Novel potassium sulfonate-containing flame retardant as well as preparation method and application thereof
Through the preparation of a new potassium-containing sulfonate flame retardant, the low flame retardant efficiency and high cost of polycarbonate are solved by using hexaphenoxycyclotriphosphazene and 50% fuming sulfuric acid sulfonation and potassium sulfate substitution reactions. solve the problem, achieve high-efficiency flame retardant effect and low impact on material performance, and are suitable for high-end applications.
Patent Information
- Application Number
- CN202410829840.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polycarbonate flame retardants have problems such as low flame retardant efficiency, impact on mechanical properties and transparency, and high cost during use. In particular, sulfonate and phosphazene flame retardants are added in large amounts to polycarbonate. , high cost and great impact on material properties.
Using a new potassium-containing sulfonate flame retardant, hexaphenoxy cyclotriphosphazene is sulfonated with 50% fuming sulfuric acid, barium carbonate is used to remove by-products, and potassium sulfate replaces barium ions to prepare hexaphenoxy cyclotriphosphazene. Potassium triphosphazene sulfonate (HPCTP-SK), this flame retardant has three elements of N, P and S, which are synergistically flame retardant. It has a novel structure, is non-toxic, heat and oxygen insulating, and is suitable for high-efficiency flame retardancy at low addition amounts.
The flame retardant efficiency of polycarbonate is significantly improved at low additive amounts, with an LOI value of 35.5% and passing the UL-94V-0 grade. It has little impact on the mechanical properties and transparency of the material, reducing the cost of use and the process is simple. Easy to operate.
Smart Images

Figure CN118812596A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardant synthesis, and in particular to a novel potassium sulfonate-containing flame retardant for polycarbonate, and a preparation method and application thereof. Background Art
[0002] Polycarbonate (PC) itself has certain flame retardancy and has been widely used in glass assembly, automobile, electrical and other fields. Its LOI value is 25%, and its vertical burning level reaches UL-94V-2. Although it is better than ordinary thermoplastic resins such as polyethylene and polypropylene, it drips severely when burning and releases a lot of toxic smoke, which cannot meet the application requirements of high-end fields such as medical equipment, electronic appliances, and automotive parts.
[0003] At present, the commonly used flame retardants for PC mainly include: inorganic boron series, metal hydroxide, silicon series, organic phosphorus series, sulfonate series and synergistic flame retardants, etc. Although they all show certain flame retardant effects, there are still defects of varying degrees in the process of use, such as: sulfonate series flame retardants are very efficient in flame retardant PC. Generally, a low addition amount can make the LOI value of the material reach about 35%, and pass the vertical combustion UL-94V-0 level, but sulfonate flame retardants will affect the mechanical properties of PC; phosphazene flame retardants are widely used in various flame retardant fields due to their high reactivity, high thermal stability and excellent flame retardant efficiency, but their disadvantages are large addition amount and high use cost. The addition amount in PC is generally 10wt%, basically maintained at 150,000 yuan / ton, while the unit price of PC is 10,000 yuan / ton. If compounded, it will increase the use cost of PC.
[0004] In summary, in view of the above problems, the present invention aims to provide a new flame retardant to overcome or alleviate at least one defect of the existing flame retardants. Summary of the invention
[0005] To solve the above problems, the present invention provides a novel potassium sulfonate-type flame retardant and a preparation method and application thereof; the flame retardant has a novel structure, is non-toxic, heat-insulating and oxygen-insulating, and the three elements of N, P and S are synergistic flame retardant, which greatly improves the flame retardant efficiency, can achieve a high flame retardant effect while adding a low amount, and reduce the impact on the mechanical properties and transparency of the PC substrate. The synthesis process is simple, easy to operate, and suitable for popularization and application.
[0006] The present invention is achieved through the following technical solutions:
[0007] A novel potassium sulfonate-type flame retardant, the flame retardant is a flame retardant for polycarbonate (PC); the flame retardant is compound I, and the chemical structure of compound I is as follows:
[0008]
[0009] The present invention also provides a preparation method of the novel potassium sulfonate-type flame retardant. The preparation method comprises the following steps: firstly, using hexaphenoxy cyclotriphosphazene and 50% fuming sulfuric acid as raw materials to realize one-step sulfonation; secondly, using barium carbonate as an acid scavenger to remove waste acid and combine barium ions with sulfonic acid groups; and finally, using potassium sulfate as a substituent to replace barium ions to obtain the compound I.
