Graphene heat conduction film, preparation method thereof and thermal interface material

By using a mixed slurry of a porous substrate and graphene oxide with different degrees of oxidation in the graphene thermally conductive film, combined with high-temperature annealing thermal reduction and nanoparticle layers, the problem of insufficient longitudinal thermal conductivity of the graphene thermally conductive film is solved, and cost reduction and Improved performance for industrial production of thermal interface materials.

CN118812263APending Publication Date: 2024-10-22GUANGDONG AEROSPACE SCI & TECH RES INST (NANSHA)
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410657466.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-25
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing graphene thermal conductive film has insufficient longitudinal thermal conductivity and cannot meet the needs of thermal interface materials for efficient longitudinal heat dissipation. At the same time, the cost is high and it is not conducive to industrial production.

Method used

Using a porous substrate coating process, graphene oxide mixed slurries with different oxidation degrees are coated and carbonized and graphitized to form a graphene thermal conductive film, and a 3D thermal conductive network is established through high-temperature annealing and thermal reduction, combining nanoparticle layers and high-temperature Thermal conductivity adhesive to improve longitudinal thermal conductivity and mechanical properties.

Benefits of technology

It effectively improves the longitudinal thermal conductivity of graphene thermal conductive film, reduces production costs, and enhances the flexibility and mechanical properties of the material to meet the needs of industrial production and practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004858444070000121
    Figure BDA0004858444070000121
  • Figure HDA0004858444080000011
    Figure HDA0004858444080000011
  • Figure HDA0004858444080000012
    Figure HDA0004858444080000012
Patent Text Reader

Abstract

The invention relates to the technical field of heat conduction materials, and particularly discloses a graphene heat conduction film, a preparation method thereof and a thermal interface material. The preparation method of the graphene heat-conducting film specifically comprises the following steps: coating a porous substrate with graphene oxide mixed slurry, and performing carbonization and graphitization to obtain the graphene heat-conducting film, the graphene oxide mixed slurry comprises graphene oxide with different oxidation degrees. The thermal interface material at least comprises a first graphene heat-conducting film, a second graphene heat-conducting film and a nanoparticle layer which is stacked between the first graphene heat-conducting film and the second graphene heat-conducting film and used for anchoring the first graphene heat-conducting film and the second graphene heat-conducting film, and an adhesive is also arranged between the first graphene heat-conducting film and the second graphene heat-conducting film. The graphene in the prepared graphene heat-conducting film is arranged in the longitudinal direction, has good heat-conducting and electric-conducting performance in the longitudinal direction, and can effectively solve the problem of longitudinal heat conduction of an interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of thermally conductive materials, and more specifically, to a graphene thermally conductive film and a preparation method thereof, and a thermal interface material. Background Art

[0002] Graphene has good thermal conductivity and has broad application prospects. A common process for preparing graphene thermal conductive films is to arrange and assemble graphene oxide into graphene oxide films and then perform high-temperature treatment to prepare graphene thermal conductive films. Specifically, existing graphene thermal conductive films are generally prepared by coating graphene oxide slurry into a film, foaming it through high-temperature treatment to form a graphene foam film, and then calendering to obtain a graphene thermal conductive film.

[0003] As for graphene oxide slurry, the graphene oxide currently used is graphene oxide obtained by chemical oxidation of graphite, which has rich oxygen-containing functional groups and generally has a carbon content of about 50%, belonging to strong graphene oxide. The oxidation degree of strong graphene oxide is relatively high, with many oxygen-containing functional groups, and the sheets can be peeled thinner. Strong graphene oxide is more orderly when assembled into a film, and the assembly effect is good. However, the carbon content of strong graphene oxide is low, and the amount of graphene obtained after high-temperature treatment is small, so the cost is high and it is not conducive to industrial production.

[0004] Compared with strong graphene oxide, weak graphene oxide has a high carbon content, generally above 80%. However, weak graphene oxide has a low degree of oxidation, contains fewer oxygen functional groups, and has more layers when peeled off. If only weak graphene oxide is used for film assembly, a highly oriented structure cannot be obtained during film formation, and the order is poor, which affects the thermal conductivity of the graphene thermal conductive film prepared after high-temperature treatment. Therefore, selecting a single degree of oxidation graphene oxide to configure the slurry cannot produce a graphene thermal conductive film suitable for industrial production and with good thermal conductivity.

[0005] For graphene thermal conductive film, it has super high thermal conductivity in the horizontal direction, but its thermal conductivity in the vertical direction is not ideal. This is due to the difference caused by the high orientation of graphene in the horizontal direction. In many application scenarios, such as thermal interface materials, in order to facilitate efficient and rapid heat conduction in the vertical direction, it is often necessary to obtain higher thermal conductivity in the vertical direction, which requires the graphene thermal conductive film to have a higher thermal conductivity in the vertical direction. In this regard, the existing graphene thermal conductive film can no longer meet the requirements of such application scenarios, and a new preparation method is needed to obtain a graphene thermal conductive film with high thermal conductivity in the vertical direction.

[0006] The thermal conductivity of traditional thermal interface materials is usually only 4-5W / mK in the vertical direction. In order to solve this problem, researchers have made great efforts to develop high-performance thermal interface materials based on carbon materials (e.g., graphene nanosheets, carbon nanotubes, and carbon fibers). In current research, the thermal conductivity of thermal interface materials is usually increased by increasing the graphene loading in graphene-based thermal conductive adhesives. However, when the graphene content is high, it is not practical for the manufacturing process of thermal interface materials.

