Method for preparing ceramic mechanical arm through integrated dry pressing
Through an integrated dry pressing preparation method, hard elastic components and lost foam materials are used to prepare regular pore grooves in the ceramic robot arm, which solves the problems of long processing time, high cost and difficulty in ensuring air tightness of the ceramic robot arm, and achieves high efficiency and Low-cost ceramic robotic arm production.
Patent Information
- Application Number
- CN202411226885.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing manufacturing methods of ceramic robot arms have problems such as long processing time, high cost, low yield, and difficulty in ensuring air tightness. In particular, when processing pore grooves, the efficiency is low and defects are easily introduced.
Adopting an integrated dry pressing preparation method, by pasting hard elastic components on the dry pressing mold, pre-pressing and dry pressing ceramic powder, combined with the lost foam material to make regular pore grooves, cold isostatic pressing and sintering, reducing machining links and improve the air tightness of the product.
It significantly reduces the production cost of ceramic robotic arms, improves the yield of finished products, ensures the regularity and flatness of pore grooves, is suitable for processing high-purity alumina ceramic materials, and adapts to large-scale production needs.
Smart Images

Figure CN118809771A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor and photovoltaic industry equipment, and in particular to a method for preparing a ceramic robot arm by integrated dry pressing. Background Art
[0002] The robotic arms used in the semiconductor processing industry have air holes and pores. When in use, air is drawn from the pores to form a vacuum to absorb the semiconductor parts. This method of handling can achieve light contact and is not easy to damage the workpiece. In addition, due to the special environment in semiconductor parts processing, the robotic arms should also have the properties of not polluting parts, high temperature resistance, and acid and alkali corrosion resistance.
[0003] Ceramic robotic arms play a role in the handling of semiconductor equipment, responsible for carrying silicon wafers to designated locations. Since silicon wafers are extremely susceptible to contamination by other particles, they are generally carried out in a vacuum environment, and strict requirements are placed on the material and performance of the robotic arms. In this environment, robotic arms made of most materials generally have difficulty completing their work, and the materials used to make the robotic arms need to be resistant to high temperatures, wear-resistant, high in hardness, and high in purity.
[0004] For the production of ceramic robotic arms, the current more mature technology is generally achieved by splicing, that is, two ceramic sheets are processed separately according to the drawings, and then bonded with a specific glue, and finally the ceramic robotic arm is obtained by processing its outer contour, that is, 1. Arm body processing: ceramic plate sintering molding → machining according to the drawings; 2. Cover plate machining: ceramic cover plate sintering molding → machining according to the drawings; 3. Cover plate and arm body gluing; 4. Overall surface grinding. However, there are the following problems in using this method to make ceramic robotic arms: on the one hand, it is necessary to process two ceramic sheets, the processing time is long, the processing is complicated, and a large amount of machining is required, especially CNC machining. Ceramic CNC machining itself is time-consuming, has high process requirements, low yield, and high cost. Especially for robotic arms, there are a large number of machining thin-walled links, which have extremely high requirements for material and CNC process matching, and also have high requirements for operators. Traditional machining can easily introduce cracks or collapse edges in this link, resulting in product scrapping. On the other hand, the gluing link has high requirements for glue performance, which is prone to uneven bonding and affects air tightness. In particular, it needs to be resistant to high temperatures and has high requirements for gluing technology. It is necessary to ensure the air tightness of the ceramic robot arm, the air groove is not blocked, the flatness accuracy of the product after gluing meets the requirements, and the thickness is strictly controlled; the glue also has the problem of aging and yellowing. In addition, traditional processing methods are often inefficient and costly when processing pore grooves, and it is difficult to meet the needs of large-scale production. High-purity alumina ceramics can meet the above performance requirements, but for ceramic materials, the regular morphology required inside the robot arm and the smooth pore grooves are difficult to process. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a ceramic robot arm by integrated dry pressing, which can directly internally sinter a ceramic robot arm with regular pore grooves with controllable sizes.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a ceramic robot arm by integrated dry pressing, comprising the following steps:
[0008] A hard elastic component is attached to the upper pressing head of the dry pressing die to form a hard elastic pressing head;
[0009] Laying a first layer of ceramic powder on the bottom of the dry pressing mold and performing pre-pressing to obtain a first pressed product;
[0010] Placing the lost mold on the surface of the first pressed product, laying a second layer of ceramic powder, and performing dry pressing to obtain a second pressed product;
[0011] cold isostatically pressing the second pressed product and then sintering it to obtain a ceramic robot arm;
[0012] The lost mold is obtained by making the lost mold material into the shape required by the robot arm air groove.
