. After ultrasonic treatment, a casting liquid is obtained; S4, casting: preheat the mold to 600°C in advance. When the temperature of the casting liquid reaches 1400°C, inject the casting liquid in the molten iron ladle into the preheated mold. During the pouring process of the casting liquid, add a tertiary inoculant with a particle size D90 of 0.6 mm. The mass ratio of the tertiary inoculant to the refined melt is 0.15:100. Taking the mass fraction of the tertiary inoculant as 100wt%, it is composed of the following elements in mass fractions: 75wt% silicon, 10wt% calcium, 3wt% aluminum and 0.015wt% bismuth, and the balance is iron; After all the casting liquid is injected into the mold, it is naturally cooled to 1200°C, and then the cooling rate is adjusted to 2°C / min. The mold after casting is subjected to ultrasonic vibration, and the ultrasonic power used is 800W and the ultrasonic frequency is 20kHz. When the mold is cooled to 1050°C, the ultrasonic vibration is stopped and kept warm for 8 hours, and then naturally cooled to room temperature. After demolding, the flange casting is obtained; S5. Quenching and tempering heat treatment: the flange casting after casting is subjected to annealing, normalizing, quenching and tempering treatments in sequence; First, the flange casting after casting was heated to 1050℃ at a heating rate of 30℃ / min and kept at this temperature for 1.5h, then quickly cooled to 750℃ at a cooling rate of 40℃ / min and kept at this temperature for 30min, then slowly cooled to 600℃ at a cooling rate of 20℃ / min, and air-cooled to room temperature after being taken out of the furnace to complete the annealing treatment; Then, the flange casting after annealing treatment was heated to 900°C at a heating rate of 12°C / min and kept at this temperature for 1h, and then taken out of the furnace and air-cooled to room temperature to complete the normalizing treatment; Then, the flange casting after normalizing treatment is heated to 860°C at a heating rate of 10°C / min and kept at this temperature for 20 minutes. After the end of the heat preservation, it is cooled to 600°C with the furnace. Then, the flange casting is taken out and immediately buried in 320°C molten salt, and kept in the molten salt for 1 hour. When the surface temperature of the flange casting drops to 300°C, the flange casting is taken out from the molten salt and air-cooled to room temperature to complete the quenching treatment. Finally, the flange casting after quenching treatment was heated to 550°C at a heating rate of 5°C / min and kept at this temperature for 3h, and then air-cooled to room temperature in the furnace to complete the tempering treatment and obtain the flange green body; S6, nitrocarburizing: carbon dioxide is introduced into the reactor, the flange green body is placed in the reactor, the flange green body is heated to 900°C and kept warm for 0.5h for carburizing treatment; argon is introduced into the reactor to cool the flange green body, and after the flange green body is cooled to 600°C, a mixed gas composed of ammonia, nitrogen and carbon dioxide is introduced into the reactor, and the amount of the mixed gas introduced is 1500L / h; based on the total volume fraction of the mixed gas being 100%, the volume fraction of ammonia is 40%, the volume fraction of carbon dioxide is 8%, and the remainder is nitrogen; after keeping warm for 8h, the nitrocarburizing treatment is completed, the depth of nitrocarburizing is 20μm, and a flange rough product is obtained; S7, sandblasting roughening: the flange rough product is sandblasted with brown corundum sand with a particle size D90 of 500 μm, the sandblasting pressure is 0.8 MPa, the vertical distance between the nozzle and the surface of the flange rough product is 250 mm, the angle between the axis of the nozzle and the surface of the flange rough product is 30°, and the surface roughness of the flange rough product formed after sandblasting is 60 μm; then the flange rough product after sandblasting is placed in a mixed solvent of anhydrous ethanol and acetone for ultrasonic cleaning, and taken out and dried after cleaning; S8, coating cladding: anhydrous ethanol and a binder are mixed in a mass ratio of 20:1 to prepare a binder solution, and the cladding material and the binder solution are mixed in a ratio of 1 g:0.3 mL to prepare a paste-like cladding slurry; Taking the mass fraction of the cladding material as 100wt%, it is composed of the following components in mass fractions: 1wt% cerium dioxide, 40wt% tungsten carbide, and the balance nickel-based alloy powder; The nickel-based alloy powder is composed of the following elements in the following mass fractions, based on the mass fraction of the nickel-based alloy powder being 100wt%: 20wt% chromium, 4wt% iron, 5wt% silicon, 3wt% boron and 1wt% carbon, with the balance being nickel; The cladding slurry is evenly coated on the rough surface of the flange after sandblasting, and a cladding slurry layer is formed after drying; the cladding slurry layer is laser clad by a laser, and the process parameters of the laser cladding are: the laser spot diameter is 4 mm, the laser power is 1200 W, and the laser scanning speed is 4 mm / s. After cooling, a cladding layer with a thickness of 1.5 mm is formed on the surface of the rough flange to obtain the main body flange.