[0007] Faced with the problem of needing to improve the thermal conductivity of thermal interface materials in the vertical direction, it is essential to assemble graphene into a vertically oriented structure to promote heat dissipation in the normal direction of the contact solid interface. In addition, due to the high stiffness and weak interlayer bonding strength of graphite, the vertically assembled graphite composite material shows high hardness and is relatively brittle in the direction perpendicular to the assembly direction. Therefore, it is necessary to prepare a new type of thermal interface material that has both good thermal conductivity and certain flexibility for practical application. Summary of the invention

[0008] In order to provide a thermal interface material having both excellent thermal conductivity and flexibility, the present application provides a graphene thermal conductive film and a preparation method thereof, and a thermal interface material.

[0009] In a first aspect, the present application provides a method for preparing a graphene thermally conductive film, which adopts the following technical solution:

[0010] A method for preparing a graphene thermally conductive film, the preparation method specifically comprising the following steps:

[0011] The graphene oxide mixed slurry is coated on a porous substrate, and carbonized and graphitized to obtain a graphene thermal conductive film; the graphene oxide mixed slurry includes graphene oxide with different oxidation degrees.

[0012] Since the porous substrate coating process is used in the present application, the graphene in the prepared graphene thermal conductive film is arranged longitudinally, and has good thermal and electrical conductivity in the longitudinal direction, which can effectively solve the problem of longitudinal heat conduction at the interface. In addition, after the porous substrate is carbonized, the pore wall is carbonized into a mesh structure of carbonaceous fibers, which can further enhance the longitudinal arrangement of graphene, making its structure and mechanical properties more stable.

[0013] The present application adopts at least two different degrees of graphene oxide to mix and prepare the graphene thermal conductive film. The strong graphene oxide is rich in functional groups and has good assembly order, while the weak graphene oxide has a high carbon content, so that the prepared graphene thermal conductive film is thicker and the final residual carbon ratio is increased, which can improve production efficiency and effectively reduce costs.

[0014] In the present application, the graphene oxide mixed slurry includes graphene oxide with different oxidation degrees. The reasons are as follows: the graphene oxide currently used generally has a carbon content of about 50%, which belongs to strong graphene oxide. The oxidation degree of strong graphene oxide is relatively high, it contains many oxygen functional groups, and the flakes can be peeled off thinner. Strong graphene oxide is more orderly when assembled into a film, and the assembly effect is good. However, the carbon content of strong graphene oxide is low, and the amount of graphene obtained after high-temperature treatment is small, so the cost is high and it is not conducive to industrial production. Compared with strong graphene oxide, weak graphene oxide has a high carbon content, generally above 80%. However, weak graphene oxide has a low oxidation degree, contains few oxygen functional groups, and has a large number of layers when peeled off. If only weak graphene oxide is used for film assembly, a highly oriented structure cannot be obtained during film formation, and the orderliness is poor, thereby affecting the thermal conductivity of the graphene thermal conductive film prepared after high-temperature treatment. Therefore, in order to prepare a graphene thermally conductive film suitable for industrial production and having good thermal conductivity, the present application adopts a mixed slurry.

[0015] In addition, in order to solve the agglomeration problem when strong graphene oxide and weak graphene oxide are mixed in solution, the preparation of mixed slurry is to prepare strong graphene oxide dispersion and weak graphene oxide dispersion respectively, and then two dispersions are mixed.Due to the different oxidation degrees of two kinds of graphene oxide, the amount of-COOH contained therein is different, when adding alkali to the dispersion containing strong graphene oxide and weak graphene oxide simultaneously and neutralizing, it will cause-COOH and alkali reaction uneven, thereby causing the poor dispersion effect of strong graphene oxide and weak graphene oxide.Therefore, the present application first disperses two kinds of graphene oxide respectively, and after each adds alkali to fully neutralize the-COOH group on graphene oxide, the two are mixed again, effectively avoiding the above-mentioned problem of uneven dispersion.

[0016] Optionally, the porous substrate has at least one or more of the following features (a)-(d):

[0017] (a) the holes of the porous substrate are vertical through holes extending longitudinally along the porous substrate;

[0018] (b) the holes of the porous substrate are through holes that are inclined with respect to the horizontal plane of the porous substrate;

[0019] (c) the porous substrates are multiple and uniformly arranged in an array;

[0020] (d) The porous substrate is a polyimide porous material.

[0021] In a specific embodiment, the porous substrate is multiple and evenly arranged in an array, and the holes of the porous substrate are vertical through holes extending longitudinally along the porous substrate.

[0022] In a specific embodiment, the porous substrate is multiple and evenly arranged in an array, and the holes of the porous substrate are through holes that are inclined with respect to the horizontal plane of the porous substrate.

[0023] When the pore size of the porous substrate extends in the longitudinal direction, it is beneficial to fix the graphene oxide in the longitudinal direction, thereby improving the thermal conductivity of the graphene thermal conductive film in the vertical direction.

[0024] When the aperture of the porous substrate is tilted, when the tilt angle of the aperture is greater than 45°, it is beneficial to the heat dissipation of the graphene thermal conductive film in the horizontal direction; when the tilt angle of the aperture is less than 45°, it is beneficial to the heat dissipation of the graphene thermal conductive film in the vertical direction.