[0013] Preferably, the lost foam material includes graphite paper, paraffin sheet or acrylic board.
[0014] Preferably, the purity of the graphite paper is ≥99.5%.
[0015] Preferably, the hard elastic component includes rubber or PU; and the ceramic powder includes aluminum oxide powder or zirconium oxide powder.
[0016] Preferably, the thickness of the first layer of ceramic powder is 1 to 20 mm.
[0017] Preferably, the pre-pressing method is unidirectional pressurization; the pre-pressing pressure is 2 to 10 MPa, and the time is 30 to 100 s.
[0018] Preferably, the thickness of the second layer of ceramic powder is 1 to 30 mm.
[0019] Preferably, the dry pressing is performed in a bidirectional manner; the pressure of the dry pressing is 8 to 20 MPa, and the time is 40 to 100 s.
[0020] Preferably, the cold isostatic pressing pressure is 50-200 MPa, and the time is 100-500 s.
[0021] Preferably, the sintering temperature is 1400-1620° C. and the sintering time is 30-300 min.
[0022] The present invention adopts a lost foam combined with secondary dry pressing and cold isostatic pressing method, embeds a lost foam in ceramic powder, and after high-temperature sintering, the mold disappears to leave regular and smooth pore grooves, which can be directly fired inside to form a ceramic mechanical arm with regular, size-controllable and smooth pore grooves.
[0023] Compared with the traditional scheme of machining the cover plate and the arm blank, the integrated robotic arm scheme can reduce the machining of the cover plate and the pore groove. Since the ceramic is hard and brittle after firing, it needs to be processed by grinding. Due to the high brittleness and low toughness of ceramics, the single grinding amount is relatively limited, so the processing time is long, and a large number of grinding heads need to be consumed, resulting in an increase in processing costs; at the same time, defects such as cracks and broken edges may also be introduced, affecting the product yield, so most of the robotic arms on the market are 99 porcelain products with better toughness and better machining performance. In addition, because it is a split type, it needs to be glued, which may affect the air tightness of the product and even introduce impurities. The present invention introduces lost foam, and directly forms an integrated shape through dry pressing, which directly reduces the processing of the pore groove and the cover plate, greatly reduces the amount of machining, and thus can significantly reduce costs, thereby reducing the defect rate caused by machining. In addition, the method of the present invention can also be used to produce brittle ceramic robotic arms that are difficult to process by conventional CNC.
[0024] Since the material of the lost foam is different from that of the ceramic body, the present invention optimizes the traditional dry pressing process and adopts a secondary pressurization method to avoid the defects caused by pressing different materials. The present invention first uses a hard elastic pressure head for pre-pressing, then buries the lost foam, and then performs secondary dry pressing. The material of the elastic material can be adjusted to make the material to be pressed in the mold evenly stressed to achieve the effect of isostatic pressing, so that the powder is pressed evenly, and finally sintered after cold isostatic pressing to ensure that ceramic stratification will not occur. This method ensures that the powder is evenly distributed during pressing and that the shrinkage is consistent during sintering, thereby avoiding deformation of the pore grooves.