[0130] Example 6 This embodiment provides a method for producing a body flange, which differs from Embodiment 1 in that, in step S3, the mass ratio of the spheroidizing agent to the refined melt is adjusted to 1:100, and other process parameters and operating conditions are exactly the same as those in Embodiment 1.
[0131] Example 7 This embodiment provides a method for producing a body flange, which differs from Embodiment 1 in that, in step S3, the mass ratio of the spheroidizing agent to the refined melt is adjusted to 3:100, and other process parameters and operating conditions are exactly the same as those in Embodiment 1.
[0132] Example 8 This embodiment provides a method for producing a body flange, which differs from Embodiment 1 in that, in step S3, the particle size D90 of the spheroidizing agent is adjusted to 5 mm, and other process parameters and operating conditions are exactly the same as those in Embodiment 1.
[0133] Example 9 This embodiment provides a method for producing a body flange, which differs from Embodiment 1 in that, in step S3, the particle size D90 of the spheroidizing agent is adjusted to 20 mm, and other process parameters and operating conditions are exactly the same as those in Embodiment 1.
[0134] Example 10 This embodiment provides a method for producing a body flange, which differs from Embodiment 1 in that, in step S8, the mass fraction of cerium dioxide in the cladding material is adjusted to 0.1wt%, the mass fraction of tungsten carbide remains unchanged, and the remainder is nickel-based alloy powder. Other process parameters and operating conditions are exactly the same as those in Embodiment 1.
[0135] Embodiment 11 This embodiment provides a method for producing a body flange, which differs from Embodiment 1 in that, in step S8, the mass fraction of cerium dioxide in the cladding material is adjusted to 1.5wt%, the mass fraction of tungsten carbide remains unchanged, and the remainder is nickel-based alloy powder. Other process parameters and operating conditions are exactly the same as those in Embodiment 1.
[0136] Comparative Example 1 This comparative example provides a method for producing a body flange, which differs from Example 1 in that applying ultrasonic waves to the refining solution is omitted in step S3, and other process parameters and operating conditions are exactly the same as those in Example 1.
[0137] The graphite metallographic structure and matrix metallographic structure of the flange green body prepared in this comparative example were observed using a metallographic microscope, and the following results were obtained: Figure 4 and Figure 5 The metallographic micrograph shown in Example 1 Figure 2 and Figure 3 compared to, Figure 4 and Figure 5 The graphite nodules in the metallographic micrographs shown are fewer in number and larger in size.
[0138] Comparative Example 2 This comparative example provides a method for producing a body flange, which differs from Example 1 in that ultrasonic vibration of the mold is omitted in step S4, and other process parameters and operating conditions are exactly the same as those in Example 1.
[0139] The graphite metallographic structure and matrix metallographic structure of the flange green body prepared in this comparative example were observed using a metallographic microscope, and the following results were obtained: Figure 6 and Figure 7 The metallographic micrograph shown in Example 1 Figure 2 and Figure 3 compared to, Figure 6 and Figure 7 The graphite nodules in the metallographic micrographs shown are fewer in number and larger in size.
[0140] Comparative Example 3 This comparative example provides a method for producing a body flange, which differs from Example 1 in that in step S4, no tertiary inoculant is added to the casting liquid during the pouring process, and other process parameters and operating conditions are exactly the same as those in Example 1.
[0141] The graphite metallographic structure and matrix metallographic structure of the flange green body prepared in this comparative example were observed using a metallographic microscope, and the following results were obtained: Figure 8 and Fig. 9 The metallographic micrograph shown in Example 1 Figure 2 and Figure 3 compared to, Figure 8 and Fig. 9 The graphite nodules in the metallographic micrographs shown are fewer in number and larger in size.
[0142] Comparative Example 4 This comparative example provides a method for producing a body flange, which differs from Example 1 in that no cerium dioxide is added to the cladding material in step S8, the mass fraction of tungsten carbide is the same as that in Example 1, and the remainder is nickel-based alloy powder. Other process parameters and operating conditions are exactly the same as those in Example 1.
