Preparation method and application of zinc oxide antibacterial dispersion liquid for in-situ polymerization polyamide

By modifying the zinc oxide surface with a modifier and adding it during the polyamide polymerization process, the problem of insufficient dispersion of nano-zinc oxide is solved, and the efficient and low-cost preparation of antibacterial polyamide fibers is achieved.

CN118812918APending Publication Date: 2024-10-22ZHEJIANG HENGYI PETROCHEMICAL RES INST CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410772805.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing antibacterial polyamide fibers have insufficient dispersion of nano-zinc oxide during the spinning process, resulting in high production costs, poor dispersion, and the need for complex preparation steps and frequent component replacement.

Method used

Modifiers are used to modify the surface of zinc oxide, grind it to a specific particle size to form a stable dispersion, and add it directly during the polyamide polymerization process to achieve uniform dispersion of zinc oxide.

Benefits of technology

The dispersion and compatibility of nano-zinc oxide in polyamide is improved, the production cost is reduced, the spinning process is simplified, and the one-step preparation of antibacterial polyamide fiber is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812918A_ABST
    Figure CN118812918A_ABST
Patent Text Reader

Abstract

The invention relates to the field of polyamide, and discloses a preparation method and application of a zinc oxide antibacterial dispersion liquid for in-situ polymerization of polyamide. The preparation method comprises the following steps: 1) preparing a zinc oxide pre-dispersion liquid; 2) dissolving a modifier in water for hydrolysis to obtain a modifier hydrolysate; 3) dropwise adding the modifier hydrolysate into the zinc oxide pre-dispersion liquid, and heating for reaction; (4) grinding until the particle size is D99lt; 1 [mu] m; and 5) adding a stabilizer, and uniformly dispersing to obtain the zinc oxide antibacterial dispersion liquid for in-situ polymerization polyamide. According to the invention, the surface of zinc oxide is modified by adopting the modifier which has good compatibility with polyamide and can participate in polyamide polymerization reaction, and the zinc oxide antibacterial dispersion liquid which is stably dispersed can be obtained after grinding to a specific particle size and can be directly added into a reaction system in a polyamide polymerization stage; and performing in-situ polymerization to obtain the antibacterial polyamide with uniformly dispersed zinc oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyamide, and in particular to a preparation method and application of a zinc oxide antibacterial dispersion for in-situ polymerized polyamide. Background Art

[0002] In recent years, antibacterial fibers added with antibacterial agents have been widely used in the field of textiles and clothing. This antibacterial fabric, which is different from the post-finishing method, has excellent weather resistance and durability. It has the function of inhibiting or killing harmful bacteria. It can effectively reduce human contact with pathogenic bacteria during use. With the trend of widespread application of antibacterial materials, different types of antibacterial agents have emerged. As a commonly used synthetic fiber for clothing, polyamide fiber is corrosion-resistant, mildew-resistant, has high breaking strength and excellent wear resistance. It can be further endowed with antibacterial, antistatic, flame retardant and other properties to adapt to a variety of uses. Among many inorganic nano antibacterial agents, nano zinc oxide has a strong inhibitory effect on Escherichia coli, Staphylococcus aureus, Candida albicans, etc., and has been widely used in fibers.

[0003] The main method for producing antibacterial fibers is to blend and melt-blend the fiber substrate and nano zinc oxide. This technology requires the addition of zinc oxide antibacterial masterbatch during the spinning process. For example, a Chinese patent (publication number CN112144132B) discloses a method for preparing nano zinc oxide antibacterial chemical fiber masterbatch, which requires the modification, grinding, and spray drying of nano zinc oxide in a solution, and the high-speed mixing of the modified nano zinc oxide with the masterbatch matrix, and the melt extrusion and pelletizing to obtain the chemical fiber masterbatch. The masterbatch spinning method is easy to operate, but the preparation steps of zinc oxide masterbatch are cumbersome, the procedure is complicated, and there are still certain problems with dispersibility, and the component cycle is short in the spinning process.