[0025] In addition, when the material of the porous substrate is polyimide, after carbonization, the pore wall of the substrate will be carbonized into a fiber network structure, which can play a role in strengthening the longitudinally arranged graphene oxide, thereby making the structure and mechanical properties of the graphene thermal conductive film more stable.

[0026] Optionally, the graphene oxide mixed slurry has at least one or more of the following features (e)-(i):

[0027] (e) the graphene oxide mixed slurry comprises at least two graphene oxides with different oxidation degrees;

[0028] (f) the solid content of graphene oxide in the graphene oxide mixed slurry is 4.5-8%;

[0029] (g) In the graphene oxide mixed slurry, the solvent is any one or more of water, NMP, and DMF;

[0030] (h) in the graphene oxide mixed slurry, weak graphene oxide accounts for 5-50% by weight of the graphene oxide, and strong graphene oxide accounts for 50-95% by weight of the graphene oxide;

[0031] (i) In the graphene oxide mixed slurry, the carbon content of the weak graphene oxide is 80-90%, and the carbon content of the strong graphene oxide is 45-55%.

[0032] The graphene oxide mixed slurry can be prepared by mixing a strong graphene oxide and a weak graphene oxide in a solvent, or by mixing three or more graphene oxides with different oxidation degrees.

[0033] When the graphene oxide mixed slurry is prepared from two graphene oxides with different oxidation degrees, the solvent may be any one of water, NMP, and DMF, or a mixed solvent of two or more thereof.

[0034] In a specific embodiment, the solid content of graphene oxide in the graphene oxide mixed slurry is 4.5%, 5%, 6%, 6.5%, 7%, or 8%.

[0035] In some specific embodiments, the solid content of graphene oxide in the graphene oxide mixed slurry is 4.5-5%, 4.5-6%, 4.5-6.5%, 4.5-7%, 5-6%, 5-6.5%, 5-7%, 5-8%, 6-6.5%, 6-7%, 6-8%, 6.5-7%, 6.5-8%, and 7-8%.

[0036] In a specific embodiment, the weak graphene oxide accounts for 5%, 15%, 20%, 35%, 40%, or 50% of the weight of the graphene oxide.

[0037] In some specific embodiments, weak graphene oxide accounts for 5-15%, 5-20%, 5-35%, 5-40%, 15-20%, 15-35%, 15-40%, 15-50%, 35-40%, 35-50%, 40-50% of the weight of the graphene oxide.

[0038] In a specific embodiment, the strong graphene oxide accounts for 50%, 60%, 65%, 80%, 85%, or 95% of the weight of the graphene oxide.

[0039] In some specific embodiments, the strong graphene oxide accounts for 50-60%, 50-65%, 50-80%, 50-85%, 60-65%, 60-80%, 60-85%, 60-95%, 80-85%, 80-95%, 85-95% of the weight of the graphene oxide.

[0040] Optionally, the method for preparing the polyimide porous material specifically comprises the following steps:

[0041] The polyamic acid solution and the dispersion liquid containing the pore-forming sacrificial material and prepared by using an organic solvent are mixed and ultrasonically treated to prepare a membrane-forming liquid;

[0042] and coating the film-forming liquid on the surface of the substrate and drying it to obtain an organic-inorganic composite film;

[0043] The organic-inorganic composite membrane is placed in a template remover to react and remove the pore-forming sacrificial material to obtain a polyimide porous material.

[0044] Optionally, the method for preparing the polyimide porous material has at least one or more of the following features (j)-(o):

[0045] (j) the pore-forming sacrificial material is inorganic nanoparticles;

[0046] (k) In the dispersion, the weight ratio of the pore-forming sacrificial material to the organic solvent is (0.05-0.5):1;

[0047] (l) In the membrane-forming solution, the weight ratio of the pore-forming sacrificial material to the polyimide is (0.3-2):1;

[0048] (m) the template removing agent is an acid solution, including any one or more of hydrochloric acid, hydrofluoric acid, sulfuric acid, nitric acid, acetic acid and formic acid;

[0049] (n) The template removing agent is an acid solution, and the concentration of the acid solution is 5-40wt%.

[0050] In a specific embodiment, in the dispersion, the weight ratio of the inorganic nanoparticles to the organic solvent is (0.05-0.5):1.

[0051] In a specific embodiment, in the membrane-forming solution, the weight ratio of the inorganic nanoparticles to the polyimide is (0.3-2):1.

[0052] Optionally, the inorganic nanoparticles are any one or more of nano silicon dioxide (SiO2), nano titanium dioxide (TiO2), nano aluminum oxide (AI2O3), nano calcium carbonate (CaCO3), nano magnesium hydroxide (Mg(OH)2), nano magnesium oxide (MgO), nano magnesium carbonate (MgCO3), nano barium carbonate (BaCO3), nano zinc hydroxide (Zn(OH)2) and nano zinc carbonate (ZnCO3).

[0053] Optionally, the template removing agent is a substance that chemically reacts with the pore-forming sacrificial material to remove the pore-forming sacrificial material and does not react with polyimide.

[0054] Optionally, the template removing agent may be an acid solution, including any one or more of hydrochloric acid, hydrofluoric acid, sulfuric acid, nitric acid, acetic acid and formic acid.

[0055] Optionally, the concentration of the acid solution is 5-40wt%.

[0056] In the method for preparing the graphene thermal conductive film, the carbonization and graphitization treatment includes high-temperature annealing and thermal reduction, and the process is related to the equipment used.