[0143] The cladding layer on the surface of the body flange prepared in this comparative example was observed using an optical microscope, and the following results were obtained: Fig.11 The optical micrograph shown is similar to that shown in Example 1. Fig.10 compared to, Fig.11 There are obvious defects such as cracks and holes in the cladding layer shown in the optical micrograph.
[0144] The tensile strength, elongation and surface hardness of the flange crude products prepared in Examples 1-11 and Comparative Examples 1-4 were tested, and the specific test steps are as follows: (1) An electronic universal material testing machine was used to test the tensile strength and elongation of the flange rough product. The flange specimens used in the test were GB1348-2009 ductile iron standard tensile specimens. Each group of three specimens had an average value as the test result. The test parameters were set as follows: the specimen gauge length was 30 mm, the inner diameter of the specimen gauge length was 6 mm, and the tensile rate was 2 mm / min.
[0145] (2) The surface hardness of the flange rough product is tested using a hardness tester. The test parameters are set as follows: loading force is 750 kg, the pressure head diameter is 5 mm, and the test force holding time is 15 s. During the test, 5 measurement points are selected on each sample, and the average value is taken as the test result of the measured sample.
[0146] The wear rate of the surface cladding layer of the body flange prepared in Examples 1-11 and Comparative Examples 1-4 was tested, and the specific test steps were as follows: The wear resistance of the cladding layer on the surface of the body flange was tested using a disc-type friction and wear tester. The test method was reciprocating sliding friction. Alumina corundum balls were used as sliding friction pairs. The sliding speed was set to 20 cm / s. The test time for a single sample was 20 s. The wear rate was calculated using the following formula: ; Where W r is the wear rate (mm 3 ·N -1 ·m -1 ), V is the wear volume (mm 3 ), F is the vertical load (N), and L is the wear distance (m). The wear volume V is calculated using the following formula: ; Where r is the wear scar radius (mm), S is the cross-sectional area of the wear scar (mm 2 ).
[0147] The test results are shown in Table 1.
[0148] Table 1 Test results
[0149] It can be seen from the test data of Examples 1-11 and Comparative Examples 1-4 that the tensile strength and hardness of the flange crude product prepared in Examples 1-5 are higher than those in Examples 6-9 and Comparative Examples 1-3, and the wear rate of the cladding layer prepared in Examples 1-5 is higher than that in Examples 10-11 and Comparative Example 4, which indicates that the main flange prepared by the production method provided by the present invention has excellent mechanical properties and wear resistance.
[0150] It can be seen from the test data of Example 1, Example 6 and Example 7 that the tensile strength and hardness of the flange crude products prepared in Example 6 and Example 7 are lower than those in Example 1. This is because the amount of spheroidizer used in Example 6 is too low, and the amount of spheroidizer used in Example 7 is too high, which affects the number and roundness of graphite balls, and ultimately leads to a decrease in the comprehensive mechanical properties of the flange crude product.
[0151] It can be seen from the test data of Example 1, Example 8 and Example 9 that the tensile strength and hardness of the flange crude products prepared in Example 8 and Example 9 are lower than those in Example 1. This is because the particle size D90 of the spheroidizer in Example 8 is too small, and the particle size D90 of the spheroidizer in Example 9 is too large, which affects the number and roundness of the graphite balls, and ultimately leads to a decrease in the comprehensive mechanical properties of the flange crude product.
[0152] It can be seen from the test data of Example 1, Example 10 and Example 11 that the wear rate of the surface cladding layer of the body flange prepared in Example 10 and Example 11 is lower than that in Example 1. This is because the amount of cerium dioxide added in Example 10 is too low, and the amount of cerium dioxide added in Example 11 is too high, which affects the morphology and organizational structure of the cladding layer, and ultimately leads to a decrease in the wear resistance of the cladding layer.
[0153] It can be seen from the test data of Example 1, Comparative Example 1 and Comparative Example 2 that the tensile strength and hardness of the flange crude products prepared in Comparative Example 1 and Comparative Example 2 are lower than those in Example 1, which indicates that applying ultrasound during the spheroidization inoculation process and the casting process is beneficial to increasing the number and roundness of graphite balls, so that the comprehensive mechanical properties of the flange crude product finally prepared are significantly improved.
