ABS sulfonate flame retardant as well as preparation method and application thereof

By combining sulfonate with ABS structure, ABS sulfonate flame retardant is designed, which solves the loss problem of flame retardant on the mechanical properties of polycarbonate in the prior art, and achieves a significant improvement in flame retardant performance under low addition amount and impact strength effect, meet the application needs of high performance and high flame retardant requirements.

CN118978643APending Publication Date: 2024-11-19ZHONGBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049321.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

While improving the flame retardant effect of polycarbonate, existing small molecule sulfonate flame retardant may have a negative impact on its mechanical properties, especially the notch impact strength, and it is difficult to meet the industry standards of high performance and high flame retardant requirements.

Method used

Develop an ABS sulfonate flame retardant to design and synthesize ABS sulfonate flame retardant with unique properties by combining sulfonate with ABS structure, using specific preparation methods including sulfonation reaction and neutralization The process is used to form a flame retardant with excellent compatibility, which is used to improve the flame retardant and mechanical properties of polycarbonate.

Benefits of technology

The ultimate oxygen index and UL-94 test level of polycarbonate are significantly improved under low addition amount, with an impact strength of 60.98kJ/m2, while maintaining good mechanical properties, achieving high-efficiency flame retardant effect and low toxicity, suitable for promotion and application .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978643A_ABST
    Figure CN118978643A_ABST
Patent Text Reader

Abstract

The invention discloses an ABS sulfonate flame retardant as well as a preparation method and application thereof, and belongs to the technical field of flame retardants. Sulfur trioxide is extracted through fuming sulfuric acid with the mass fraction of 50%, the sulfur trioxide and 1, 4-dioxane are complexed to generate a sulfur trioxide-dioxane complex which is used as a sulfonating agent for sulfonating ABS, and the sulfonating product is neutralized through potassium hydroxide to obtain the ABS sulfonate flame retardant. When the addition amount of the product in polycarbonate is 0.5 wt%, the LOI of the composite material is improved from 24.7% of PC to 40.5%, the UL-94 test is improved from V-2 level to V-0 level, and the impact strength reaches 60.98 kJ / m < 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardants, and in particular relates to an ABS sulfonate flame retardant and a preparation method and application thereof. Background Art

[0002] Polycarbonate (PC), as a high-performance thermoplastic engineering plastic, has been widely used in many fields including building materials, automotive parts manufacturing, and electronic and electrical components. Pure PC material has shown certain flame retardant properties, with a limiting oxygen index (LOI) of 24-26%, and a V-2 rating in the UL-94 vertical burning test. However, in industries such as construction and electronic components, where the risk of fire is high and the potential losses are huge, more stringent standards are imposed on the flame retardant properties of materials.

[0003] Sulfonate flame retardants have certain advantages in flame retardant modification of polycarbonate due to their small addition amount and excellent self-extinguishing property. However, while some small molecule sulfonate flame retardants improve the flame retardant effect, they may have a significant negative impact on the mechanical properties of polycarbonate, especially the notched impact strength. Therefore, it is necessary to develop an innovative flame retardant that has low addition amount, high flame retardant performance, and minimizes the loss of mechanical properties of the substrate, especially the adverse effect on notched impact strength. Summary of the invention

[0004] In view of the above technical problems, the present invention proposes an ABS (acrylonitrile-butadiene-styrene copolymer) sulfonate flame retardant and a preparation method thereof. The present invention combines sulfonate with ABS structure to design and synthesize a series of ABS sulfonate flame retardants with unique properties, aiming to improve the flame retardant properties of PC while maintaining and optimizing its mechanical properties to the maximum extent, providing a feasible solution for the development of high-performance and high flame retardant PC composite materials.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical purposes: an ABS sulfonate flame retardant, which is a compound obtained by ion exchange of sulfonated acrylonitrile (A)-butadiene (B)-styrene (S) copolymer, and the chemical structure of the compound is shown in Formula I:

[0007]

[0008] The values ​​of a, b, and c are related to the model of ABS and are not fixed. The ABS used in the present invention comes from Ningbo LG Yongxing Chemical Co., Ltd.