[0057] In a specific embodiment, when a connected furnace is used, the high temperature annealing and thermal reduction specifically includes the following:

[0058] The first stage: heating from room temperature to 900-1500°C at a heating rate of 1-10°C / min in an argon / nitrogen atmosphere;

[0059] The second stage: heating to 2800-3200°C at a heating rate of 5-20°C / min under argon atmosphere, and then naturally cooling to room temperature;

[0060] In a specific embodiment, when a split furnace is used, the high temperature annealing thermal reduction specifically includes the following:

[0061] The first stage: in an argon / nitrogen atmosphere, the temperature is raised from room temperature to 900-1500°C at a heating rate of 1-10°C / min, and then naturally cooled to room temperature;

[0062] The second stage: in an argon atmosphere, the temperature is raised from room temperature to 2800-3200°C at a heating rate of 5-20°C / min, and then naturally cooled to room temperature.

[0063] Through high-temperature annealing and thermal reduction, a 3D thermal conductive network was established in the graphene thermal conductive film, which improved the overlapping problem between graphene sheets and thereby increased the thermal conductivity of the graphene thermal conductive film.

[0064] In a specific embodiment, in the first stage, the temperature is increased from room temperature to 1200° C. at a heating rate of 5° C. / min in an argon atmosphere / nitrogen atmosphere, and then naturally cooled to room temperature.

[0065] In a specific embodiment, the second stage: heating from room temperature to 3100° C. at a heating rate of 10° C. / min under an argon atmosphere, and then naturally cooling to room temperature.

[0066] In a second aspect, the present application provides a graphene thermally conductive film prepared using the above-mentioned preparation method.

[0067] In a third aspect, the present application provides a thermal interface material prepared by the above-mentioned preparation method, using the following technical solution:

[0068] A thermal interface material comprises at least: a first graphene thermal conductive film, a second graphene thermal conductive film, and a nanoparticle layer stacked between the first graphene thermal conductive film and the second graphene thermal conductive film for anchoring the two; an adhesive is also arranged between the first graphene thermal conductive film and the second graphene thermal conductive film.

[0069] The present application uses an adhesive containing high thermal conductivity nanoparticles to bond graphene thermal conductive films, and the thermal interface material obtained is a thicker thermal conductive film to meet the requirements of high-flux heat dissipation. On the one hand, since the thermal conductivity of high thermal conductivity nanoparticles themselves is better than that of simple adhesives, the use of adhesives containing high thermal conductivity nanoparticles can effectively improve the longitudinal thermal conductivity of thermal interface materials; on the other hand, the use of adhesives containing high thermal conductivity nanoparticles can also enhance the mechanical properties of thermal interface materials.

[0070] Optionally, the thermal interface material has at least one or more of the following features (o)-(q):

[0071] (o) the nanoparticles in the nanoparticle layer comprise needle-shaped nanoparticles or spider-shaped nanoparticles;

[0072] (p) the adhesive comprises any one or more of polyurethane, silicone rubber, polyimide, epoxy resin and polyacrylic resin;

[0073] (q) The adhesive is a silicone rubber-based transparent polymer having high elasticity.

[0074] Optionally, the nanoparticles in the nanoparticle layer include needle-shaped nanoparticles, and the needle-shaped nanoparticles are configured to anchor the first graphene thermally conductive film to the second graphene thermally conductive film.

[0075] Optionally, the needle-shaped nanoparticles include any one of Al2O3, SiO2, Fe2O3, NiO2, Cr2O3, ZnO, Ag, Al, Cu, Ni, Cr, Ti, Mo, Fe, Mg and Li.

[0076] Needle-shaped nanoparticles can be used to greatly enhance the adhesion between adjacent layers of graphene thermally conductive films.

[0077] Alternatively, the nanoparticle may also have a spider-like shape in which many needle-like structures protrude from a central portion.

[0078] Optionally, the length of the needle-shaped nanoparticles may be in the range of 5-100 nm.

[0079] Optionally, the spider-shaped nanoparticles will have a diameter in the range of about 5-200 nm.

[0080] The adhesive can be cured under external pressure and heat, so that the first graphene thermal conductive film, the nanoparticle layer and the second graphene thermal conductive film are tightly bonded, thereby forming a laminated graphene-based thermal interface material.

[0081] Optionally, the adhesive includes any one or more of polyurethane, silicone rubber, polyimide, epoxy resin and polyacrylic resin.

[0082] Optionally, the adhesive is a silicone rubber-based transparent polymer having high elasticity.

[0083] The use of a transparent polymer based on silicone rubber can improve the flexibility and compression ratio of the assembled graphene thermal conductive film structure. When preparing the thermal interface material, the adhesive can be printed, dispensed or sprayed onto the graphene thermal conductive film. For example, screen printing or template printing can be used for printing.

[0084] Alternatively, the flexibility and thermal properties of the thermal interface material can be controlled by controlling the ratio between the adhesive and the graphene thermal conductive film. For example, in applications exposed to external pressure or with a greater risk of cracking, a graphene thermal conductive film with high flexibility is required.

[0085] In summary, this application has the following beneficial effects:

[0086] Since the porous substrate coating process is used in the present application, the graphene in the prepared graphene thermal conductive film is arranged longitudinally, and has good thermal and electrical conductivity in the longitudinal direction, which can effectively solve the problem of longitudinal heat conduction at the interface. In addition, after the porous substrate is carbonized, the pore wall is carbonized into a mesh structure of carbonaceous fibers, which can further enhance the longitudinal arrangement of graphene, making its structure and mechanical properties more stable.