[0025] The present invention combines the characteristics of strength increasing with temperature during sintering of ceramic green bodies, selects a specific lost foam material, and uses a hard elastic pressure head for pre-pressing before placing the lost foam. Compared with the traditional metal pressure head, the hard elastic pressure head can transmit a balanced isostatic pressure when pressing down; after placing the lost foam, bidirectional pressure is applied for secondary pressing to ensure that the powder near the lost foam is also compacted; at the same time, it can also alleviate the problem of greater rebound of the lost foam caused by the different rigidity between the lost foam and the ceramic body, and ensure that the surface of the ceramic body is flat regardless of whether there is a lost foam directly below the dry pressing. After vacuum packaging, a cold isostatic pressing process is carried out to further improve the density of the ceramic body, and at the same time further ensure that no ceramic stratification occurs in the subsequent process. For samples that have not been pre-pressed, due to the different rigidity between the lost foam and the ceramic, a greater rebound will occur at the lost foam after dry pressing, resulting in a bulge easily generated at the position directly above the lost foam during the pressing process, and this position is prone to cracking after sintering.
[0026] The method of the present invention adopts one-piece molding to prepare a ceramic robot arm, which reduces the ceramic machining link, and at the same time, there is no split or glue link, so the air tightness of the product is guaranteed from the source. In addition, the dry pressing process is more mature and has higher production efficiency. The process of secondary pressing and subsequent cold isostatic pressing by a hard elastic pressure head ensures that the surface of the ceramic body is flat and has no stratification, and a defect-free one-piece ceramic robot arm is obtained during subsequent sintering, thereby improving the yield rate. In addition, the molding of airways of complex structures (such as turns) can be completed by machining of lost foam. At the same time, the dry pressing process is not affected by the characteristics of ceramic materials such as large brittleness and poor toughness that make them difficult to machine, and can produce robots of other more brittle materials, breaking through the limitations of traditional machining split product processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a flow chart of the method for preparing a ceramic robot arm by integrated dry pressing of the present invention;
[0028] Figure 2 Schematic diagram of the three-dimensional structure (a), the front structural diagram (b) and the back structural diagram (c) of the ceramic robot arm according to an embodiment of the present invention;
[0029] Figure 3 The actual pictures of the graphite paper cut manually in Example 1 and Comparative Examples 1-2;
[0030] Figure 4 This is a schematic diagram of the placement effect of the graphite paper after pre-pressing in Example 1;
[0031] Figure 5 This is a physical picture of the sample after cold isostatic pressing prepared in Comparative Example 1;
[0032] Figure 6 This is a schematic diagram of the front structure of the hollow ceramic prepared in Comparative Example 2;
[0033] Figure 7 This is a schematic diagram of the side structure of the hollow ceramic prepared in Comparative Example 2. DETAILED DESCRIPTION
[0034] like Figure 1 As shown, the present invention provides a method for preparing a ceramic robot arm by dry pressing, comprising the following steps:
[0035] A hard elastic component is attached to the upper pressing head of the dry pressing die to form a hard elastic pressing head;
[0036] Laying a first layer of ceramic powder on the bottom of the dry pressing mold and performing pre-pressing to obtain a first pressed product;
[0037] Placing the lost mold on the surface of the first pressed product, laying a second layer of ceramic powder, and performing dry pressing to obtain a second pressed product;
[0038] cold isostatically pressing the second pressed product and then sintering it to obtain a ceramic robot arm;
[0039] The lost mold is obtained by making the lost mold material into the shape required by the robot arm air groove.
[0040] In the present invention, unless otherwise specified, the required materials or equipment are commercially available products well known to those skilled in the art.
[0041] The present invention adheres a hard elastic component to the upper pressing head of the dry pressing mold to form a hard elastic pressing head; the hard elastic component includes rubber or PU. The present invention has no special restrictions on the source or specific specifications of the rubber or PU, and corresponding commercial products known in the art can be used.