[0009] Technical purpose 2: A method for preparing the ABS sulfonate flame retardant, comprising the following steps:

[0010] Using fuming sulfuric acid as a raw material, distilling sulfur trioxide and collecting it in a dichloroethane solution to obtain a dichloroethane solution containing sulfur trioxide;

[0011] The dichloroethane solution containing sulfur trioxide is mixed with 1,4-dioxane to carry out complex reaction, and filtered to obtain sulfur trioxide·dioxane complex powder;

[0012] The sulfur trioxide·dioxane complex powder is added to a dichloromethane solution of acrylonitrile-butadiene-styrene copolymer for sulfonation, distilled (to remove the remaining sulfur trioxide and dioxane), and filtered to obtain an intermediate compound;

[0013] The intermediate compound is added to a dichloromethane solution, and a potassium hydroxide solution is added dropwise for neutralization. The organic phase is separated, washed with water, distilled, and filtered. The obtained sample is further added to dichloromethane for distillation to obtain an ABS sulfonate flame retardant.

[0014] Furthermore, the mass-to-liquid ratio of the sulfur trioxide solution to the ethylene dichloride solution is 1 g:4.8 mL.

[0015] Furthermore, the complexation reaction is carried out by dropping the 1,4-dioxane into the dichloroethane solution containing sulfur trioxide at a temperature below -10°C and under stirring, and the dropping speed is controlled at 5-10s / drop.

[0016] Furthermore, the sulfonation treatment is carried out at room temperature with stirring for 4 hours;

[0017] The mass-to-liquid ratio of the acrylonitrile-butadiene-styrene copolymer to the dichloromethane solution is 1 g: 10 mL;

[0018] The mass ratio of the acrylonitrile-butadiene-styrene copolymer to the sulfur trioxide-dioxane complex powder is 1:0.32.

[0019] Furthermore, the neutralization treatment is carried out at room temperature with stirring for 12 hours until the pH value of the solution reaches 8;

[0020] The mass-to-liquid ratio of the intermediate compound to the dichloromethane solution is 1 g:10 mL.

[0021] Technical purpose three: A polycarbonate flame retardant, using the ABS sulfonate flame retardant and polycarbonate as raw materials, wherein the mass ratio of the polycarbonate to the ABS sulfonate flame retardant is 0.5:99.5.

[0022] Technical purpose four: A method for preparing the polycarbonate flame retardant, comprising the following steps: mixing the polycarbonate and ABS sulfonate flame retardant and adding them to a twin-screw extruder for melt mixing and extrusion, and then molding by an injection molding machine to obtain a polycarbonate material containing the sulfonate flame retardant.

[0023] Compared with the prior art, the present invention has the following advantages and technical effects:

[0024] (1) The butadiene rubber phase in the ABS polymer provides excellent stress dispersion and absorption capabilities. Especially under low temperature conditions, this rubber phase can effectively alleviate the problem of reduced impact strength of polycarbonate materials caused by low-temperature embrittlement. The styrene-acrylonitrile copolymer has good compatibility with polycarbonate and can form a microstructure with multiple phases coexisting with polycarbonate. Therefore, the addition of ABS sulfonate flame retardant to polycarbonate in the present invention can significantly enhance the impact resistance and toughness of polycarbonate, thereby obtaining a polycarbonate flame retardant having the advantages of both sulfonate and ABS.

[0025] (2) When the ABS sulfonate flame retardant prepared by the present invention is added in an amount of 0.5 wt / %, the LOI of the polycarbonate material is increased from 24.7% of PC to 40.5%, and the UL-94 test is increased from V-2 to V-0.

[0026] (3) It has little effect on the mechanical properties of polycarbonate materials, and the impact strength reaches 60.98 kJ / m 2 .

[0027] (4) The prepared ABS sulfonate flame retardant has a novel structure, is non-toxic, heat-insulating and oxygen-insulating, and achieves a high flame retardant effect at a low addition amount while maintaining good mechanical properties. The synthesis process is simple and easy to operate, making it suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0029] Figure 1 is a Fourier transform infrared spectrum of the yellow-white solid compound in Example 1 of the present invention;

[0030] Figure 2 The TGA graphs of the ABS sulfonate flame retardant and ABS in Example 1 of the present invention under a nitrogen atmosphere;

[0031] Figure 3 This is the DTG diagram of the ABS sulfonate flame retardant and ABS in nitrogen atmosphere in Example 1 of the present invention;

[0032] Figure 4 The TGA graphs of PC and PC / ABS sulfonate in Application Example 1 of the present invention under nitrogen atmosphere;

[0033] Figure 5 This is the DTG diagram of PC and PC / ABS sulfonate in Application Example 1 of the present invention under nitrogen atmosphere. DETAILED DESCRIPTION

[0034] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0035] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0036] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0037] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0038] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0039] The "room temperature" in the present invention refers to 20-25°C unless otherwise specified.