[0087] The present application adopts at least two different degrees of graphene oxide to mix and prepare the graphene thermal conductive film. The strong graphene oxide is rich in functional groups and has good assembly order, while the weak graphene oxide has a high carbon content, so that the prepared graphene thermal conductive film is thicker and the final residual carbon ratio is increased, which can improve production efficiency and effectively reduce costs.

[0088] In the thermal interface material of the present application, nanoparticles are configured to anchor the first graphene thermally conductive film to the second graphene thermally conductive film. The use of anchored nanoparticles can be used to greatly enhance the adhesion between adjacent layers of the graphene thermally conductive film. In addition, the adhesive used in the present application to bond the graphene films together can be a silicone rubber-based polymer with high elastic properties. The use of silicone rubber-based polymers can improve the flexibility and compression ratio of the assembled graphene film structure. The flexibility and thermal properties of the film can be controlled by controlling the ratio between the adhesive and the graphene film layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0089] Figure 1 The process flow chart of the preparation method of polyimide porous material.

[0090] Figure 2 The process flow chart of the method for preparing graphene oxide mixed slurry.

[0091] Figure 3 The present invention is a process flow chart of the preparation method of polyimide-graphene oxide composite board.

[0092] Figure 4 This is the process flow chart for carbonization and graphitization treatment.

[0093] Figure 5 Schematic diagram of thermal interface material molding. DETAILED DESCRIPTION

[0094] Before describing the embodiments of the present application in detail, it should be understood that the terms used herein are only used for the purpose of describing specific embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by ordinary technicians in the field to which the terms belong.

[0095] The present application provides a graphene thermal conductive film and a preparation method thereof.

[0096] The preparation method specifically comprises the following steps:

[0097] (1) preparing a graphene oxide mixed slurry by mixing graphene oxide dispersions with different oxidation degrees and then evaporating them;

[0098] (2) coating the graphene oxide mixed slurry on the porous substrate;

[0099] (3) Carbonizing and graphitizing the coated porous substrate to obtain a graphene thermal conductive film.

[0100] In a specific embodiment, the porous substrate may be a polyimide porous material.

[0101] In a specific embodiment, reference Figure 1 , a method for preparing a porous polyimide material, comprising the following steps:

[0102] (1) preparing a polyamic acid solution using monomers;

[0103] (2) using inorganic nanoparticles as pore-forming sacrificial materials, firstly treating the inorganic nanoparticles with a surface treatment agent in an organic solvent, drying them, and then adding them to a polar solvent to disperse the inorganic nanoparticles in the organic solvent to prepare a dispersion;

[0104] (3) mixing the polyamic acid solution with the dispersion and subjecting the mixture to ultrasonic treatment to obtain a membrane-forming solution, i.e., an organic-inorganic mixed solution;

[0105] (4) coating the film-forming liquid on the surface of the substrate and drying it to form an organic-inorganic composite film;

[0106] (5) placing the organic-inorganic composite membrane in a template remover solution to react and remove the inorganic nanoparticles to obtain a polyimide porous material.

[0107] In a specific embodiment, the monomers in step (1) are dianhydride and diamine.

[0108] In a specific embodiment, the solid content of the monomer in the organic-inorganic mixed solution in step (3) is in the range of 15-30%.

[0109] In a specific embodiment, the polar solvent in step (2) is DMAc, NMP or DMF.

[0110] In a specific embodiment, the organic solvent in step (2) is water or an alcohol solution.

[0111] In a specific embodiment, the surface treatment agent in step (2) is any one or more of LAS (alkylbenzene sulfonate), AES (fatty alcohol polyoxyethylene ether sulfate), MES (α-sulfonic acid fatty acid salt), AOS (α-olefin sulfonate), alkyl polyoxyethylene ether, alkylphenol polyoxyethylene ether, fatty acyl diethanolamine, amino acid type, betaine type, etc.

[0112] In a specific embodiment, the method for preparing the polyimide porous material comprises the following steps:

[0113] (1) Inorganic nanoparticles are used as pore-forming sacrificial materials, the inorganic nanoparticles are first surface treated with a surface treatment agent in an organic solvent, and then added to a polar solvent after drying, so that the inorganic nanoparticles are dispersed in the organic solvent to prepare a dispersion;

[0114] (2) preparing a membrane-forming liquid, i.e., an organic-inorganic mixed liquid, by using monomers in the above-mentioned dispersion;

[0115] (3) coating the film-forming liquid on the surface of the substrate and drying it to form an organic-inorganic composite film;

[0116] (4) placing the organic-inorganic composite membrane in a template remover solution to react and remove the inorganic nanoparticles to obtain a polyimide porous material.

[0117] In a specific embodiment, reference Figure 2 , a method for preparing a graphene oxide mixed slurry specifically comprises the following steps:

[0118] Alkali is added to strong graphene oxide and weak graphene oxide respectively to fully neutralize -COOH, thereby obtaining strong graphene oxide dispersion and weak graphene oxide dispersion respectively, and then the two dispersions are mixed and evaporated to obtain graphene oxide mixed slurry; the solid content of graphene oxide in the graphene oxide mixed slurry is 4.5-8%.

[0119] In a specific embodiment, the base can be a base that is easily soluble in water, such as NaOH, KOH, Na2CO3, NaHCO3, K2CO3, KHCO3, and ammonia water.