[0010] Furthermore, the preparation method specifically comprises the following steps:
[0011] Step 1: sulfonate hexaphenoxy cyclotriphosphazene with 50% fuming sulfuric acid as a sulfonating agent to obtain an acid solution of intermediate compound II, wherein the acid solution of intermediate compound II is an acid solution of benzenesulfonic acid oxycyclotriphosphazene. The reaction of this step is shown in the following formula (I):
[0012]
[0013] Step 2: using barium carbonate as a sulfate removal agent to remove the byproduct sulfuric acid in the sulfuric acid solution of the intermediate compound II in step 1, and simultaneously replacing the hydrogen ions in the hexabenzenesulfonyloxycyclotriphosphazene solution to obtain a salt solution of the intermediate compound II, wherein the hydrochloric acid solution of the intermediate compound II is a salt solution of benzenesulfonyloxycyclotriphosphazene;
[0014] Step 3: using 0.1 mol / L potassium sulfate as a barium ion replacing reagent to replace the barium ions in the salt solution of the intermediate compound II in step 2 to obtain a compound I solution, wherein the compound I solution is a potassium hexaphenoxycyclotriphosphazene sulfonate solution;
[0015] Step 4: Perform an evaporation experiment, evaporate the potassium hexaphenoxycyclotriphosphazene sulfonate solution in step 3 to obtain the compound I, which is potassium hexaphenoxycyclotriphosphazene sulfonate HPCTP-SK.
[0016] Furthermore, the specific content of the reaction in step 1 is:
[0017] Under the condition of 35-40° C., 50% fuming sulfuric acid is slowly added dropwise to the dichloromethane solution of hexaphenoxycyclotriphosphazene while stirring, wherein the solid-liquid ratio of hexaphenoxycyclotriphosphazene (g): dichloromethane (ml) is 1:12-17; the reaction end point is monitored by thin layer chromatography, and the reaction is terminated when there is no color development of hexaphenoxycyclotriphosphazene. After standing to room temperature, distilled water is added for liquid separation, and the upper layer liquid is taken to obtain an acid solution of the intermediate compound II.
[0018] Furthermore, the solid-liquid ratio of the hexaphenoxy cyclotriphosphazene to 50% oleum is: hexaphenoxy cyclotriphosphazene (g): 50% oleum (mL) = 1:0.2-1.2, and the optimal solid-liquid ratio is 1:0.5; a decrease in the concentration of oleum will affect the sulfonation effect.
[0019] Furthermore, the reaction temperature in step 1 is 35-40°C; the boiling point of dichloromethane is 39.8°C. During the reaction, attention should be paid to whether the solvent volatilization leads to too little solvent. If it is significantly reduced, the solvent should be replenished in time.
[0020] Furthermore, the reaction in step 1 is a sulfonation reaction, and multiple monitoring is required during the reaction process, with the time interval being as short as possible. The reaction endpoint is monitored by thin layer chromatography to avoid excessive sulfonation. The developing solvent is ethyl acetate and petroleum ether, and the volume ratio of ethyl acetate to petroleum ether is 1:2.
[0021] Further, distilled water was added, the liquids were separated, and the upper layer of liquid was taken to obtain an acid solution of the intermediate compound II.
[0022] Furthermore, dichloromethane was removed by liquid separation.
[0023] Furthermore, the obtained compound II is benzenesulfonic acid oxycyclotriphosphazene, and the acid solution of compound II is yellow.
[0024] Furthermore, the specific content of the step 2 reaction is:
[0025] The reaction temperature is 20-30°C, and a 500mL three-necked flask is used as a reactor; barium carbonate powder is added to the acid solution of compound II, and the pH value of the solution is measured. If the pH value is 7.0, the reaction is completed, and the solution is allowed to stand and filtered to remove insoluble matter; the filtrate is taken to obtain a salt solution of compound II.
[0026] Furthermore, in step 2, the mass ratio of compound II to barium carbonate powder is 1:15-20, which can be adjusted according to the actual reaction.
[0027] Furthermore, the barium carbonate powder in step 2 needs to be added slowly, with an addition amount of about 5.0 g each time, and the addition is completed according to the above ratio.
[0028] Furthermore, in the reaction of step 2, the supernatant is taken to track the reaction endpoint, a small amount of barium carbonate is added, and the pH value is observed. If the pH = 7.0, it is the reaction endpoint.