[0040] The raw materials used in the present invention are all purchased from the market.

[0041] The present invention extracts sulfur trioxide with a mass fraction of 50% fuming sulfuric acid, and uses the sulfur trioxide·dioxane complex generated by complexation with 1,4-dioxane as a sulfonating agent to sulfonate ABS, and neutralizes the sulfonated product with potassium hydroxide to obtain an ABS sulfonate flame retardant. The sulfonate structure can catalyze the isomerization and cross-linking of polycarbonate to form carbon, has a good flame retardant effect, and improves the limiting oxygen index of polycarbonate; ABS and polycarbonate have good compatibility, wherein PB (polybutadiene graft) can effectively absorb and disperse energy when impacted by external forces, and can improve the impact strength and other properties of polycarbonate. When the flame retardant of the present invention is added in an amount of 0.5wt / %, the LOI of the composite material is increased from 24.7% of PC to 40.5%, the UL-94 test is increased from V-2 level to V-0 level, and the impact strength reaches 60.98kJ / m 2 .

[0042] A method for preparing an ABS sulfonate flame retardant comprises the following steps:

[0043] 1) distilling 50% oleum as a raw material to obtain sulfur trioxide and collecting the sulfur trioxide in a dichloroethane solution to obtain a dichloroethane solution containing sulfur trioxide;

[0044] 2) mixing the dichloroethane solution containing sulfur trioxide with 1,4-dioxane for complex reaction, filtering, and obtaining sulfur trioxide·dioxane complex powder (sulfonating agent);

[0045] 3) adding the sulfur trioxide·dioxane complex powder and acrylonitrile-butadiene-styrene copolymer to the dichloromethane solution for sulfonation, distillation, and filtration to obtain an intermediate compound;

[0046] The reaction of this step is shown in the following formula (1):

[0047]

[0048] 4) adding the intermediate compound to a dichloromethane solution, dropping a 1 mol / L potassium hydroxide solution for neutralization, separating the organic phase, washing with water, distilling, filtering, and further adding the obtained sample to distillation to obtain an ABS sulfonate flame retardant;

[0049] The reaction of this step is shown in the following formula (2):

[0050]

[0051] In some preferred embodiments of the present invention, in step 1), the mass-to-liquid ratio of the sulfur trioxide to the dichloroethane solution is 1g:4.8mL. The distillation temperature is 80-85°C, oleum stops releasing visible bubbles, the distillation ends, and the heating is stopped. The specific steps are: distilling oleum with a mass fraction of 50% at 80-85°C, using a condenser to condense the distilled sulfur trioxide gas into liquid, dripping the liquid into a conical flask filled with dichloroethane through a receiving tube, oleum stops releasing visible bubbles, the distillation ends, and the heating is stopped to obtain a dichloroethane solution of sulfur trioxide. By weighing the mass of the conical flask before and after the collection, the mass difference is obtained, and finally the mass of the collected sulfur trioxide is obtained, and a sulfur trioxide dichloroethane solution of a certain concentration is prepared.

[0052] In some preferred embodiments of the present invention, step 2) the complex reaction refers to: under the condition of -15 to -8°C (if the temperature rises, the drop rate of sulfur trioxide dichloroethane solution will be reduced), using a 500mL three-necked flask as a reaction container, adding dichloroethane solution containing sulfur trioxide to 1,4-dioxane while stirring, the drop rate is controlled at 5-10s / drop, the reaction is terminated when no sulfur trioxide smoke is generated in the system, the solution is filtered to remove the sulfur trioxide·dioxane complex white powder, and the powder is stored in the dark at -15 to -8°C. The molar ratio of sulfur trioxide to 1,4-dioxane is 1:(1-1.2), preferably 1:1.2.

[0053] In step 3) of some preferred embodiments of the present invention, the sulfonation treatment refers to: at room temperature, using a 500mL three-necked flask as a reaction container, adding sulfur trioxide·dioxane complex powder to the dichloromethane solution of acrylonitrile-butadiene-styrene copolymer while stirring, the reaction time is 4 hours, and a dichloromethane solution containing the sample is obtained; the solution is dripped into boiling distilled water to remove the solvent and impurities, and filtered to obtain an intermediate compound (yellow-white solid). The sulfur trioxide·dioxane complex is added in small amounts and multiple times, and the complex is divided into several equal parts and added in batches. The mass-to-liquid ratio of the acrylonitrile-butadiene-styrene copolymer and the dichloromethane solution is 1g:10mL; the mass ratio of the acrylonitrile-butadiene-styrene copolymer to the sulfur trioxide·dioxane complex powder is 1:0.32.