[0004] Therefore, how to change the existing development mode of antibacterial polyamide fibers, improve the dispersion of nano zinc oxide antibacterial agents in the polyamide matrix, reduce the frequency of component replacement during the spinning process, reduce production costs, and realize the one-step preparation of antibacterial polyamide fibers is a problem that needs to be solved urgently. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for preparing an antibacterial zinc oxide dispersion for in-situ polymerization of polyamide and its application. The present invention uses a modifier that has good compatibility with polyamide and can participate in the polymerization reaction of polyamide to modify the surface of zinc oxide, and after grinding to a specific particle size, a stably dispersed antibacterial zinc oxide dispersion can be obtained, which can be directly added to the reaction system in the polyamide polymerization stage, and in-situ polymerization is performed to obtain an antibacterial polyamide with uniformly dispersed zinc oxide.

[0006] The specific technical scheme of the present invention is: In a first aspect, the present invention provides a method for preparing an antibacterial zinc oxide dispersion for in-situ polymerization of polyamide, comprising the following steps: 1) Prepare an acidic or alkaline zinc oxide pre-dispersion liquid with a zinc oxide particle size D50 <2 μm.

[0007] 2) dissolving the modifier in water and stirring to hydrolyze to obtain a modifier hydrolyzate; the modifier is a silane containing a polyether segment and a terminal hydroxyl group, or one or more zirconate, titanate or silane compounds containing a hydrolyzable group and a terminal amino group or epoxy group or polyhydroxyl group.

[0008] 3) adding the modifier hydrolyzate dropwise to the zinc oxide pre-dispersion solution, and heating the solution for reaction after the addition is complete.

[0009] 4) Grinding until the particle size D99 of the modified nano zinc oxide in the obtained dispersion is less than 1 μm.

[0010] 5) adding a stabilizer to the dispersion obtained in step 4) and dispersing the dispersion uniformly to obtain an antibacterial zinc oxide dispersion for in-situ polymerized polyamide.

[0011] The present invention uses a modifier to modify the surface of zinc oxide, and after grinding to a specific particle size, a stably dispersed zinc oxide antibacterial dispersion can be obtained, which can be directly added to the reaction system in the polyamide polymerization stage to obtain antibacterial polyamide with uniformly dispersed zinc oxide through in-situ polymerization.

[0012] Specifically, the molecular structure of the above modifier has the following structural features: ① It contains a hydrolyzable group, which can react with the hydroxyl group on the surface of zinc oxide after hydrolysis, thereby achieving the purpose of chemical grafting modification; ② It contains active groups such as terminal amino groups, epoxy groups or hydroxyl groups that can react after the ring opening of caprolactam, thereby achieving covalent cross-linking with the polymer, improving the dispersibility and compatibility of nano zinc oxide, and not easy to fall off and precipitate. In particular, when the modifier is a silane containing a polyether segment and a terminal hydroxyl group, its molecule also has a polyether segment, and the polyether segment has good compatibility with polyamide, so it can further improve the dispersibility and compatibility of nano zinc oxide in polyamide.

[0013] The present invention found that the particle size of zinc oxide in the dispersion has a significant effect on its dispersion stability. After testing, it was finally determined that the best effect was achieved when the particle size D99 of the modified nano zinc oxide in the antibacterial dispersion was less than 1 μm. After being added to the polyamide matrix, the dispersion was uniform and fewer particles were visible to the naked eye under an optical microscope.

[0014] Preferably, in step 1), the pH of the zinc oxide pre-dispersion liquid is 5-6 or 8-10.

[0015] The pH value of the zinc oxide pre-dispersion affects the dehydration condensation effect of zinc oxide and the modifier during the subsequent modification. The modifier can undergo dehydration condensation with the zinc oxide surface under acidic or alkaline conditions, but when the pH value is too low, the modifier tends to self-condense to form chain molecules; when it is too high, it tends to self-condense to form agglomerated particles. The reaction rate with zinc oxide is low, and the degree of modification of the zinc oxide surface is low.

[0016] Preferably, in step 2), the hydrolysis is carried out until the conductivity reaches 400-500 μs / cm.