[0154] It can be seen from the test data of Example 1 and Comparative Example 3 that the tensile strength and hardness of the flange crude product prepared in Comparative Example 3 are lower than those in Example 1, which indicates that the addition of bismuth-containing tertiary inoculant during the casting process is beneficial to increasing the number and roundness of graphite balls, so that the comprehensive mechanical properties of the flange crude product finally prepared are significantly improved.
[0155] It can be seen from the test data of Example 1 and Comparative Example 4 that the wear rate of the surface cladding layer of the body flange prepared in Comparative Example 4 is lower than that in Example 1, which indicates that adding cerium dioxide to the cladding material can significantly improve the structural density of the cladding layer, reduce defects such as sand holes and pores in the cladding layer, and significantly improve the wear resistance of the body flange finally prepared.
[0156] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for producing a body flange, characterized in that: The production method comprises: S1. Alloy smelting: putting the raw material mixture into a smelting furnace, and smelting the raw material mixture to obtain an alloy melt; S2, refining and purification: adjusting the temperature of the alloy melt to the refining temperature, then adding a purifier to the alloy melt, keeping it at the refining temperature for a period of time, then continuously introducing nitrogen into the smelting furnace, removing scum on the liquid surface to obtain a refined melt; S3, spheroidization inoculation: placing a spheroidizer on one side of the bottom dam of the ladle, compacting and tamping to form a spheroidizer layer, evenly spreading a primary inoculant on the surface of the spheroidizer layer, compacting and tamping to form a primary inoculant layer covering the surface of the spheroidizer layer, and sequentially stacking a perlite layer and an iron plate on the surface of the primary inoculant layer; flushing the refined molten metal in the smelting furnace into the ladle from the side of the bottom dam where the spheroidizer layer and the primary inoculant layer are not placed, and adding a secondary inoculant along the flow during the flushing of the refined molten metal; after the refined molten metal in the smelting furnace is completely flushed into the ladle, extending an ultrasonic probe from above the refined molten metal to below the liquid level of the refined molten metal, applying ultrasonic waves to the refined molten metal, and obtaining a casting liquid after ultrasonic treatment; S4, casting: preheating the mold in advance, when the temperature of the casting liquid reaches the casting temperature, injecting the casting liquid in the molten iron ladle into the preheated mold, adding three inoculants during the pouring process of the casting liquid; after the casting liquid is completely injected into the mold, naturally cooling to a first cooling temperature, then adjusting the cooling rate, ultrasonically vibrating the mold after casting, stopping the ultrasonic vibration when the mold is cooled to a second cooling temperature and keeping the temperature for a period of time, then naturally cooling to room temperature, and demolding to obtain a flange casting; S5, quenching and tempering heat treatment: first, the flange casting after casting is heated to the annealing temperature and kept warm for a period of time, then quickly cooled to the first temperature and kept warm for a period of time, then slowly cooled to the second temperature, taken out of the furnace and air-cooled to room temperature, and the annealing treatment is completed; then, the flange casting after annealing is heated to the normalizing temperature and kept warm for a period of time, then taken out of the furnace and air-cooled to room temperature, and the normalizing treatment is completed; then, the flange casting after normalizing is heated to the quenching temperature and kept warm for a period of time, and after the end of the insulation, it is cooled to the third temperature with the furnace, and then the flange casting is taken out and immediately buried in the preheated molten salt, and after a period of time, the surface temperature of the flange casting is reduced to the fourth temperature, and then it is taken out from the molten salt and air-cooled to room temperature, and the quenching treatment is completed; finally, the flange casting after quenching is heated to the tempering temperature and kept warm for a period of time, and air-cooled to room temperature with the furnace, and the tempering treatment is completed to obtain the flange green billet; S6, nitrocarburizing: introducing carbon dioxide into the reaction furnace, placing the flange green body in the reaction furnace, heating the flange green body to the carburizing temperature and keeping it warm for a period of time to perform carburizing treatment; introducing protective gas into the reaction furnace to cool the flange green body, after the flange green body is cooled to the co-carburizing temperature, introducing a mixed gas consisting of ammonia, nitrogen and carbon dioxide into the reaction furnace, keeping it warm for a period of time, completing the nitrocarburizing treatment, and obtaining a rough flange product; S7, sandblasting roughening: sandblasting the rough flange product with a sandblasting device, then placing the rough flange product after sandblasting in a mixed solvent of anhydrous ethanol and acetone for ultrasonic cleaning, and taking it out and drying it after cleaning; S8, coating cladding: anhydrous ethanol and a binder are mixed in proportion to prepare a binder solution, and a cladding material and the binder solution are mixed in proportion to prepare a paste-like cladding slurry, wherein the cladding material includes nickel-based alloy powder, cerium dioxide and tungsten carbide; the cladding slurry is uniformly applied to the surface of the rough flange after sandblasting, and a cladding slurry layer is formed after drying; the cladding slurry layer is laser clad by a laser, and a cladding layer is formed on the surface of the rough flange after cooling to obtain the body flange.