[0054] The sulfonation degree of the intermediate compound is determined by acid-base titration. The specific method is as follows: 0.2 g of the intermediate compound is dissolved in 10 mL of dichloromethane solvent, and after the solid is completely dissolved, a phenolphthalein indicator is added, and 3 mL of 0.1 mol / L NaOH ethanol aqueous solution is added dropwise to change the solution from colorless to pink, and 0.1 mol / L HCl aqueous solution is added dropwise until the pink color fades and the titration end point is reached, and the amount of HCl used is recorded. The average value is taken after the result is calculated. The sulfonation degree calculation formula is shown in the following formula (I):

[0055]

[0056] Wherein: S% is the sulfonation degree of ABS, (%); c1 is the concentration of sodium hydroxide (NaOH) solution, (mol / L); v1 is the consumption of sodium hydroxide (NaOH), (mL); c2 is the concentration of hydrochloric acid (HCl) solution, (mol / L); v2 is the consumption of hydrochloric acid (HCl) solution, (mL); m is the mass of the substance to be tested, (g).

[0057] In step 4) of some preferred embodiments of the present invention, the neutralization treatment refers to: under room temperature conditions, dripping 1 mol / L potassium hydroxide solution into the dichloromethane solution of the intermediate compound while stirring, pH detection of the dripping end point, ending at pH of about 8.0, and continuing to stir the reaction for 12 hours to obtain a mixed solution containing the compound; adding the mixed solution containing the compound to a 500 mL constant pressure separatory funnel, taking the lower organic phase solution, washing with water to neutrality to obtain a dichloromethane solution of the compound again; dripping it into boiling distilled water to remove the solvent and impurities, filtering to obtain the compound; dissolving the compound again with dichloromethane, dripping it into boiling distilled water to remove the solvent and impurities, and obtaining a pure compound.

[0058] The change of butadiene content in the compound is determined by back titration, and the reaction formula is shown in the following formula (II):

[0059] KBrO3+5KBr+6H + →3Br2+3H2O+6K +

[0060] Br2+C=C→BrC-CBr

[0061] Br2+2KI→2KBr+I2

[0062] 2Na2S2O3+2I2→Na2S4O6+4NaI Formula (II)

[0063] The specific steps are:

[0064] A. Take 0.2g of ABS and 0.2g of compound and dissolve them in 10mL of dichloromethane respectively in an iodine volumetric flask. At the same time, take 10mL of dichloromethane and place it in an iodine volumetric flask as a blank group. Prepare a 0.02mol / L KBrO3-KBr solution with deionized water and ethanol solution, take 25mL and add it to the iodine volumetric flask, then add 2mL of concentrated HCl, cover the flask, shake well, and place it away from light for 2h.

[0065] B. Add 1.5g of potassium iodide solid to the iodine volume bottle and place the bottle in a dark place for 5 minutes. Titrate with 0.1mol / L sodium thiosulfate standard solution. When the titration is close to the end point, the solution is light yellow. Add 1mL of 1% starch solution and continue to titrate until the blue color disappears and the titration end point is reached. Record the volume of sodium thiosulfate standard solution consumed in each titration, calculate the result and take the average value. The calculation formula of butadiene content is shown in the following formula (III):

[0066]

[0067] Wherein: C1 is the concentration of potassium bromate (KBrO3) solution, (mol / L); v1 is the consumption of potassium bromate (KBrO3), (mL); C2 is the concentration of potassium bromate (Na2S2O3) solution, (mol / L); v2 is the consumption of potassium bromate (Na2S2O3) solution, (mL); m is the mass of the analyte, (g); b is the blank group error, (mol).

[0068] The compound (yellow-white solid) prepared by the above preparation method is the ABS sulfonate flame retardant.

[0069] The ABS sulfonate flame retardant can be used in polycarbonate to prepare a polycarbonate flame retardant, and the mass ratio of polycarbonate to ABS sulfonate flame retardant is 0.5:99.5.

[0070] The preparation method of the polycarbonate flame retardant comprises the following steps: mixing the polycarbonate and ABS sulfonate flame retardant, adding the mixture into a twin-screw extruder for melt mixing and extrusion, and then molding the mixture through an injection molding machine to obtain a polycarbonate material containing the sulfonate flame retardant, namely the polycarbonate flame retardant.