[0042] The present invention has no special limitation on the sticking thickness of the hard elastic component, which can be adjusted according to actual needs.
[0043] The present invention preferably adheres a hard elastic component to the bottom of the upper pressing head of the dry pressing mold and around the mold to form a hard elastic pressing head to provide balanced stress. Compared with the traditional metal pressing head, it can ensure that the force is applied more evenly during the subsequent pressing process.
[0044] The present invention has no particular limitation on the pasting method, and the pasting method may be performed according to a process well known in the art.
[0045] The present invention lays a first layer of ceramic powder on the bottom of the dry pressing mold, adopts a unidirectional pressurizing method to perform pre-pressing, and obtains a first pressed product.
[0046] The present invention has no special limitation on the dry pressing mold, and any corresponding mold well known in the art can be used.
[0047] Ceramic dry pressing is to fill the powder with good fluidity after spray granulation into the hard metal mold cavity, apply pressure through the pressure head, and the pressure head moves in the mold cavity, transmitting pressure, so that the powder particles in the mold cavity are rearranged and deformed and compacted, forming a ceramic blank with a certain strength and shape. According to the different movement modes of the pressure head and the mold cavity, dry pressing is divided into: (1) unidirectional pressurization, that is, the mold cavity and the lower pressure head are fixed, and the upper pressure head moves; (2) bidirectional pressurization, the mold cavity is fixed, and the upper and lower pressure heads move; (3) movable die, the lower pressure head is fixed, and the mold cavity and the upper pressure head move, that is, the movement of the pressure head and the mold cavity is synchronized. When hydraulic control is used, the pressure head stops moving at a certain set pressure.
[0048] In the present invention, the ceramic powder preferably includes alumina powder or zirconium oxide powder; the alumina powder is preferably 99 alumina ceramic granulation powder or 96 alumina ceramic granulation powder.
[0049] In the present invention, the thickness of the first layer of ceramic powder is preferably 1-20 mm, more preferably 15 mm.
[0050] In the present invention, the pre-pressing method is preferably unidirectional pressurization, the pre-pressing pressure is preferably 2-10 MPa, more preferably 5-8 MPa, and the pre-pressing time is preferably 30-100 s, more preferably 30-80 s.
[0051] After completing the pre-pressing, the present invention preferably releases the pressure to obtain a first pressed product.
[0052] After obtaining the first pressed product, the present invention places the lost mold on the surface of the first pressed product, lays a second layer of ceramic powder, and performs dry pressing to obtain the second pressed product.
[0053] In the present invention, the lost mold is obtained by making the lost mold material into the shape required by the robot arm air groove.
[0054] In the present invention, the lost foam material preferably includes graphite paper, paraffin sheet or acrylic board. In the present invention, the purity of the graphite paper is preferably ≥99.5%.
[0055] When the lost foam material is graphite paper, the graphite paper is preferably cut into the required shape of the robot arm air slot by cutting or laser cutting.
[0056] When the lost foam material is a paraffin sheet or an acrylic plate, it is preferably combined with a carbon-based material to form a binary lost foam. The carbon-based material preferably includes a plastic mesh, paper or cloth; the present invention has no special limitation on the plastic mesh, paper or cloth, and the corresponding materials well known in the art can be used. The present invention improves the brittleness of the paraffin or acrylic material and improves its toughness by compounding. At the same time, it can also ensure that impurities are completely removed during the ceramic sintering process without residual impurities. The homemade lost foam of the present invention can ensure its surface flatness by heating and pressing, and can also further improve its hardness by cold isostatic pressing to reduce the rebound that may occur during the dry pressing process.
[0057] In the present invention, the lost mold is preferably placed at the center of the first pressed product.
[0058] In the present invention, the thickness of the second layer of ceramic powder is preferably 1 to 30 mm, more preferably 10 to 25 mm. The present invention determines the specific thickness value of the second layer of ceramic powder according to actual product requirements.