[0017] The higher the hydrolysis degree of the modifier, the higher the silanol content in the hydrolyzate, the greater the conductivity, and the silanol will undergo a dehydration condensation reaction with zinc oxide and be covalently bonded to the surface of zinc oxide. If the hydrolysis degree is too low, the modifier will self-polymerize after being added to the pre-dispersion liquid, and the surface of zinc oxide cannot be fully modified; if it is too high, the modifier will self-polymerize to a certain extent during pre-hydrolysis due to the long hydrolysis time, resulting in a decrease in the effective modified components. Therefore, the degree of hydrolysis needs to be controlled by conductivity.

[0018] Preferably, in step 2), the silane containing a polyether segment and a terminal hydroxyl group is polyethylene glycol trimethoxysilyl propyl ether.

[0019] Preferably, in step 2): The zirconate compound is selected from one or more of tetrakis(triethanolamine)zirconium, neoalkoxytris(ethylenediamine N-ethoxy)zirconate, and bis-neoalkoxybis(4-aminobenzoyloxy)zirconate.

[0020] The phthalate compound is isopropoxy tris(ethylenediamino-N-ethoxy) titanate.

[0021] The silane compound is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-diethylenetriaminopropylmethyldimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.

[0022] Preferably, in step 2), the amount of the modifier used is 2-6 wt % of zinc oxide.

[0023] The invention can make the nano zinc oxide evenly dispersed in the polyamide matrix by controlling the amount of the modifier.

[0024] Preferably, in step 3), the modifier hydrolyzate is added dropwise within 20 min. Preferably, in step 3), the temperature of the temperature-raising reaction is 70-95° C. and the time is 2-12 h.

[0025] Preferably, in step 3), the unreacted small molecules are removed by filtering after the temperature-raising reaction.

[0026] The present invention also found that when zinc oxide is modified by the modifier hydrolyzate, the unreacted small molecules will have a negative impact on the storage stability of the dispersion. Therefore, it is preferred to filter out the unreacted small molecules after the temperature reaction.

[0027] Preferably, in step 3), a ceramic filter membrane is used for filtration, and the pore size of the membrane is smaller than the primary particle size of the nano zinc oxide used; the filtration is stopped when the conductivity of the dispersion containing the zinc oxide portion (i.e., the zinc oxide portion) is less than 100 μs / cm.

[0028] After modification by the modifier, there are some small molecular oligomers and unreacted monomers. The presence of these substances has a great influence on the storage stability of the dispersion. During long-term storage, they play a bridging role, causing the agglomeration of zinc oxide particles, resulting in an increase in the particle size of the dispersion and even precipitation. Therefore, these substances need to be removed as much as possible.

[0029] Preferably, in step 4), grinding is performed using grinding beads with a diameter of less than 0.6 mm.

[0030] Preferably, in step 5), the stabilizer is selected from one or more of polyethylene glycol (Mw < 1000), polyvinyl pyrrolidone (K15, K17, K30), hydroxypropyl methylcellulose (HPMC), carboxymethyl cellulose (CMC) and Span 80.

[0031] Since polyamide polymerization is carried out in a high temperature and high pressure environment, the present invention specifically selects the above stability with a higher thermal decomposition temperature, which can be applied to a polyamide reaction system in which water is used as a catalyst or solvent during polymerization.

[0032] Preferably, in step 5), the amount of the stabilizer is 2-10 wt % of zinc oxide.

[0033] Preferably, in step 5), the solid content of the zinc oxide antibacterial dispersion for in-situ polymerization of polyamide is 10-20wt%.

[0034] In a second aspect, the present invention provides the use of the zinc oxide antibacterial dispersion for in-situ polymerization of polyamide obtained by the above preparation method in in-situ polymerization of polyamide.

[0035] Preferably, the preparation method of the in situ polymerized polyamide is as follows: the preparation method of the in situ polymerized polyamide comprises: mixing caprolactam, zinc oxide antibacterial dispersion for in situ polymerized polyamide, water and a catalyst, heating until the caprolactam melts, beating, removing air, heating to react, pelletizing, extracting and drying to obtain in situ polymerized polyamide slices.