[0071] The technical solution of the present invention is further illustrated by the following embodiments.

[0072] Example 1

[0073] A method for preparing an ABS sulfonate flame retardant comprises the following steps:

[0074] 1) Add 50 g of 50% oleum to a 500 mL round-bottom single-mouth distillation flask, maintain the temperature above 80° C. for distillation, condense the evaporated gas through a condensation system, and guide it into a weighed conical flask containing 100 mL of dichloroethane solution to collect the colorless liquid sulfur trioxide produced by distillation; stop heating when the oleum stops releasing visible bubbles, indicating the end of the distillation stage;

[0075] The receiving bottle loaded with the sulfur trioxide / dichloroethane solution was weighed again. By calculating the difference in mass between the receiving bottle before and after distillation, the mass of sulfur trioxide dissolved in dichloroethane was obtained. The exact concentration of the solution was further calculated to obtain a sulfur trioxide / dichloroethane solution with a concentration of 20.99 g / 100 mL.

[0076] 2) Add 100 mL of 25.4 g / 100 mL 1,4-dioxane / dichloroethane solution to a 500 mL three-necked flask, place the three-necked flask in a low-temperature bath for reaction at -8°C; slowly drip 100 mL of 20.99 g / 100 mL sulfur trioxide / dichloroethane solution into the three-necked flask (the dripping speed is controlled at 5 s / drop). During the titration process, the titration rate must be closely monitored and appropriately controlled, and the mixed solution is continuously stirred; the reaction is terminated when no sulfur trioxide smoke is generated in the system, and the solution is filtered to obtain a sulfur trioxide·dioxane complex white powder, which is stored below -8°C and protected from light;

[0077] 3) Dissolve 30 g of ABS in 300 mL of dichloromethane solution, use a 500 mL three-necked flask as a reaction container, keep stirring, weigh 9.5 g of sulfur trioxide·dioxane complex and divide it into 10 portions at room temperature, add them to the three-necked flask in batches to react until the sulfonating agent (sulfur trioxide·dioxane complex) is completely dissolved, at which time the solution appears dark blue, and the reaction is continued for 4 h until the system temperature is consistent with room temperature, indicating that the reaction is completed, and a dichloromethane solution containing the intermediate compound is obtained;

[0078] Dropping the dichloromethane solution containing the intermediate compound into boiling distilled water to remove the solvent and impurities, filtering to obtain a yellow-white solid intermediate compound;

[0079] 4) Weigh 15g of the intermediate compound and dissolve it in 150mL of dichloromethane, then transfer the solution to a 500mL beaker, and adjust the pH of the system to 8 by dropping 1mol / L potassium hydroxide aqueous solution at room temperature. Perform ion exchange reaction for 12h under stirring, and monitor the reaction progress by acid-base test. When the pH of the organic phase shows neutrality, the reaction is completed, and a mixed solution containing the compound is obtained;

[0080] Add the mixed solution containing the compound into a 500mL constant pressure separatory funnel, take the lower organic phase solution, wash with water until neutral to obtain a dichloromethane solution containing the compound; drip it into boiling distilled water to remove the solvent and impurities, and filter to obtain the compound; dissolve the compound again with dichloromethane, drip it into boiling distilled water to remove the solvent and impurities, and obtain a pure yellow-white solid compound, namely ABS sulfonate flame retardant. The structural formula is

[0081] Figure 1 This is the infrared spectrum of the ABS sulfonate flame retardant prepared in Example 1. Figure 1 Available, located at 3080cm -1 、3059cm -1 and 3025cm -1 A series of absorption peaks at 2922cm are the out-of-plane distortion vibrations of the benzene ring -CH in the styrene structural unit. -1 and 2849cm -1 The peak at 1600 cm corresponds to the asymmetric and symmetric stretching vibrations of the methylene group (-CH2-), while the peak at 1600 cm -1 、1492cm -1 and 1453cm -1 The absorption peak of 2237cm -1 The absorption peak at 966cm is the stretching vibration of the nitrile group (-C≡N) unique to acrylonitrile, while the absorption peak at 966cm -1 、846cm -1 and 912cm -1 The peaks at 1180cm correspond to the 1,4-trans and cis-CH=CH-out-of-plane twisting vibrations and 1,2-trans-CH=CH-out-of-plane twisting vibrations, respectively. These characteristic peaks confirm that the sample contains acrylonitrile-butadiene structural elements. -1 Nearby is the peak of the asymmetric stretching vibration of sulfonate S=O, 1040cm -1 The peak at is the symmetric stretching vibration of the sulfonate group S=O, indicating that the compound prepared by the method of Example 1 contains sulfonate groups, indicating that ABS is successfully sulfonated.