[0029] Furthermore, the reaction solution was heated and stirred at 20-30° C. for 20 minutes to accelerate sedimentation, and then filtered to remove insoluble matter after standing for 2 hours.
[0030] Further, the filtrate is taken to obtain a salt solution of compound II.
[0031] Furthermore, the salt solution of Compound II is light yellow.
[0032] Furthermore, the specific content of the step 3 reaction is:
[0033] The reaction temperature is 20-30°C, and a 500mL three-necked flask is used as a reactor; 0.1mol / L potassium sulfate is added dropwise to the salt solution of the intermediate compound II, and the supernatant is taken to detect the reaction progress. The reaction is completed when no precipitation is produced by adding 0.1mol / L potassium sulfate solution to the supernatant; stirring, standing, and filtering to remove insoluble matter, and taking the filtrate to obtain a solution of compound I.
[0034] Furthermore, in step 3, the barium ion content in the solution can be known based on the 0.1 mol / L potassium sulfate solution added dropwise.
[0035] Furthermore, in the reaction of step 3, the supernatant is taken to track the end point of the reaction, and the end point of the reaction is determined when no precipitation is generated by adding 0.1 mol / L potassium sulfate solution.
[0036] Furthermore, the reaction solution was allowed to stand for 2 h and then filtered to remove insoluble matter.
[0037] Further, the filtrate is taken to obtain a compound I solution.
[0038] Furthermore, the solution of Compound I is colorless.
[0039] Furthermore, the specific content of the step 4 reaction is:
[0040] The compound I solution is concentrated and dried, and the solvent is removed to obtain a crystalline product, which is then removed and ground into powder to obtain compound I.
[0041] Furthermore, the crystalline product is a white powder, namely compound I.
[0042] The present invention has the following beneficial technical effects:
[0043] (1) The present invention proposes that the three elements N, P, and S have synergistic flame retardancy, which greatly improves the flame retardant efficiency and can achieve a high flame retardant effect at a low addition amount. Under the condition of similar impact on the mechanical properties of PC, the flame retardant ability of the present invention is stronger than that of hexaphenoxycyclotriphosphazene (HPCTP). When the addition amount of this product is 0.1wt%, the LOI value of PC reaches 35.5% and passes the UL-94V-0 grade. When the addition amount of HPCTP is 0.1wt%, the LOI value is only 30.5%, which only passes the UL-94V-2 grade.
[0044] (2) It has little effect on the transparency of PC composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 Fourier transform infrared spectrum of compound I in the embodiment of the present invention.
[0046] Figure 2 The limiting oxygen index curve of the flame retardant potassium phenoxycyclotriphosphazene benzenesulfonate (HPCTP-SK) at different ratios in the embodiment of the present invention.
[0047] Figure 3 TGA and DTG graphs of the flame retardant potassium phenoxycyclotriphosphazene benzenesulfonate (HPCTP-SK) under a nitrogen atmosphere in an embodiment of the present invention.
[0048] Figure 4 TGA and DTG graphs of PC and PC / HPCTP-SK in nitrogen atmosphere in the embodiments of the present invention.
[0049] Figure 5 Flow chart of the preparation method described in an embodiment of the present invention. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments and the accompanying drawings of the specification. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0051] On the contrary, the present invention covers any substitution, modification, equivalent teaching method and scheme made on the essence and scope of the present invention as defined by the claims. Further, in order to make the public have a better understanding of the present invention, some specific details are described in detail in the detailed description of the present invention below. Those skilled in the art can fully understand the present invention without the description of these details.
[0052] It should be clear that the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0054] The embodiment provides a novel potassium sulfonate-type flame retardant, which is a flame retardant for polycarbonate (PC); the flame retardant is compound I, and the chemical structure of compound I is as follows:
[0055]
[0056] The present invention also provides a preparation method of the novel potassium-containing sulfonate flame retardant. The preparation method uses hexaphenoxy cyclotriphosphazene, 50% fuming sulfuric acid, barium carbonate and potassium sulfate as raw materials; 50% fuming sulfuric acid is used to sulfonate the hexaphenoxy cyclotriphosphazene, barium carbonate powder is used to remove waste acid, neutralization reaction is carried out, and 0.1 mol / L potassium sulfate is used to replace barium ions to obtain the compound I.