[0036] Compared with the prior art, the beneficial effects of the present invention are: (1) The present invention uses a modifier that has good compatibility with polyamide and can participate in the polyamide polymerization reaction to modify the surface of zinc oxide. After grinding to a specific particle size, a stably dispersed antibacterial zinc oxide dispersion can be obtained, which can be directly added to the reaction system of the polyamide polymerization stage to obtain an antibacterial polyamide with uniformly dispersed zinc oxide through in-situ polymerization.

[0037] (2) The nano zinc oxide particles in the zinc oxide antibacterial dispersion of the present invention can be evenly dispersed in the aqueous phase and will not stratify or agglomerate after being placed for 30 days.

[0038] (3) The antibacterial zinc oxide dispersion of the present invention is applied to the polymerization process of polyamide. No special operation is required during the polymerization. The modified zinc oxide can be added to the reaction system together with the reactants, which has little effect on the polymerization reaction and has no effect on the performance indicators of polyamide, and the antibacterial ability of zinc oxide can be fully exerted. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The digital photos (magnification 100 times) of the dispersion of zinc oxide in polyamide 6 slices in Example 1 and Comparative Example 4 are shown. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with the embodiments.

[0041] Overall embodiment First, a method for preparing an antibacterial zinc oxide dispersion for in-situ polymerization of polyamide comprises the following steps: A zinc oxide pre-dispersion liquid with a zinc oxide particle size D50 less than 2 μm and being acidic or alkaline is prepared.

[0042] In some specific implementation cases, step 1) specifically includes: dispersing nano zinc oxide in water until the particle size D50 is less than 2 μm, and adding an acidic regulator or an alkaline regulator to adjust the pH to 5-6 or 8-10 to obtain a zinc oxide pre-dispersion liquid with a solid content of 10-30 wt%.

[0043] In some specific implementation cases, the primary particle size of the nano zinc oxide is less than 100 nm.

[0044] In some specific implementation cases, the acidic regulator is one or more of hydrochloric acid, acetic acid, citric acid, and lauric acid. The alkaline regulator is one or more of ammonia water or organic amines such as triethanolamine, diethanolamine, butylethanolamine, N-methylethanolamine, and 2-amino-2-methyl-1-propyl.

[0045] 2) dissolving the modifier in water and stirring to hydrolyze to obtain a modifier hydrolyzate; the modifier is a silane containing a polyether segment and a terminal hydroxyl group, or one or more zirconate, titanate or silane compounds containing a hydrolyzable group and a terminal amino group or epoxy group or polyhydroxyl group.

[0046] In some specific implementation cases, the hydrolysis is hydrolyzed to a conductivity of 400-500 μs / cm.

[0047] In some specific implementation cases, the silane containing a polyether segment and a terminal hydroxyl group is polyethylene glycol trimethoxysilyl propyl ether.

[0048] In some specific implementation cases, the zirconate compound is selected from one or more of tetrakis(triethanolamine)zirconium, neoalkoxytris(ethylenediamino-N-ethoxy)zirconate, and bis-neoalkoxybis(4-aminobenzoyloxy)zirconate. In some specific implementation cases, the phthalate compound is isopropoxytris(ethylenediamino-N-ethoxy)titanate. In some specific implementation cases, the silane compound is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-diethylenetriaminopropylmethyldimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.

[0049] In some specific implementation cases, the amount of the modifier is 2-6 wt % of zinc oxide.

[0050] 3) adding the modifier hydrolyzate dropwise to the zinc oxide pre-dispersion solution, heating the solution for reaction after the addition is complete, and filtering to remove unreacted small molecules.

[0051] In some specific implementation cases, the modifier hydrolyzate is added dropwise within 20 minutes. In some specific implementation cases, the temperature of the temperature-raising reaction is 70-95° C., and the time is 2-12 hours.