[0082] The sulfonation degree of the yellow-white solid compound was determined by acid-base titration. The calculation results are shown in Table 1 below.

[0083] Table 1 Compound sulfonation degree test results

[0084]

[0085] According to Table 1, the degree of sulfonation of the compound prepared in Example 1 is 8.70%;

[0086] The changes in the butadiene content in the blank control group, ABS and the yellow-white solid compound (ABS sulfonate flame retardant) were determined by back titration. The calculation results are shown in Tables 2 to 4 below.

[0087] Table 2 Blank group titration results

[0088]

[0089] Table 3 Determination results of butadiene content in ABS

[0090]

[0091] Table 4 Determination results of butadiene content in compounds

[0092]

[0093] According to the butadiene content determination in Tables 2 to 4, the butadiene content of the compound ABS sulfonate flame retardant is 3.85% lower than that of the raw material ABS, indicating that the sulfonation position is on the double bond of butadiene.

[0094] Comparative Example 1

[0095] The same as Example 1, except that, in step 3), the sulfonation process is as follows: 80 g of ABS and 5 mL of 50% fuming sulfuric acid are placed in a reactor and reacted at 100° C. for 12 h, 24 h, 36 h, and 48 h, respectively, and fumigated with sulfur trioxide to obtain sulfonated ABS.

[0096] The results showed that the exterior of ABS was over-sulfonated and the structure was broken, so subsequent experiments could not be performed. In contrast, in Example 1, sulfonation of ABS using sulfur trioxide·dioxane complex as the sulfonating agent can obtain sulfonated ABS with uniform sulfonation and controllable sulfonation degree.

[0097] Comparative Example 2

[0098] Same as Example 1, except that the reaction temperature in step 2) is 0°C; and the dropping speed of the sulfur trioxide / dichloroethane solution is 1 s / drop.

[0099] The results show that the yield of sulfur trioxide·dioxane complex in this reaction is less than 10%. Analysis shows that this reaction is an exothermic reaction. Too high a temperature is not conducive to the reaction and easily leads to the escape of sulfur trioxide. In addition, this reaction is extremely exothermic and the droplet acceleration is too fast to maintain the system temperature. Example 1 solves the problem of low yield by lowering the reaction temperature and adjusting the droplet acceleration.

[0100] Comparative Example 3

[0101] The same as Example 1, except that the product sulfur trioxide·dioxane complex obtained in step 2) is stored at room temperature away from light.

[0102] As a result, it was found that the sulfonating agent sulfur trioxide·dioxane complex turned black and deteriorated, so the present invention needs to place it in a low temperature environment for long-term storage.

[0103] Comparative Example 4

[0104] The same as Example 1, except that step 3) is as follows: 30 g of ABS is dissolved in 300 mL of dichloromethane solution, and a 500 mL three-necked flask is used as a reaction container, and stirring is continued; at room temperature, 9.5 g of sulfur trioxide·dioxane complex is weighed and dissolved in 100 mL of tetrahydrofuran solution to obtain a complex solution, and then the complex solution is dripped into the three-necked flask containing ABS to react until the sulfonating agent (sulfur trioxide·dioxane complex) is completely dissolved, at which time the solution appears dark blue, and the reaction is continued for 4 h until the system temperature is consistent with room temperature, indicating that the reaction is completed, and a dichloromethane solution containing the intermediate compound is obtained; the dichloromethane solution containing the intermediate compound is dripped into boiling distilled water to remove the solvent and impurities, and filtered to obtain a yellow-white solid intermediate compound.

[0105] The results showed that the sulfonation effect of the sulfonating agent obtained by dissolving the sulfur trioxide·dioxane complex in tetrahydrofuran in advance was very weak. The experimental analysis found that there was heat release during the dissolution of the complex in tetrahydrofuran, indicating that the complex would react with tetrahydrofuran and weaken the sulfonation effect. In addition, the sulfonating agent is insoluble in dichloroethane and dichloromethane, so directly adding solid sulfur trioxide·dioxane complex is the best solution.