[0059] In the present invention, the dry pressing method is preferably bidirectional pressing; the pressure of the dry pressing is preferably 8-20 MPa, more preferably 10 MPa, and the time is preferably 40-100 s, more preferably 50-60 s. The present invention adopts bidirectional pressing in the above-mentioned dry pressing mold, which can be gradually applied to the powder to make it denser and prevent subsequent stratification.
[0060] After obtaining the second pressed product, the present invention performs cold isostatic pressing on the second pressed product and then sintering to obtain a ceramic robot arm.
[0061] In the present invention, the second pressed product is preferably vacuum-sealed and cold isostatically pressed.
[0062] In the present invention, the pressure of the cold isostatic pressing is preferably 50 to 200 MPa, more preferably 100 MPa, and the time is preferably 100 to 500 s, more preferably 200 s.
[0063] In the present invention, the sintering temperature is preferably 1400-1620° C., and the sintering time is preferably 30-300 min, more preferably 120-200 min.
[0064] During the sintering process, the lost foam material is burned away to obtain a hollow ceramic robotic arm with pore grooves and pores.
[0065] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0066] Example 1
[0067] (1) Prepare the lost foam:
[0068] Select graphite paper with a thickness of 1mm (the purity of graphite paper is 99.5%) as the lost foam, and cut out the corresponding graphite paper shape according to the airway shape in the design drawing, such as Figure 3 As shown;
[0069] (2) Dry pressing mold adjustment:
[0070] Use a 1mm thick polyester fiber pad to stick it on the bottom of the upper pressure head (the surface that contacts the powder) and around the mold (the part that holds the powder);
[0071] (3) Laying the first layer of ceramic powder and pre-pressing
[0072] First, a 15 mm thick layer of 99 alumina ceramic granulation powder was spread in the dry pressing mold, and a unidirectional pressurization method was used, with a pre-pressing of 5 MPa for 30 seconds, and then the pressure was released to obtain the first pressed product;
[0073] Lift the upper pressing head and place the cut graphite paper pattern in the center of the first pressed product. Figure 4 As shown;
[0074] (4) Lay the second layer of ceramic powder and complete the pressing
[0075] Lay 99 alumina ceramic granulation powder with a thickness of 22 mm, adopt a bidirectional pressurization method, use a pressure of 10 MPa to dry press for 40 seconds, and obtain a second pressed product;
[0076] (5) Cold isostatic pressing
[0077] The second pressed product is vacuum sealed and cold isostatically pressed at a pressure of 100 MPa for 200 seconds.
[0078] (6) Sintering
[0079] The cold isostatically pressed sample was sintered at 1620°C for 2 h to obtain hollow ceramics.
[0080] Compared with the traditional machining solution, this embodiment reduces the air hole slot by 2807mm. 2 The CNC processing volume of the area was reduced by 45784mm 2 The surface grinding of the contact area of the cover plate significantly reduces the machining workload.
[0081] Figure 2 Schematic diagram of the three-dimensional structure (a), the front structure (b) and the back structure (c) of the ceramic robot arm of the embodiment of the present invention; Figure 2 As shown, the pore groove is inside the arm and can be observed through light, but there is no trace on the surface.
[0082] After testing, the ceramic surface of the embodiment after sintering has no cracks, no color difference, and no stratification. The inner wall of the airway is illuminated and observed to be transparent, without foreign matter, no black spots, and no additional coloring. The airtightness is good.