[0057] like Figure 5 As shown, the preparation method specifically comprises the following steps:
[0058] Step 1: 50% fuming sulfuric acid is used as a sulfonating agent to sulfonate hexaphenoxy cyclotriphosphazene to obtain an acid solution of the intermediate compound II, i.e., a phenoxy cyclotriphosphazene benzenesulfonic acid solution. The reaction of this step is shown in the following formula (I):
[0059]
[0060] Step 2: barium carbonate powder is used as a sulfate removal raw material to remove the byproduct sulfuric acid in the solution and replace the hydrogen ions in the sulfonic acid to obtain a salt solution of the intermediate compound II, i.e., a salt solution of phenoxycyclotriphosphazene benzenesulfonic acid;
[0061]
[0062] Step 3: Potassium sulfate is used as a substitution reagent to replace the barium ions in the salt solution of Compound II to obtain a solution of Compound I, i.e., potassium phenoxycyclotriphosphazene benzenesulfonate solution.
[0063]
[0064] Step 4: Concentrate and dry to obtain the compound I, namely potassium phenoxycyclotriphosphazenebenzenesulfonate (HPCTP-SK).
[0065] The specific content of the reaction in step 1 is:
[0066] Under the condition of 35-40° C., 50% fuming sulfuric acid is slowly added dropwise to the dichloromethane solution of hexaphenoxycyclotriphosphazene while stirring, wherein the solid-liquid ratio of hexaphenoxycyclotriphosphazene (g): dichloromethane (ml) is 1:12-17; the reaction end point is monitored by thin layer chromatography, and the reaction is terminated when there is no color development of hexaphenoxycyclotriphosphazene. After standing to room temperature, distilled water is added for liquid separation, and the upper layer liquid is taken to obtain an acid solution of the intermediate compound II.
[0067] In the step 1, the solid-liquid ratio of hexaphenoxy cyclotriphosphazene to 50% oleum is: hexaphenoxy cyclotriphosphazene (g): 50% oleum (mL) = 1:0.2-1.2, and the optimal solid-liquid ratio is 1:0.5; a decrease in the concentration of oleum will affect the sulfonation effect.
[0068] The reaction temperature in step 1 is 35-40°C; the boiling point of dichloromethane is 39.8°C. During the reaction, attention should be paid to whether the solvent volatilization leads to too little solvent. If it is significantly reduced, the solvent should be replenished in time.
[0069] The reaction in step 1 is a sulfonation reaction, which needs to be monitored multiple times during the reaction process with the time interval as short as possible. The reaction endpoint is monitored by thin layer chromatography to avoid excessive sulfonation. The developing solvent is ethyl acetate and petroleum ether, and the volume ratio of ethyl acetate to petroleum ether is 1:2.
[0070] When removing the solvent in step 1, dichloromethane is removed by liquid separation.
[0071] In the step 1, distilled water is added, and the upper layer of liquid is separated to obtain an acid solution of the intermediate compound II.
[0072] The acid solution of the compound II is yellow.
[0073] The specific content of the step 2 reaction is:
[0074] The reaction temperature is 20-30°C, and a 500mL three-necked flask is used as a reactor; barium carbonate powder is added to the acid solution of compound II, and the pH value of the solution is measured. If the pH value is 7.0, the reaction is completed, and the solution is allowed to stand and filtered to remove insoluble matter; the filtrate is taken to obtain a salt solution of compound II.
[0075] The mass ratio of compound II to barium carbonate powder in step 2 is 1:15-20, which can be adjusted according to the actual reaction.
[0076] In step 2, the barium carbonate powder needs to be added slowly, with an addition amount of about 5.0 g each time, and the addition is completed according to the above ratio.
[0077] In the reaction of step 2, the supernatant is taken to track the reaction endpoint, a small amount of barium carbonate is added, and the pH value is observed. If the pH is neutral, the reaction endpoint is reached.
[0078] In the step 2, the reaction solution is heated and stirred at 20-30° C. for 20 minutes to accelerate sedimentation, and then filtered to remove insoluble matter after standing for 2 hours.
[0079] The filtrate in step 2 is taken to obtain a salt solution of compound II.
[0080] The salt solution of Compound II is light yellow.
[0081] The specific content of the step 3 reaction is:
[0082] The reaction temperature is 20-30°C, and a 500mL three-necked flask is used as a reactor; 0.1mol / L potassium sulfate is added dropwise to the salt solution of the intermediate compound II, and the supernatant is taken to detect the reaction progress. The reaction is completed when no precipitation is produced by adding 0.1mol / L potassium sulfate solution to the supernatant; stirring, standing, and filtering to remove insoluble matter, and taking the filtrate to obtain a solution of compound I.