[0106] Application Example 1

[0107] 1) After dissolving the ABS sulfonate flame retardant in dichloromethane, the mixture was stirred and mixed with the polycarbonate (PC) masterbatch and placed in a 100°C blast drying oven for 10 hours (wherein the mass ratio of polycarbonate to ABS sulfonate flame retardant was 0.5:99.5), and then added to a twin-screw extruder for melt mixing and extrusion (the screw speed was set at 100 r / min), and then formed by an injection molding machine to obtain a polycarbonate material containing a sulfonate flame retardant, i.e., a polycarbonate flame retardant (composite material, denoted as PC / ABS-SK). The temperature parameter settings of each zone of the extruder are shown in Table 5.

[0108] Table 5 Temperature of each temperature section of twin screw extruder

[0109] Zone 1 Zone 2 Zone 3 District 4 District 5 District 6 District 7 District 8 District 9 Machine head 240℃ 240℃ 245℃ 245℃ 250℃ 250℃ 245℃ 240℃ 235℃ 230℃

[0110] 2) The prepared composite material was placed in a 100°C blast drying oven and dried for 10 hours. According to GB / T25156-2010, the experimental standard specimens were made by injection molding machine. The LOI values ​​of the test specimens were obtained by the ISO4589-1996 standard test, and the specimen specifications were 120mm×10mm×4mm. The vertical combustion test was measured by UL-94 standard, and the specimen specifications were 120mm×13mm×3.2mm. Injection molding pressure: 50MPa for the first and second sections respectively, and the temperature sections of the injection molding machine are listed in Table 6.

[0111] Table 6 Temperature of each zone of injection molding machine

[0112] Zone 1 Zone 2 Zone 3 District 4 District 5 270℃ 270℃ 270℃ 265℃ 260℃

[0113] Performance Test:

[0114] Table 7 Thermal performance test results of PC and PC / ABS-SK composite materials

[0115]

[0116]

[0117] Table 8 Mechanical properties test results of PC and PC / ABS-SK composites

[0118]

[0119] Figure 2 The TGA graphs of the ABS sulfonate flame retardant and ABS in Example 1 of the present invention under a nitrogen atmosphere; Figure 3 is the DTG graph of the ABS sulfonate flame retardant and ABS in Example 1 of the present invention under a nitrogen atmosphere; is the TGA and corresponding DTG curves of the ABS sulfonate flame retardant and ABS respectively measured under a nitrogen atmosphere at a heating rate of 20°C / min. Table 9 gives the main thermal degradation parameters. Definition: T onset T is the temperature at which the material loses 5% of its weight during thermal decomposition. max It is the temperature corresponding to the maximum thermal weight loss of the material.

[0120] Table 9 Thermal degradation parameters of ABS and ABS-SK in nitrogen atmosphere

[0121] sample atmosphere <![CDATA[T onset / ℃]]> <![CDATA[T max / ℃]]> Carbon residue at 800℃ / % ABS <![CDATA[N2]]> 394.3 341.7 0 ABS-SK <![CDATA[N2]]> 258.7 419.3 10.88

[0122] Depend on Figure 2 Part of the data obtained is listed in Table 9. As shown in Table 9, the T onsetIt is 258.7℃, which is the crystal water part of the flame retardant ABS-SK. The processing temperature range of PC is 240-270℃, and ABS-SK begins to decompose after 400℃, so it will not undergo thermal decomposition during PC processing and can meet the processing conditions of PC. After sulfonation modification, the initial decomposition temperature of ABS is advanced, which shows that sulfonates can promote the early decomposition of polymer ABS. As the temperature continues to rise, at 800℃, the residual carbon content of ABS-SK in a nitrogen atmosphere is 10.88%, which is a significant increase compared to 0.00% of ABS. This shows that this flame retardant has a good carbon-forming ability, thereby achieving a good flame retardant effect.

[0123] Figure 4 The TGA graphs of PC and PC / ABS-SK composite materials in Application Example 1 of the present invention under nitrogen atmosphere; Figure 5 The DTG graphs of PC and PC / ABS-SK composite materials in Application Example 1 of the present invention under nitrogen atmosphere are the TGA and corresponding DTG curves of PC and PC / ABS-SK composite materials measured under nitrogen atmosphere at a heating rate of 20°C / min. Table 9 gives the main thermal degradation parameters. Definition: V max It is the maximum mass loss rate that the sample can achieve during thermal decomposition.