[0083] Example 2
[0084] (1) Prepare the lost foam:
[0085] A commercially available blue dust-free cloth and No. 58 paraffin powder were used as the disappearing mold;
[0086] Prepare an iron mold with a bottom size of 5mm wide and 10mm long on a heating table, cut the dust-free cloth into thin strips with a width of 5mm and a length of 10mm and place them on the bottom of the mold, and spread 58 paraffin wax powder with a thickness of 2mm; turn on the heating table and heat it to 60℃ for 10min to melt the paraffin wax on the surface of the dust-free cloth, and compact the surface of the lost foam with an iron block while cooling to obtain a lost foam with a width of 5mm, a length of 10mm, a height of 2mm, a flat surface, and sufficient rigidity and toughness;
[0087] (2) Dry pressing mold adjustment:
[0088] Use a 1mm thick polyester fiber pad to stick it on the bottom of the upper pressure head (the surface that contacts the powder) and around the mold (the part that holds the powder);
[0089] (3) Laying the first layer of ceramic powder and pre-pressing
[0090] First, a 15 mm thick layer of 99 alumina ceramic granulation powder was spread in the dry pressing mold, and a unidirectional pressurization method was used, with a pre-pressing of 5 MPa for 30 seconds, and then the pressure was released to obtain the first pressed product;
[0091] Lift the upper pressing head and place the prepared lost foam in the center of the first pressed product;
[0092] (4) Lay the second layer of ceramic powder and complete the pressing
[0093] Lay 99 alumina ceramic granulation powder with a thickness of 22 mm, adopt a bidirectional pressurization method, use a pressure of 10 MPa to dry press for 40 seconds, and obtain a second pressed product;
[0094] (5) Cold isostatic pressing
[0095] The second pressed product is vacuum sealed and cold isostatically pressed at a pressure of 100 MPa for 200 seconds.
[0096] (6) Sintering
[0097] The cold isostatically pressed sample was sintered at 1620°C for 2 h to obtain hollow ceramics.
[0098] After testing, the ceramic surface of the embodiment after sintering has no cracks, no color difference, and no stratification. The inner wall of the airway is illuminated and observed to be transparent, without foreign matter, no black spots, and no additional coloring. The airtightness is good.
[0099] Example 3
[0100] (1) Prepare the lost foam:
[0101] Select 1mm thick graphite paper (purity of graphite paper 99.5%) as lost foam, and cut out a shape of 5mm, 10mm long and 1mm thick;
[0102] (2) Dry pressing mold adjustment:
[0103] Use a 1mm thick polyester fiber pad to stick it on the bottom of the upper pressure head (the surface that contacts the powder) and around the mold (the part that holds the powder);
[0104] (3) Laying the first layer of ceramic powder and pre-pressing
[0105] First, a 15 mm thick layer of 96 alumina ceramic granulation powder was spread in the dry pressing mold, and a unidirectional pressurization method was used, with a pre-pressing of 5 MPa for 30 seconds, and then the pressure was released to obtain a first pressed product;
[0106] Lift the upper pressing head and place the cut graphite paper pattern in the center of the first pressed product;
[0107] (4) Lay the second layer of ceramic powder and complete the pressing
[0108] Lay 96 alumina ceramic granulation powder with a thickness of 22 mm, adopt a bidirectional pressurization method, use a pressure of 10 MPa to dry press for 40 seconds, and obtain a second pressed product;
[0109] (5) Cold isostatic pressing
[0110] The second pressed product is vacuum sealed and cold isostatically pressed at a pressure of 100 MPa for 200 seconds.
[0111] (6) Sintering
[0112] The cold isostatically pressed sample was sintered at 1620°C for 2 h to obtain hollow ceramics.
[0113] After testing, the ceramic surface of the embodiment after sintering has no cracks, no color difference, and no stratification. The inner wall of the airway is illuminated and observed to be transparent, without foreign matter, no black spots, and no additional coloring. The airtightness is good.
[0114] Since 96 porcelain is very brittle, it is very easy to break or crack during CNC processing, resulting in a low yield rate. Therefore, there are very few ceramic robotic arms made of this material on the market. However, it can be successfully formed through the dry pressing method.