[0083] In step 3, the barium ion content in the solution can be determined based on the 0.1 mol / L potassium sulfate solution added dropwise.
[0084] The supernatant of the reaction in step 3 is taken to track the reaction endpoint, and the reaction endpoint is determined if no precipitation is generated by adding 0.1 mol / L potassium sulfate solution.
[0085] In the step 2, the reaction solution is allowed to stand for 2 hours and then filtered to remove insoluble matter.
[0086] The filtrate in step 2 is taken to obtain a solution of compound I.
[0087] The Compound I solution was colorless.
[0088] The specific content of the step 4 reaction is:
[0089] The compound I solution is concentrated and dried, and the solvent is removed to obtain a crystalline product, which is then removed and ground into powder to obtain compound I.
[0090] The crystalline product is a white powder, namely compound I.
[0091] Another object of the present invention is to provide a novel potassium sulfonate flame retardant for polycarbonate (PC).
[0092] Compound I and polycarbonate (PC) masterbatch were placed in a drum drying oven at 100° C. and dried for 10 h.
[0093] Compound I and polycarbonate (PC) were granulated in different ratios and injection molded to obtain test specimens.
[0094] The flame retardant is tested in a limiting oxygen index test and a vertical combustion test when the flame retardant is in a ratio of 0.00wt% to 0.50wt% of the composite material.
[0095] The flame retardant is added at a ratio of 0.00 wt% in the composite material, and after granulation and injection molding of the specimen, the limiting oxygen index obtained is 26.8%, passing the vertical combustion test UL-94V-2 level.
[0096] The flame retardant is added at a ratio of 0.02 wt % in the composite material, and after granulation and injection molding of the specimen, the limiting oxygen index obtained is 33.0%, and the vertical combustion test UL-94V-2 level is passed.
[0097] The flame retardant is added to the composite material at a ratio of 0.05 wt %, and after granulation and injection molding, the limiting oxygen index obtained is 34.5%, passing the vertical combustion test UL-94V-2 level.
[0098] The flame retardant is added to the composite material at a ratio of 0.10 wt %, and after granulation and injection molding, the limiting oxygen index obtained is 35.5%, passing the vertical combustion test UL-94V-0 level.
[0099] The flame retardant is added to the composite material at a ratio of 0.25 wt %, and after granulation and injection molding, the limiting oxygen index obtained is 37.0%, passing the vertical combustion test UL-94V-0 level.
[0100] The flame retardant is added at a ratio of 0.50 wt% in the composite material, and after granulation and injection molding of the specimen, the limiting oxygen index obtained is 34.5%, passing the vertical combustion test UL-94V-0 level.
[0101] Example 1
[0102] The specific step 1 of this experiment is as follows: at 35-40° C., in a three-necked flask, 50% fuming sulfuric acid is slowly added dropwise to a solution of hexaphenoxy cyclotriphosphazene dissolved in dichloromethane while stirring, wherein the solid-liquid ratio of hexaphenoxy cyclotriphosphazene (g): dichloromethane (mL) is 1:12-17, and the optimal solid-liquid ratio is 1:15; the reaction end point is monitored by thin layer chromatography, and the reaction is terminated when there is no color development of hexaphenoxy cyclotriphosphazene. After standing to room temperature, distilled water is added for liquid separation, dichloromethane is removed, and the upper liquid is taken to obtain an acid solution of the intermediate compound II.
[0103] When selecting the solvent for hexaphenoxycyclotriphosphazene in experimental step 1, dichloromethane is selected because experiments have shown that dichloromethane will not be sulfonated. Therefore, using dichloromethane as a solvent avoids the problem of non-uniform products caused by excessive by-products.
[0104] Example 2
[0105] The specific step 2 described in this experiment is as follows: the reaction temperature is 20-30°C, and a 500mL three-necked flask is used as a reactor; barium carbonate powder is added to the acid solution of compound II, and the supernatant is taken to observe the pH monitoring end point. If pH = 7.0, the reaction is completed, and the reaction is allowed to stand and filtered to remove insoluble matter, and the filtrate is taken to obtain a salt solution of compound II.
[0106] The original idea of treating byproducts in this experiment was to use calcium oxide and barium chloride as raw materials to remove the byproduct sulfuric acid. However, the experimental process was too complicated and would result in some loss of product. Therefore, the idea was readjusted to add barium carbonate to remove the waste acid and introduce barium ions to replace the hydrogen ions in the sulfonic acid.