[0120] In a specific embodiment, reference Figure 3 , a method for preparing a polyimide-graphene oxide composite plate, specifically comprising the following steps:

[0121] The obtained graphene oxide mixed slurry is coated on the polyimide porous material by using a scraper and a propulsion device to obtain a polyimide-graphene oxide composite plate. The angle of the scraper relative to the porous substrate and the speed of the propulsion device can be adjusted according to the distribution of pore sizes.

[0122] In a specific embodiment, reference Figure 4 The treatment of carbonization and graphitization includes high temperature annealing and thermal reduction. When a split furnace is used, the specific steps include:

[0123] The first stage: in an argon / nitrogen atmosphere, the temperature is raised from room temperature to 900-1500°C at a heating rate of 1-10°C / min, and then naturally cooled to room temperature;

[0124] The second stage: in an argon atmosphere, the temperature is raised from room temperature to 2800-3200°C at a heating rate of 5-20°C / min, and then naturally cooled to room temperature.

[0125] The present application also provides a thermal interface material,

[0126] refer to Figure 5 The thermal interface material at least comprises: a first graphene thermal conductive film, a second graphene thermal conductive film, and a nanoparticle layer stacked between the first graphene thermal conductive film and the second graphene thermal conductive film for anchoring the two. Furthermore, an adhesive is also arranged between the first graphene thermal conductive film and the second graphene thermal conductive film.

[0127] In order to make the purpose, technical solutions and advantages of this application clearer, the technical solutions in the embodiments of this application are clearly and completely described below in conjunction with the accompanying drawings. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of this application.

[0128] The present application is further described in detail below in combination with embodiments, comparative examples and performance test results.

[0129] Example

[0130] Example 1

[0131] This embodiment provides a method for preparing a graphene thermal conductive film.

[0132] The preparation method specifically comprises the following steps:

[0133] (1) Preparation of graphene oxide mixed slurry

[0134] The graphene oxide mixed slurry includes strong graphene oxide and weak graphene oxide, wherein the carbon content of the strong graphene oxide is 50%, and the carbon content of the weak graphene oxide is 80%.

[0135] Ammonia water is added to strong graphene oxide and weak graphene oxide respectively, with water as the solvent, to fully neutralize -COOH until the pH value of the solution is greater than 8 (weakly alkaline), thereby preparing strong graphene oxide dispersion and weak graphene oxide dispersion respectively.

[0136] The strong graphene oxide dispersion and the weak graphene oxide dispersion are mixed and evaporated to obtain a graphene oxide mixed slurry, wherein the solid content of graphene oxide in the graphene oxide mixed slurry is 5%, the strong graphene oxide accounts for 95% of the weight of the graphene oxide, and the weak graphene oxide accounts for 5% of the weight of the graphene oxide.

[0137] (2) Preparation of porous substrate

[0138] Inorganic nanoparticles are used as pore-forming sacrificial materials. The inorganic nanoparticles are first surface treated by LAS in an alcohol solution, and then added to DMAc after drying to disperse the inorganic nanoparticles in DMAc to prepare a dispersion. The inorganic nanoparticles are nano-silicon dioxide.

[0139] PMDA (pyromellitic anhydride) and ODA (4,4'-diaminodiphenyl ether) are used to prepare a film-making solution in the above-mentioned dispersion. The solid content of PMDA (pyromellitic anhydride) and ODA (4,4'-diaminodiphenyl ether) ranges from 15 to 30%, and the solid content of the inorganic nanoparticles ranges from 0.5 to 5%. In this embodiment, the solid content of PMDA (pyromellitic anhydride) and ODA (4,4'-diaminodiphenyl ether) ranges from 20%, and the solid content of the inorganic nanoparticles is 2%.

[0140] The film-forming liquid is coated on the surface of the substrate and dried to form an organic-inorganic composite film;

[0141] The organic-inorganic composite film is placed in a template remover solution to react and remove the inorganic nanoparticles to obtain a polyimide porous material. The release agent is 10 wt% hydrochloric acid.

[0142] (3) Coating of graphene oxide mixed slurry

[0143] The graphene oxide mixed slurry prepared above was coated on the polyimide porous material by using a scraper and a propulsion device to prepare a polyimide-graphene oxide composite plate with a thickness of 50 μm.

[0144] (4) Carbonization and graphitization of coated porous substrate

[0145] The coated porous substrate was carbonized and graphitized to obtain a graphene thermal conductive film. The carbonization and graphitization were divided into two stages: the first stage: in an argon atmosphere, the temperature was raised from room temperature to 1200°C at a heating rate of 5°C / min, and then naturally cooled to room temperature; the second stage: in an argon atmosphere, the temperature was raised from room temperature to 3100°C at a heating rate of 10°C / min, and then naturally cooled to room temperature. The rolled thickness of the graphene thermal conductive film was 25μm.

[0146] Example 2-18

[0147] Embodiments 2-18 provide a method for preparing a graphene thermal conductive film. The difference between the above embodiment and embodiment 1 is that the parameters in the preparation method are different, as shown in Table 1. The details are as follows:

[0148] The difference between Example 2-9 and Example 1 is: the weight percentage of strong graphene oxide and weak graphene oxide in graphene oxide.

[0149] The difference between Examples 10-18 and Example 4 is: the solid content of graphene oxide in the graphene oxide mixed slurry.