[0115] Comparative Example 1
[0116] (1) Prepare the lost foam:
[0117] Select 1mm thick graphite paper (purity 99.5%) as lost foam, and cut out the corresponding graphite paper shape according to the airway shape in the design drawing, such as Figure 3 As shown;
[0118] (2) Laying the first layer of ceramic powder and pre-pressing
[0119] First, a 15 mm thick layer of 99 alumina ceramic granulation powder was spread in the dry pressing mold, and a unidirectional pressurization method was used, with a pre-pressing of 5 MPa for 30 seconds, and then the pressure was released to obtain the first pressed product;
[0120] Lift the upper pressing head and place the cut graphite paper pattern in the center of the first pressed product;
[0121] (3) Lay the second layer of ceramic powder and complete the pressing
[0122] Lay 99 alumina ceramic granulation powder with a thickness of 22 mm, adopt a bidirectional pressurization method, use a pressure of 10 MPa to dry press for 40 seconds, and obtain a second pressed product;
[0123] (4) Cold isostatic pressing
[0124] The second pressed product is vacuum sealed and cold isostatically pressed at a pressure of 100 MPa for 200 seconds.
[0125] (5) Sintering
[0126] After being kept at 1620℃ for 2h, the product cracked.
[0127] Figure 5 This is a physical picture of the sample after cold isostatic pressing prepared in Comparative Example 1, which shows obvious stratification.
[0128] By comparing Example 1 with Comparative Example 1, it can be seen that if the dry pressing mold is not adjusted, obvious stratification will occur during pre-pressing, and the subsequent cold isostatic pressing process cannot eliminate this defect, and finally cracking will occur during the sintering process.
[0129] Comparative Example 2
[0130] (1) Prepare the lost foam:
[0131] Select 1mm thick graphite paper (Baoyue carbon material, purity 99%) as lost foam, and cut out the corresponding graphite paper shape according to the airway shape in the design drawing, such as Figure 3 As shown;
[0132] (2) Dry pressing mold adjustment:
[0133] Use a 1mm thick polyester fiber pad to stick it on the bottom of the upper pressure head (the surface that contacts the powder) and around the mold (the part that holds the powder);
[0134] (3) Laying the first layer of ceramic powder and pre-pressing
[0135] First, a 15 mm thick layer of 99 alumina ceramic granulation powder was spread in the dry pressing mold, and a unidirectional pressurization method was used, with a pre-pressing of 5 MPa for 30 seconds, and then the pressure was released to obtain the first pressed product;
[0136] Lift the upper pressing head and place the cut graphite paper pattern in the center of the first pressed product;
[0137] (3) Lay the second layer of ceramic powder and complete the pressing
[0138] Lay 99 alumina ceramic granulation powder with a thickness of 22 mm, adopt a bidirectional pressurization method, use a pressure of 10 MPa to dry press for 40 seconds, and obtain a second pressed product;
[0139] (4) Cold isostatic pressing
[0140] The second pressed product was vacuum sealed and subjected to cold isostatic pressing at a pressure of 100 MPa for 200 seconds.
[0141] (5) Sintering
[0142] The cold isostatically pressed sample was sintered at 1620°C for 2 h to obtain a hollow ceramic part.
[0143] Figure 6 This is a front view of the hollow ceramic prepared in Comparative Example 2. Figure 7 This is a side view of the hollow ceramic prepared in Comparative Example 2. Figures 6-7 It can be seen that there is no stratification on the side of the sample, but the air groove is colored red, and there is a partial collapse on the upper surface of the air groove.
[0144] By comparing Example 1 with Comparative Example 2, it can be seen that low purity of graphite paper will produce metal ion impurities and affect the accuracy of the pore grooves, thereby affecting the accuracy of the ceramic arm, and also affecting the cleanliness, limiting its use in wafer applications.