[0107] Example 3
[0108] The specific step 3 described in this experiment is as follows: the reaction temperature is 20-30°C, and a 500mL three-necked flask is used as a reactor; potassium sulfate is added to the salt solution of the intermediate compound II, and the supernatant is taken to observe whether there is precipitation to monitor the end point. If no precipitation is generated, the reaction is completed; let it stand, filter and remove insoluble matter, take the filtrate, and obtain a solution of compound I.
[0109] In the process of selecting the replacement reagent, potassium hydroxide was initially selected. However, no obvious phenomenon was observed during the actual reaction monitoring process, and it was difficult to observe the progress of the reaction. Excessive addition could easily lead to impure products. Potassium sulfate was finally selected. During the reaction, potassium sulfate reacted with barium ions to form a precipitate. The supernatant was taken, potassium sulfate was added to observe whether there was a precipitate, and the reaction progress could be monitored. If no precipitate was formed, the reaction was over.
[0110] Example 4
[0111] The specific step 4 described in this experiment is as follows: the compound I solution is concentrated and dried, and the solvent is removed to obtain a crystalline product, which is then removed and ground into powder to obtain compound I.
[0112] The experiment was carried out according to the steps described and compound I was successfully obtained for subsequent experiments.
[0113] Example 5
[0114] In this experiment, a flame retardant was prepared according to the preparation method of the present invention and then melt-blended with polycarbonate (PC) to test its flame retardant properties. The specific reaction process is as follows:
[0115] The flame retardant HPCTP-SK and polycarbonate (PC) masterbatch prepared in the experiment were placed in a drum drying oven at 100°C and dried for 10 hours. The flame retardant HPCTP-SK and polycarbonate (PC) were granulated in different proportions and injection molded to obtain test specimens for subsequent testing.
[0116] The structural characterization data of HPCTP-SK are as follows, and the specific spectrum is shown in the attached figure of the specification.
[0117] Figure 1 The infrared spectrum of the novel potassium sulfonate flame retardant HPCTP-SK of the present invention is shown in FIG. Figure 1 Available: 1595, 1494 and 1446cm -1 It is the absorption peak of the skeleton deformation vibration of the benzene ring unique to HPCTP, 1183cm -1 It is the stretching vibration absorption peak of P=N of cyclotriphosphazene, 1007cm -1 It is the characteristic absorption peak of POC; 675cm -1 The absorption peaks of the benzene ring are monosubstituted; 1128 and 1037 cm-1 It is the characteristic absorption peak of O=S=O, 838cm -1 It is the stretching vibration absorption peak of SO.
[0118] Flame retardant performance research:
[0119] The present invention directly compounds HPCTP-SK with PC without adding any other additives, thereby testing the flame retardant properties of the flame retardant. The specific operation is as follows:
[0120] (1) PC masterbatch was placed in a drum drying oven at 100°C and dried for 10 hours. Then HPCTP-SK was pre-mixed in different proportions and then extruded, cooled and granulated using a twin-screw extruder at a screw speed of 100 r / min. The amount of HPCTP-SK added is shown in Table 1; Table 2 shows the temperature of each temperature section set for the twin-screw extruder.
[0121] Table 1 Addition amount of HPCTP-SK in PC
[0122]
[0123] Table 2 Temperature of each temperature section of twin screw extruder
[0124]
[0125] (2) The pellets were placed in a drum drying oven at 100°C and dried for 10 hours. According to GB / T 25156-2010, the experimental standard specimens were made using an injection molding machine. The LOI values of the test specimens were obtained using the ISO4589-1996 standard test, and the specimen specifications were 120mm×10mm×4mm. The vertical combustion test was measured using the UL-94 standard, and the specimen specifications were 120mm×13mm×3.2mm. Injection molding pressure: 50MPa for the first and second stages, respectively. The temperature stages of the injection molding machine are listed in Table 3.