[0124] Table 10 Thermal degradation parameters of PC and PC / ABS-SK composites in nitrogen atmosphere

[0125] sample atmosphere <![CDATA[T onset / ℃]]> <![CDATA[T max / ℃]]> <![CDATA[V max / (% / ℃)]]> Carbon residue at 800℃ / % PC <![CDATA[N2]]> 457.7 521 1.7 14.31 PC / ABS-SK <![CDATA[N2]]> 457.5 520 1.84 21.2

[0126] Table 10 shows that the initial decomposition temperature and maximum thermal weight loss temperature of PC and PC / ABS-SK composite materials under nitrogen atmosphere are basically the same, indicating that ABS-SK does not work in the early stage of thermal decomposition. max From 1.70% / ℃ to 1.84% / ℃, it shows that ABS-SK can promote the decomposition of PC. At 800℃, the residual carbon content of PC / ABS-SK increased from 14.31% to 21.20%, indicating that ABS-SK is mainly flame retardant in the condensed phase. This may be because the high temperature cross-links the olefins, resulting in incomplete combustion of PC, and the degradation of the PC substrate generates a more stable carbon layer, which slows down the decomposition rate of the carbon layer and increases the residual carbon content.

[0127] In summary, after thermal and mechanical property tests, the LOI of PC / ABS-SK composite material with an addition amount of 0.5wt / % was increased from 24.7% of PC to 40.5%, and the UL-94 test was increased from V-2 to V-0. With other mechanical properties basically unchanged, the impact strength reached 60.98kJ / m 2, which is not much different from pure PC, achieving the purpose of combining the characteristics of sulfonate flame retardant and ABS, and developing a flame retardant with good flame retardant properties and less effect on mechanical properties when the addition amount is not high.

[0128] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. An ABS sulfonate flame retardant, characterized in that: The flame retardant is a compound obtained by ion exchange of sulfonated acrylonitrile-butadiene-styrene copolymer, and the chemical structural formula of the compound is shown in Formula I:

2. A method for preparing the ABS sulfonate flame retardant according to claim 1, characterized in that: The following steps are involved: Using fuming sulfuric acid as a raw material, distilling sulfur trioxide and collecting it in a dichloroethane solution to obtain a dichloroethane solution containing sulfur trioxide; The dichloroethane solution containing sulfur trioxide is mixed with 1,4-dioxane to carry out complex reaction, and filtered to obtain sulfur trioxide·dioxane complex powder; adding the sulfur trioxide·dioxane complex powder into a dichloromethane solution of acrylonitrile-butadiene-styrene copolymer to carry out sulfonation treatment, distilling, filtering, and obtaining an intermediate compound; The intermediate compound is added to a dichloromethane solution, and a potassium hydroxide solution is added dropwise for neutralization. The organic phase is separated, washed with water, distilled, and filtered. The obtained sample is further added to dichloromethane for distillation to obtain an ABS sulfonate flame retardant.

3. The method for preparing the ABS sulfonate flame retardant according to claim 2, characterized in that: The mass-to-liquid ratio of the sulfur trioxide solution to the dichloroethane solution is 1 g:4.8 mL.

4. The method for preparing the ABS sulfonate flame retardant according to claim 2, characterized in that: The complexation reaction is carried out by dropping the 1,4-dioxane into the dichloroethane solution containing sulfur trioxide at a temperature below -10°C and under stirring, with the dropping speed being controlled at 5-10s / drop.

5. The method for preparing the ABS sulfonate flame retardant according to claim 2, characterized in that: The sulfonation treatment is carried out at room temperature under stirring for 4 hours; The mass-to-liquid ratio of the acrylonitrile-butadiene-styrene copolymer to the dichloromethane solution is 1 g: 10 mL; The mass ratio of the acrylonitrile-butadiene-styrene copolymer to the sulfur trioxide-dioxane complex powder is 1:0.

32.

6. The method for preparing the ABS sulfonate flame retardant according to claim 2, characterized in that: The neutralization treatment is carried out at room temperature with stirring for 12 hours until the pH of the solution reaches 8; The mass-to-liquid ratio of the intermediate compound to the dichloromethane solution is 1 g:10 mL.

7. A polycarbonate flame retardant, characterized in that: The ABS sulfonate flame retardant according to claim 1 and polycarbonate are used as raw materials, wherein the mass ratio of the polycarbonate to the ABS sulfonate flame retardant is 0.5:99.

5.

8. A method for preparing a polycarbonate flame retardant as claimed in claim 7, characterized in that: The method comprises the following steps: mixing the polycarbonate and the ABS sulfonate flame retardant, adding the mixture into a twin-screw extruder for melt mixing and extrusion, and then molding the mixture through an injection molding machine to obtain a polycarbonate material containing the sulfonate flame retardant.