[0145] Comparative Example 3
[0146] (1) Prepare the lost foam:
[0147] Select 1mm thick graphite paper (purity 99.5%) as the lost foam and cut out 3×5×1mm 3 Graphite paper strips;
[0148] (2) Laying the first layer of ceramic powder and graphite paper
[0149] First, spread 15mm thick 99 alumina ceramic granulation powder in the dry pressing mold; place the cut graphite paper pattern in the center of the powder surface;
[0150] (3) Lay the second layer of ceramic powder and complete the pressing
[0151] Lay 99 alumina ceramic granulation powder with a thickness of 22 mm, use a two-way pressurization method, use a pressure of 10 MPa to dry press for 40 seconds, and obtain a pressed product;
[0152] (4) Cold isostatic pressing
[0153] The pressed product is vacuum sealed and cold isostatically pressed at a pressure of 100 MPa for 200 seconds.
[0154] (5) Sintering
[0155] After being kept at 1620℃ for 2h, the product cracked.
[0156] By comparing Example 1 with Comparative Example 3, it can be seen that without pre-pressing, due to the large difference in elasticity between the lost foam and the ceramic body, the lost foam will produce a larger rebound after dry pressing, resulting in obvious bulging on the top of the product. The subsequent cold isostatic pressing process cannot eliminate this defect, and cracks will occur during the sintering process.
[0157] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a ceramic robot arm by integrated dry pressing, The following steps are involved: A hard elastic component is attached to the upper pressing head of the dry pressing die to form a hard elastic pressing head; Laying a first layer of ceramic powder on the bottom of the dry pressing mold and performing pre-pressing to obtain a first pressed product; Placing the lost mold on the surface of the first pressed product, laying a second layer of ceramic powder, and performing dry pressing to obtain a second pressed product; cold isostatically pressing the second pressed product and then sintering it to obtain a ceramic robot arm; The lost mold is obtained by making the lost mold material into the shape required by the robot arm air groove.
2. The method for preparing a ceramic robot arm by dry pressing according to claim 1, It is characterized in that The lost foam material includes graphite paper, paraffin sheet or acrylic board.
3. The method for preparing a ceramic robot arm by dry pressing according to claim 2, It is characterized in that The purity of the graphite paper is ≥99.5%.
4. The method for preparing a ceramic robot arm by dry pressing according to claim 1, It is characterized in that The hard elastic component includes rubber or PU; the ceramic powder includes aluminum oxide powder or zirconium oxide powder.
5. The method for preparing a ceramic robot arm by dry pressing according to claim 1 or 4, It is characterized in that The thickness of the first layer of ceramic powder is 1 to 20 mm.
6. The method for preparing a ceramic robot arm by dry pressing according to claim 5, It is characterized in that The pre-pressing method is unidirectional pressurization; the pre-pressing pressure is 2-10 MPa, and the time is 30-100 s.
7. The method for preparing a ceramic robot arm by integrated dry pressing according to claim 1, It is characterized in that The thickness of the second layer of ceramic powder is 1 to 30 mm.
8. The method for preparing a ceramic robot arm by dry pressing according to claim 1 or 7, It is characterized in that The pressurization method of the dry pressing is bidirectional pressurization; the pressure of the dry pressing is 8 to 20 MPa, and the time is 40 to 100 seconds.
9. The method for preparing a ceramic robot arm by integrated dry pressing according to claim 1, It is characterized in that The cold isostatic pressing has a pressure of 50 to 200 MPa and a time of 100 to 500 seconds.
10. The method for preparing a ceramic robot arm by integrated dry pressing according to claim 1, It is characterized in that The sintering temperature is 1400-1620° C. and the sintering time is 30-300 minutes.
Citation Information
Patent Citations
Isostatic cool pressing molding die for ceramic tube and molding method
CN108372573A
Ceramic structure member and preparation method thereof
CN110655415A
Preparation method of ceramic arm based on hot die-casting molding
CN115849880A
Manufacturing method of aluminum oxide ceramic mechanical arm
CN117735959A
Method of forming ceramic ware
GB776798A