[0126] Table 3 Temperature of each temperature range of injection molding machine
[0127]
[0128] The test results are shown in Table 4:
[0129] Table 4 Flame retardant test results of PC / HPCTP-SK system with different addition ratios
[0130]
[0131] Figure 2This is a limiting oxygen index curve at different addition amounts of the flame retardant HPCTP-SK in the embodiment of the present invention. Through the limiting oxygen index and vertical combustion tests, it is concluded that the LOI value of pure PC is 26.8%, and the UL-94 vertical combustion grade is UL-94V-2. As the amount of HPCTP-SK added increases, the LOI value of the composite material gradually increases. When 0.02wt.% HPCTP-SK is added, the LOI value of the composite material is 33.0%. When the addition amount is 0.1wt.%, the LOI value reaches 35.5% and passes the UL-94V-0 level. This shows that HPCTP-SK can well improve the LOI value of the composite material and show a good flame retardant effect.
[0132] Thermal performance study:
[0133] Figure 3 TGA and corresponding DTG curves of flame retardant HPCTP-SK measured under nitrogen atmosphere at a heating rate of 20℃ / min.
[0134] Table 5 gives the main thermal degradation parameters. Definition: T onset T is the temperature at which the material loses 5% of its weight during thermal decomposition. max It is the temperature corresponding to the maximum thermal weight loss of the material.
[0135] Table 5 Thermal degradation parameters of HPCTP-SK in nitrogen atmosphere
[0136]
[0137] Depend on Figure 3 Some of the data obtained are listed in Table 5. As shown in Table 5, the T onset The temperature of the flame retardant is 429.7℃, which proves that the flame retardant has good thermal stability. The processing temperature range of PC is 240-270℃. HPCTP-SK powder begins to decompose after 400℃, so it will not be thermally decomposed during PC processing and can meet the processing conditions of PC. As the temperature continues to rise, at 700℃, the residual carbon content in a nitrogen atmosphere is 63.04%, which shows that this flame retardant has a good carbonization ability, thus achieving a good flame retardant effect.
[0138] Table 6 Thermal degradation performance parameters and carbon residue rate of PC and PC / HPCTP-SK systems under nitrogen
[0139]
[0140] Figure 4Table 6 shows the thermal stability data of PC and PC / HPCTP-SK system in nitrogen atmosphere at a heating rate of 20°C / min. Compared with PC, the T onset The temperature of PC increased by 3.4℃, which may be due to the effect of the high thermal stability of the hexaphenoxy cyclotriphosphazene group in the flame retardant molecule, which improved the overall stability of the PC substrate. max The T of PC / 0.1wt% HPCTP-SK is 520.6℃. max The temperature was reduced to 498.7℃, and the addition of HPCTP-SK brought forward the peak of PC decomposition rate. At 700℃, the final carbon residue rate of PC was 19.58%. After the addition of HPCTP-SK, the final carbon residue rate was 21.52% when the addition amount was 0.1wt.%, which was mainly related to the sulfonate group in HPCTP-SK. The increase in carbon residue rate may be due to the fact that the sulfonate group promotes the isomerization and rearrangement of PC at high temperature, and promotes the formation of intermediate coke at lower temperature, thereby increasing the carbon residue.
[0141] In summary, HPCTP-SK flame retardant plays an effective flame retardant role and improves the flame retardant properties of the substrate, causing PC to decompose and rearrange in advance, and undergo a cross-linking reaction, increasing the stability and density of the carbon layer, and playing a role in isolating oxygen. The flame retardant has a novel structure, is non-toxic, and is heat-insulating and oxygen-insulating, and has the following advantages: 1. It has little effect on the mechanical properties of PC. When the product of the present invention is added at 0.1wt%, the LOI value of PC reaches 35.5%, and passes the UL-94V-0 grade (while when the commercial HPCTP is added at 0.1wt%, the LOI value only reaches 30.5%, and only passes the UL-94V-2 grade); 2. It has little effect on the transparency of the material.
[0142] The beneficial effects of the present invention are as follows: the flame retardant is non-toxic, has good flame retardant effect, can achieve high flame retardant effect at a low addition amount, and has a simple synthesis process, is easy to operate, and is suitable for popularization and application.
[0143] Although specific embodiments of the present invention have been given herein, those skilled in the art should understand that the embodiments herein may be modified without departing from the spirit of the present invention. The above embodiments are merely exemplary and should not be used as a limitation on the scope of the present invention.
Claims
1. A novel potassium sulfonate-type flame retardant, which is a flame retardant for polycarbonate; characterized in that: The flame retardant is compound I; The chemical structural formula of the compound I is as follows:
2. A method for preparing the novel potassium sulfonate flame retardant according to claim 1, characterized in that: The preparation method comprises the following steps: firstly, using hexaphenoxy cyclotriphosphazene and 50% fuming sulfuric acid as raw materials to realize one-step sulfonation; secondly, using barium carbonate as an acid scavenger to remove waste acid and combine barium ions with sulfonic acid groups; finally, using potassium sulfate as a substitution agent to replace barium ions to obtain the compound I.