[0150] Embodiment 19

[0151] Example 19 provides a method for preparing a graphene thermal conductive film. The difference between the above example and Example 4 lies in the preparation process of the porous substrate, which is as follows:

[0152] (1) A polyamic acid solution is prepared in the above dispersion using PMDA (pyromellitic dianhydride) and ODA (4,4'-diaminodiphenyl ether).

[0153] (2) Inorganic nanoparticles are used as pore-forming sacrificial materials. The inorganic nanoparticles are first surface treated with a surface treatment agent in an organic solvent, and then added to a polar solvent after drying to disperse the inorganic nanoparticles in the organic solvent to prepare a dispersion.

[0154] (3) The polyamic acid solution is mixed with the dispersion liquid, and subjected to ultrasonic treatment to obtain a membrane-forming liquid, i.e., an organic-inorganic mixed liquid, wherein the solid content of PMDA (pyromellitic anhydride) and ODA (4,4'-diaminodiphenyl ether) is in the range of 20%, and the solid content of the inorganic nanoparticles is in the range of 2%.

[0155] (4) The film-forming liquid is coated on the surface of the substrate and dried to form an organic-inorganic composite film.

[0156] (5) placing the organic-inorganic composite membrane in a template remover solution to react and remove the inorganic nanoparticles to obtain a polyimide porous material.

[0157] Comparative Example

[0158] Comparative Example 1-2

[0159] Comparative Examples 1-2 respectively provide a method for preparing a graphene thermal conductive film. The difference between the above comparative examples and Example 4 is that the graphene oxide mixed slurry contains only one degree of oxidation of graphene oxide, and no porous substrate is used, as shown in Table 1. The remaining steps are the same as Example 4.

[0160] Comparative Examples 3-4

[0161] Comparative Examples 3-4 respectively provide a method for preparing a graphene thermal conductive film. The difference between the above comparative examples and Example 4 is that the graphene oxide mixed slurry contains only one type of graphene oxide with one oxidation degree, as shown in Table 1. The remaining steps are the same as those in Example 4.

[0162] Comparative Example 5

[0163] Comparative Example 5 provides a method for preparing a graphene thermal conductive film. The difference between the comparative example and Example 4 is that no porous substrate is used in the graphene oxide mixed slurry, as shown in Table 1. The remaining steps are the same as those in Example 4.

[0164] Table 1 Partial parameters and test results of the preparation methods of the embodiments and comparative examples

[0165]

[0166]

[0167] Performance test 1

[0168] The thermal conductivity of the graphene thermal conductive films prepared in the above-mentioned embodiment and comparative example was tested using a laser thermal conductivity tester (model: LFA467). The test results are shown in Table 1.

[0169] As can be seen from Table 1, graphene oxide filling has little effect on the transverse thermal conductivity, but significantly improves the longitudinal thermal conductivity, and a larger content of weak graphene oxide is conducive to improving the longitudinal thermal conductivity, but it needs to be matched with strong graphene oxide to achieve a better filling effect. When weak graphene oxide accounts for 5-50% of the weight of the graphene oxide and strong graphene oxide accounts for 50-95% of the weight of the graphene oxide, the obtained graphene thermal conductive film has good longitudinal thermal conductivity. In addition, the solid content of strong graphene oxide in graphene oxide is higher, which is more conducive to processing.

[0170] Comparative Example 1-2 does not use mixed graphene oxide, nor does it use a porous substrate, so the scheme of Comparative Example 1-2 is basically not helpful for improving the longitudinal thermal conductivity of the graphene thermal conductive film. Comparative Example 1-2 does not use mixed graphene oxide, but uses a porous substrate. Compared with Comparative Example 1-2, the longitudinal thermal conductivity of the graphene thermal conductive film obtained is improved, but it is still worse than that of Example 4, indicating that the use of mixed graphene oxide is beneficial to improving the longitudinal thermal conductivity of the graphene thermal conductive film. Although Comparative Example 5 uses mixed graphene oxide, it does not use a porous substrate. The longitudinal thermal conductivity of the graphene thermal conductive film obtained is close to that of Comparative Example 1-2. Compared with Example 4, it is shown that the use of a porous substrate is beneficial to improving the longitudinal thermal conductivity of the graphene thermal conductive film. Based on the above, it is shown that the joint action of the porous substrate and mixed graphene oxide can effectively improve the longitudinal thermal conductivity of the graphene thermal conductive film.

[0171] Performance test 2

[0172] The thermal conductivity of the thermal interface material prepared by using the graphene thermal conductive film obtained in Example 4 above was tested.

[0173] The preparation method of the thermal interface material is as follows: the thermal interface material at least includes: a first graphene thermal conductive film, a second graphene thermal conductive film (both of which are 25 μm thick thermal conductive films prepared in Example 4), and a nanoparticle layer stacked between the first graphene thermal conductive film and the second graphene thermal conductive film for anchoring the two. Furthermore, an adhesive is also provided between the first graphene thermal conductive film and the second graphene thermal conductive film. Here, the nanoparticles in the nanoparticle layer are Al2O3 needle-shaped nanoparticles with a length of 50 nm; the adhesive is polyurethane, and the total thickness after bonding is 60 μm.

[0174] The thermal conductivity of the prepared thermal interface material was tested using a laser thermal conductivity tester (model: LFA467). The transverse thermal conductivity of the thermal interface material was measured to be 1330 W / (m·K), and the longitudinal thermal conductivity was 32 W / (m·K). It can be seen that the use of the graphene thermal conductive film of the present application to prepare the thermal interface material can effectively improve the longitudinal thermal conductivity of the thermal interface material.