2. The method for producing a body flange according to claim 1, characterized in that: In step S1, the raw material mixture is composed of the following elements in mass fractions, taking the mass fraction of the raw material mixture as 100 wt %: Carbon 3.5~3.7wt%, silicon 2~2.5wt%, manganese 0.3~0.6wt%, nickel 0.1~0.2wt%, molybdenum 0.3~0.4wt% and vanadium 0.2~0.5wt%, the balance is iron; The smelting temperature is 1450-1460°C; The smelting time is 1 to 2 hours.
3. The method for producing a body flange according to claim 1, characterized in that: In step S2, the refining temperature is 1520-1540°C; The mass ratio of the purifier to the alloy melt is (0.4-0.6):100; Keeping the temperature at the refining temperature for 50 to 60 minutes; The nitrogen gas introduction pressure is 1.5-1.8 MPa; The nitrogen gas flow rate is 100-150 Nm 3 / h; The nitrogen is introduced for 10 to 20 minutes.
4. The method for producing a body flange according to claim 1, characterized in that: In step S3, the mass ratio of the spheroidizing agent to the refined melt is (1.5-2.5):100; Taking the mass fraction of the spheroidizing agent as 100wt%, it is composed of the following elements in mass fractions: Silicon 40-45wt%, magnesium 7-7.5wt%, manganese 3-4wt%, calcium 2-3wt%, yttrium 1.2-1.5wt%, cerium 0.4-0.5wt%, lanthanum 0.4-0.5wt%, neodymium 0.4-0.5wt%, aluminum 0.1-0.5wt% and titanium 0.1-0.5wt%, the balance is iron; The particle size D90 of the spheroidizing agent is 10-15 mm; The primary inoculant layer is composed of silicon-calcium-barium alloy and silicon carbide, wherein the mass ratio of the silicon-calcium-barium alloy to the refined melt is (0.2-0.3):100, and the mass ratio of the silicon carbide to the refined melt is (0.1-0.2):100; Taking the mass fraction of the silicon-calcium-barium alloy as 100wt%, it is composed of the following elements in mass fractions: Silicon 40-45wt%, calcium 12-15wt%, barium 10-12wt%, zirconium 0.3-0.6wt% and antimony 0.15-0.3wt%, the balance being iron; The particle size D90 of the primary inoculant is 8-10 mm; The mass ratio of the secondary inoculant to the refined melt is (0.03-0.05):100; Taking the mass fraction of the secondary inoculant as 100wt%, it is composed of the following elements in mass fractions: Silicon 50-60wt%, barium 8-15wt%, calcium 10-20wt%, aluminum 2-3wt%, cerium 6-10wt% and strontium 5-9wt%, the balance being iron; The particle size D90 of the secondary inoculant is 1-3 mm; The outlet temperature of the refined molten metal in the smelting furnace before being poured into the ladle is controlled at 1500-1520°C; The ultrasonic probe extends to 80-100 mm below the liquid surface of the refined molten liquid; The transmitting power of the ultrasonic probe is 1000~1200W; The ultrasonic frequency emitted by the ultrasonic probe is 20~30kHz; The ultrasonic treatment time is 1 to 3 minutes.
5. The method for producing a body flange according to claim 1, characterized in that: In step S4, the mold is preheated to 500-600°C; The casting temperature is 1380-1400°C; The mass ratio of the tertiary inoculant to the refined melt is (0.1-0.15):100; Taking the mass fraction of the tertiary inoculant as 100wt%, it is composed of the following elements in mass fractions: Silicon 65-75wt%, calcium 10-20wt%, aluminum 2-3wt% and bismuth 0.01-0.015wt%, the balance is iron; The particle size D90 of the tertiary inoculant is 0.2-0.6 mm; The first cooling temperature is 1100-1200° C.; After naturally cooling to the first cooling temperature, adjust the cooling rate to 1~2℃ / min; The ultrasonic power of the ultrasonic vibration is 700-800W; The ultrasonic frequency of the ultrasonic vibration is 10-20 kHz; The second cooling temperature is 950-1050°C; Keep at the second cooling temperature for 8 to 12 hours.