3. The preparation method according to claim 2, characterized in that: The preparation method specifically comprises the following steps: Step 1: sulfonating hexaphenoxy cyclotriphosphazene with 50% fuming sulfuric acid as a sulfonating agent to obtain an acid solution of an intermediate compound II, wherein the acid solution of the intermediate compound II is a benzenesulfonic acid oxycyclotriphosphazene solution; Step 2: using barium carbonate as an acid removal agent to remove the byproduct sulfuric acid in the sulfuric acid solution of the intermediate compound II in step 1, and simultaneously replacing the hydrogen ions in the hexabenzenesulfonyloxycyclotriphosphazene solution to obtain a salt solution of the intermediate compound II, wherein the hydrochloric acid solution of the intermediate compound II is a salt solution of benzenesulfonyloxycyclotriphosphazene; Step 3: using 0.1 mol / L potassium sulfate as a substitution reagent to replace the barium ions in the salt solution of the intermediate compound II in step 2 to obtain a solution of compound I, wherein the solution of compound I is a potassium phenoxycyclotriphosphazene sulfonate solution; Step 4: Concentrate and dry, and dry the potassium hexaphenoxycyclotriphosphazene sulfonate solution in step 3 to obtain the compound I, which is potassium hexaphenoxycyclotriphosphazene sulfonate HPCTP-SK.
4. The preparation method according to claim 3, characterized in that: In the step 1, the solid-to-liquid ratio of hexaphenoxy cyclotriphosphazene to 50% fuming sulfuric acid is 1:0.2-1.
2.
5. The preparation method according to claim 3, characterized in that: The specific content of the reaction in step 1 is: slowly adding 50% fuming sulfuric acid to a dichloromethane solution of hexaphenoxy cyclotriphosphazene while stirring at 35-40° C., wherein the solid-liquid ratio of hexaphenoxy cyclotriphosphazene (g): dichloromethane (ml) is 1:12-17; monitoring the end point of the reaction by thin layer chromatography, the reaction is terminated when no color is shown on hexaphenoxy cyclotriphosphazene, and the reaction is allowed to stand to room temperature, and then distilled water is added for separation, and the upper layer is taken to obtain an acid solution of the intermediate compound II.
6. The preparation method according to claim 3, characterized in that: In the step 2, the ratio of the amount of compound II to the amount of barium carbonate powder is 1:5.0-7.
0.
7. The preparation method according to claim 3, characterized in that: The specific content of the step 2 reaction is: The reaction temperature is 20-30°C, and a 500mL three-necked flask is used as a reactor; barium carbonate powder is added to the acid solution of compound II, and the pH value of the solution is measured. If the pH is neutral, the reaction is completed, and the solution is allowed to stand and filtered to remove insoluble matter; the filtrate is taken to obtain a salt solution of compound II.
8. The preparation method according to claim 3, characterized in that: In step 3, the ratio of compound II to potassium sulfate is 1:15-17. The specific content of the reaction in step 3 is: The reaction temperature is 20-30°C, and a 500mL three-necked flask is used as a reactor; 0.1mol / L potassium sulfate is added dropwise to the salt solution of the intermediate compound II, and the supernatant is taken to detect the reaction progress. The reaction is completed when no precipitation is produced by adding 0.1mol / L potassium sulfate solution to the supernatant; stirring, standing, and filtering to remove insoluble matter, and taking the filtrate to obtain a solution of compound I.
9. The preparation method according to claim 3, characterized in that: The specific content of the step 4 reaction is: The compound I solution is concentrated and dried to remove the solvent to obtain a crystalline product, which is then removed and ground into powder to obtain compound I.
10. Application of a novel potassium sulfonate-type flame retardant, characterized in that: The novel potassium sulfonate-type flame retardant as claimed in claim 1 is used to provide flame retardancy in polycarbonate.
Citation Information
Patent Citations
Novel N-P-S expansion type phosphorus flame retardant and preparation method thereof
CN109796629A
Water-soluble sulfonate aryl bis-triazine pyridine derivative and preparation method thereof
CN115215836A
Phase transfer PPS fiber catalyst, preparation method and application of phase transfer PPS fiber catalyst in catalytic synthesis of triphosphazene sulfonate flame retardant