[0175] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for preparing a graphene thermally conductive film, characterized in that: The preparation method specifically comprises the following steps: The graphene oxide mixed slurry is coated on a porous substrate, and carbonized and graphitized to obtain a graphene thermal conductive film; the graphene oxide mixed slurry includes graphene oxide with different oxidation degrees.

2. The preparation method according to claim 1, characterized in that: The porous substrate has at least one or more of the following features (a) to (d): (a) the holes of the porous substrate are vertical through holes extending longitudinally along the porous substrate; (b) the holes of the porous substrate are through holes that are inclined with respect to the horizontal plane of the porous substrate; (c) the porous substrates are multiple and evenly arranged in an array; (d) The porous substrate is a polyimide porous material.

3. The preparation method according to claim 1, characterized in that: The graphene oxide mixed slurry has at least one or more of the following features (e)-(i): (e) the graphene oxide mixed slurry comprises at least two graphene oxides with different oxidation degrees; (f) the solid content of graphene oxide in the graphene oxide mixed slurry is 4.5-8%; (g) In the graphene oxide mixed slurry, the solvent is any one or more of water, NMP, and DMF; (h) in the graphene oxide mixed slurry, weak graphene oxide accounts for 5-50% by weight of the graphene oxide, and strong graphene oxide accounts for 50-95% by weight of the graphene oxide; (i) In the graphene oxide mixed slurry, the carbon content of the weak graphene oxide is 80-90%, and the carbon content of the strong graphene oxide is 45-55%.

4. The preparation method according to claim 2, characterized in that: The preparation method of the polyimide porous material specifically comprises the following steps: The polyamic acid solution and the dispersion liquid containing the pore-forming sacrificial material and prepared by using an organic solvent are mixed and ultrasonically treated to prepare a membrane-forming liquid; and coating the film-forming liquid on the surface of the substrate and drying it to obtain an organic-inorganic composite film; The organic-inorganic composite membrane is placed in a template remover to react and remove the pore-forming sacrificial material to obtain a polyimide porous material.

5. The preparation method according to claim 4, characterized in that: The method for preparing the polyimide porous material also has at least one or more of the following features (j)-(n): (j) the pore-forming sacrificial material is inorganic nanoparticles; (k) In the dispersion, the weight ratio of the pore-forming sacrificial material to the organic solvent is (0.05-0.5):1; (l) In the membrane-forming solution, the weight ratio of the pore-forming sacrificial material to the polyimide is (0.3-2):1; (m) the template removing agent is an acid solution, including any one or more of hydrochloric acid, hydrofluoric acid, sulfuric acid, nitric acid, acetic acid and formic acid; (n) The template removing agent is an acid solution, and the concentration of the acid solution is 5-40wt%.

6. The preparation method according to claim 5, characterized in that: The inorganic nanoparticles are any one or more of nano silicon dioxide, nano titanium dioxide, nano aluminum oxide, nano calcium carbonate, nano magnesium hydroxide, nano magnesium oxide, nano magnesium carbonate, nano barium carbonate, nano zinc hydroxide and nano zinc carbonate.

7. The preparation method according to claim 1, characterized in that: The carbonization and graphitization treatment includes high temperature annealing and thermal reduction, which specifically includes the following contents: The first stage: heating from room temperature to 900-1500°C at a heating rate of 1-10°C / min in an argon / nitrogen atmosphere; The second stage: heating to 2800-3200°C at a heating rate of 5-20°C / min under argon atmosphere, and then naturally cooling to room temperature; Or, the first stage: heating from room temperature to 900-1500°C at a heating rate of 1-10°C / min under an argon atmosphere / nitrogen atmosphere, and then naturally cooling to room temperature; The second stage: in an argon atmosphere, the temperature is raised from room temperature to 2800-3200°C at a heating rate of 5-20°C / min, and then naturally cooled to room temperature.

8. A graphene thermally conductive film prepared by the preparation method according to any one of claims 1 to 7.

9. A thermal interface material prepared using the graphene thermally conductive film according to claim 8, characterized in that: The thermal interface material at least includes: a first graphene thermally conductive film, a second graphene thermally conductive film, and a nanoparticle layer stacked between the first graphene thermally conductive film and the second graphene thermally conductive film for anchoring the two; an adhesive is also arranged between the first graphene thermally conductive film and the second graphene thermally conductive film.

10. The thermal interface material according to claim 9, characterized in that: The thermal interface material has at least one or more of the following features (o)-(q): (o) the nanoparticles in the nanoparticle layer include needle-shaped nanoparticles or spider-shaped nanoparticles; (p) the adhesive comprises any one or more of polyurethane, silicone rubber, polyimide, epoxy resin and polyacrylic resin; (q) The adhesive is a transparent polymer based on silicone rubber having high elasticity.

Citation Information

Patent Citations

  • Preparation method of polyimide micro-pore diaphragm

    CN103383996A

  • Mixed slurry of strong and weak graphene oxide, preparation method thereof, composite film of strong and weak graphene oxide, and preparation method of the composite film

    CN110482539A

  • Heat-conducting film and preparation method thereof

    CN113526957A

  • Graphite high-thermal-conductivity film and preparation method thereof

    CN113620711A

  • Graphene heat-conducting film, graphene heat-conducting sheet, preparation method and mold

    CN114573358A