[0052] In some specific implementation cases, a ceramic filter membrane is used for filtration, and the pore size of the membrane is smaller than the primary particle size of the nano zinc oxide used; when the conductivity of the unfiltered portion of the dispersion is less than 100 μs / cm, filtration is stopped.

[0053] 4) Grinding until the particle size D99 of the modified nano zinc oxide in the obtained dispersion is less than 1 μm.

[0054] In some specific implementation cases, the grinding uses grinding beads with a diameter of less than 0.6 mm.

[0055] 5) adding a stabilizer to the dispersion obtained in step 4) and dispersing the dispersion uniformly to obtain an antibacterial zinc oxide dispersion for in-situ polymerized polyamide.

[0056] In some specific implementation cases, the stabilizer is selected from one or more of polyethylene glycol (Mw < 1000), polyvinyl pyrrolidone (K15, K17, K30), hydroxypropyl methylcellulose (HPMC), carboxymethyl cellulose (CMC) and Span 80. In some specific implementation cases, the amount of the stabilizer is 2-10wt% of the zinc oxide.

[0057] In some specific implementation cases, the solid content of the zinc oxide antibacterial dispersion for in-situ polymerization of polyamide is 10-20wt%.

[0058] Secondly, the zinc oxide antibacterial dispersion for in-situ polymerization of polyamide obtained by the above preparation method is used in in-situ polymerization of polyamide.

[0059] In some specific implementation cases, the preparation method of the in situ polymerized polyamide is as follows: caprolactam, zinc oxide antibacterial dispersion for in situ polymerized polyamide (solvent is not included), deionized water (water in the dispersion is included) and a catalyst are added into a reactor in a mass ratio of 100:(0.5-2):(3-8):(0.1-1), heated until the caprolactam is melted, slurried, nitrogen is introduced to remove air from the device, the internal temperature is increased to 220-240°C, the pressure is 0.5-1.2Mpa, and after reacting for 2-3h, the pressure is slowly released; the internal temperature is increased to 240-255°C, and vacuumed to -0.05Mpa, reacting for 2-4h, pelletizing, extracting, and drying to obtain in situ polymerized polyamide slices.

[0060] Specific Examples and Comparative Examples Example 1 Take 50g of zinc oxide powder with a particle size of about 50nm, put it in a container, add 430g of deionized water, disperse at high speed for 30 minutes, and the particle size test shows that D50 is 1.68μm. Add ammonia water to adjust the pH value to about 9. Slowly add 20g of 10% 3-aminopropyltriethoxysilane aqueous solution hydrolyzed to a conductivity of about 420μs / cm, and add it dropwise within 10 minutes. Heat to 70℃, stir and react for 12 hours, filter with a ceramic membrane until the conductivity of the dispersion containing the zinc oxide part is less than 100μs / cm, and remove small molecules that have not reacted with zinc oxide. Grind the zinc oxide dispersion with 0.3mm grinding beads, keep the grinding temperature not higher than 50℃, and grind until D99 is less than 1μm. Dilute the dispersion to 10%, take 350g, add 1.4g PEG400 and stir evenly to obtain a nano zinc oxide dispersion for polyamide.

[0061] The final particle size data of the nano zinc oxide dispersion using this method is shown in Table 1.

[0062] Comparative Example 1 (the difference from Example 1 is that no modification with a modifier is performed) Take 50g of zinc oxide powder with a particle size of about 50nm, put it in a container, add 430g of deionized water, disperse at high speed for 30 minutes, and the particle size test D50 = 1.68μm, add ammonia water to adjust the pH value to about 9. Use 0.3mm grinding beads for grinding, keep the grinding temperature not higher than 50℃, and grind for 40min. Take 350g of the ground dispersion, add 1.4g PEG400 and stir evenly to obtain a nano zinc oxide dispersion for polyamide.

[0063] The final particle size data of the nano zinc oxide dispersion using this method is shown in Table 1.