6. The method for producing a body flange according to claim 1, characterized in that: In step S5, the flange casting is heated to the annealing temperature at a heating rate of 20-30°C / min; The annealing temperature is 1000-1050°C; Keeping the annealing temperature for 1.5 to 2.5 hours; Cooling from the annealing temperature to the first temperature at a cooling rate of 30-40°C / min; The first temperature is 700-750°C; Keep warm at the first temperature for 30 to 40 minutes; Cooling from the first temperature to the second temperature at a cooling rate of 10-20°C / min; The second temperature is 500-600° C.; The flange casting after annealing is heated to the normalizing temperature at a heating rate of 8-12°C / min; The normalizing temperature is 880~900℃; Keep at the normalizing temperature for 1 to 2 hours; The flange casting after normalizing treatment is heated to the quenching temperature at a heating rate of 5-10°C / min; The quenching temperature is 840~860℃; Keeping the quenching temperature for 20 to 30 minutes; The third temperature is 580-600° C. The preheating temperature of the molten salt is 280-320°C; The flange casting is buried in the molten salt for 1 to 2 hours; The fourth temperature is 260-300° C. The flange casting after quenching treatment is heated to the tempering temperature at a heating rate of 3-5°C / min; The tempering temperature is 530-550°C; Keep at the tempering temperature for 3 to 4 hours.
7. The method for producing a body flange according to claim 1, characterized in that: In step S6, the carburizing temperature is 800-900°C; Keeping the temperature at the carburizing temperature for 0.5 to 1.5 hours; The co-penetration temperature is 500-600°C; Taking the total volume fraction of the mixed gas as 100%, the volume fraction of ammonia is 30-40%, the volume fraction of carbon dioxide is 5-8%, and the balance is nitrogen; The amount of the mixed gas introduced is 1000-1500 L / h; Keeping the temperature at the co-osmosis temperature for 5 to 8 hours; The depth of the nitrocarburizing is 10-20 μm.
8. The method for producing a body flange according to claim 1, characterized in that: In step S7, the sandblasting medium used in the sandblasting process is brown corundum sand; The particle size D90 of the sandblasting medium is 400-500 μm; The blasting pressure of the blasting treatment is 0.6-0.8 MPa; During the sandblasting process, the vertical distance between the nozzle and the rough surface of the flange is 150-250 mm; During the sandblasting process, the angle between the axis of the nozzle and the rough surface of the flange is 20-30°; The surface roughness of the flange rough product formed after the sandblasting treatment is 50-60 μm.
9. The method for producing a body flange according to claim 1, characterized in that: In step S8, the mass ratio of the anhydrous ethanol to the binder is (10-20):1; The ratio of the cladding material to the binder solution is 1 g: (0.2-0.3) mL; Taking the mass fraction of the cladding material as 100wt%, it is composed of the following components in mass fractions: Cerium dioxide 0.5~1wt%; Tungsten carbide 30~40wt%; The balance is nickel-based alloy powder; Taking the mass fraction of the nickel-based alloy powder as 100wt%, it is composed of the following elements in mass fractions: Chromium 15-20wt%, iron 4-6wt%, silicon 3-5wt%, boron 3-4wt% and carbon 0.5-1wt%, the balance is nickel; The laser spot diameter used in the laser cladding process is 3-4 mm; The laser power used in the laser cladding process is 1000~1200W; The laser scanning speed used in the laser cladding process is 2~4mm / s; The thickness of the cladding layer is 0.5-1.5 mm.
10. A body flange obtained according to the production method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for integrally casting large-sized V-shaped diesel engine body by utilizing nodular cast iron
CN103215488A
Casting process method for nodular cast iron casting used at ultralow temperature
CN103752781A
Wear-resistant and antifriction composite coating for aluminum alloy component surfaces and preparation method thereof
CN105624670A
Method for cladding nickel-based alloy coating on surface of vermicular graphite cast iron mould after laser pre-heating treatment
CN105779997A
Spheroidizing inoculation method of spheroidal graphite cast iron
CN108624802A
Cited By
High-spheroidization-rate spheroidal graphite cast iron for silicon carbide auxiliary spheroidization inoculation and preparation method thereof
CN119332042A