[0064] Comparative Example 2 (the only difference from Example 1 is that the particle size is too large) Take 50g of zinc oxide powder with a particle size of about 50nm, put it in a container, add 430g of deionized water, disperse at high speed for 5 minutes, and the particle size test shows that D50 = 4.8μm. Add ammonia water to adjust the pH value to about 9. Slowly add 20g of 10% 3-aminopropyltriethoxysilane aqueous solution hydrolyzed to a conductivity of about 420μs / cm, and add it dropwise within 10 minutes. Heat to 75℃, stir and react for 6 hours, filter with a ceramic membrane until the conductivity of the dispersion containing zinc oxide is less than 100μs / cm, and remove small molecules that have not reacted with zinc oxide. Use 0.3mm grinding beads for grinding, keep the grinding temperature not higher than 50℃, grind for 60min, and then D99 = 5.57μm. Dilute the dispersion to 10%, take 350g, add 1.4g PEG400 and stir evenly to obtain a zinc oxide dispersion.

[0065] Since the particle size of the nano zinc oxide pre-dispersion is relatively large, and the particle size after final grinding is still relatively large, the particle size data of the final nano zinc oxide dispersion is shown in Table 1.

[0066] Comparative Example 3 (the only difference from Example 1 is that the pre-hydrolysis degree of the modifier is insufficient) Take 50g of zinc oxide powder with a particle size of about 50nm, put it in a container, add 430g of deionized water, disperse at high speed for 30 minutes, and the particle size test D50 = 1.68μm, add ammonia water to adjust the pH value to about 9. Slowly add 20g of 10% 3-aminopropyltriethoxysilane aqueous solution hydrolyzed to a conductivity of about 220μs / cm, and add it dropwise within 10 minutes. Heat to 70℃, stir and react for 12 hours, filter with a ceramic membrane until the conductivity of the unfiltered part of the dispersion is less than 100μs / cm, and remove small molecules that do not react with zinc oxide. Use 0.3mm grinding beads for grinding, keep the grinding temperature not higher than 50℃, and grind for 40min. Dilute the dispersion to 10%, take 350g, add 1.4g PEG400 and stir evenly to obtain a nano zinc oxide dispersion for polyamide. The final nano zinc oxide dispersion particle size data of this method is shown in Table 1.

[0067] Comparative Example 4 (the only difference from Example 1 is that the degree of pre-hydrolysis of the modifier is too high) Take 50g of zinc oxide powder with a particle size of about 50nm, put it in a container, add 430g of deionized water, disperse at high speed for 30 minutes, and the particle size test D50 = 1.68μm, add ammonia water to adjust the pH value to about 9. Slowly add 20g of 10% 3-aminopropyltriethoxysilane aqueous solution hydrolyzed to a conductivity of about 550μs / cm, and add it dropwise within 10 minutes. Heat to 70℃, stir and react for 12 hours while heating, filter with a ceramic membrane until the conductivity of the dispersion containing zinc oxide is less than 100μs / cm, remove small molecules that do not react with zinc oxide, grind with 0.3mm grinding beads, keep the grinding temperature not higher than 50℃, and grind for 40min. Dilute the dispersion to 10%, take 350g, add 7g PEG400 and stir evenly, and get a nano zinc oxide dispersion for polyamide. The final nano zinc oxide dispersion particle size data of this method is shown in Table 1.

[0068] Example 2 Take 100g of zinc oxide powder with a particle size of about 30nm, put it in a container, add 214g of deionized water, disperse at high speed for 40 minutes, and the particle size test shows that D50=1.76μm. Add diethanolamine to adjust the pH value to about 10. Slowly add 20g of 30% γ-glycidyloxypropyltrimethoxysilane aqueous solution hydrolyzed to a conductivity of about 450μs / cm, and add it dropwise within 20 minutes. Heat to 95℃, stir and react for 2 hours, filter with a ceramic membrane until the conductivity of the dispersion containing the zinc oxide part is less than 100μs / cm, and remove small molecules that have not reacted with zinc oxide. Use 0.3mm grinding beads for grinding, keep the grinding temperature not higher than 50℃, grind for 60min, and then D99<1μm. Dilute the dispersion to 20%, take 300g, add 3g Span 80 and stir evenly to obtain a nano zinc oxide dispersion for polyamide.

[0069] The final particle size data of the nano zinc oxide dispersion using this method is shown in Table 1.

[0070] Comparative Example 5 (the difference from Example 2 is that ultrafiltration treatment was not performed) Take 100g zinc oxide powder with a particle size of about 30nm, put it in a container, add 214g deionized water, disperse at high speed for 40 minutes, and the particle size test D50 = 1.76μm, add diethanolamine to adjust the pH value to about 10. Slowly add 20g 30% γ-glycidyl ether oxypropyl trimethoxysilane aqueous solution hydrolyzed to a conductivity of about 450μs / cm, and add it dropwise within 20 minutes. Heat to 95℃, stir and react for 2 hours, grind with 0.3mm grinding beads, keep the grinding temperature not higher than 50℃, and grind for 60min until D99 <1μm. Dilute the dispersion to 20%, take 300g, add 3g Span 80 and stir evenly to obtain a nano zinc oxide dispersion for polyamide.

[0071] The final particle size data of the nano zinc oxide dispersion using this method is shown in Table 1.

[0072] Example 3 Take 100g of zinc oxide powder with a particle size of about 80nm, put it in a container, add 380g of deionized water, disperse at high speed for 40 minutes, and the particle size test D50 = 1.92μ m, add hydrochloric acid to adjust the pH value to about 5. Slowly add 20g of 20% new alkoxy tris (ethylenediamine N-ethoxy) zirconate aqueous solution hydrolyzed to a conductivity of about 450μ s / cm, and add it dropwise within 20 minutes. Heat to 80℃, stir and react for 5 hours, filter with a ceramic membrane until the conductivity of the dispersion containing the zinc oxide part is less than 100μ s / cm, and remove small molecules that do not react with zinc oxide. Use 0.3mm grinding beads for grinding, keep the grinding temperature not higher than 50℃, and grind to D99 <1μ m. Dilute the dispersion to 10%, take 300g, add 3g polyvinyl pyrrolidone (K30) and stir evenly to obtain a nano zinc oxide dispersion for polyamide.

[0073] The final particle size data of the nano zinc oxide dispersion using this method is shown in Table 1.

[0074] Example 4 Take 50g of zinc oxide powder with a particle size of about 50nm, put it in a container, add 430g of deionized water, disperse it at high speed for 30 minutes, and the particle size test D50=1.68μ m, add ammonia water to adjust the pH value to about 8. Slowly add 40g of 15% polyethylene glycol trimethoxysilyl propyl ether aqueous solution hydrolyzed to a conductivity of about 400μ s / cm, and add it dropwise within 20 minutes. Heat to 80℃, stir and react for 6 hours, filter with a ceramic membrane until the conductivity of the dispersion containing the zinc oxide part is less than 100μ s / cm, and remove small molecules that do not react with zinc oxide. Grind the zinc oxide dispersion with 0.3mm grinding beads, keep the grinding temperature not higher than 50℃, and grind to D99<1μ m. Dilute the dispersion to 10%, take 300g, add 0.6g PEG2000 and stir evenly, and obtain a nano zinc oxide dispersion for polyamide.

[0075] The final particle size data of the nano zinc oxide dispersion using this method is shown in Table 1.

[0076] Example 5 Take 50g of zinc oxide powder with a particle size of about 50nm, put it in a container, add 430g of deionized water, disperse at high speed for 30 minutes, and the particle size test D50=1.68μ m, add ammonia water to adjust the pH value to about 10. Slowly add 50g of 10% tetrakis(triethanolamine) zirconium aqueous solution hydrolyzed to a conductivity of about 400μ s / cm, and add it dropwise within 10 minutes. Heat to 85℃, stir and react for 12 hours, filter with a ceramic membrane until the conductivity of the dispersion containing the zinc oxide part is less than 100μ s / cm, and remove small molecules that do not react with zinc oxide. Grind the zinc oxide dispersion with 0.3mm grinding beads, keep the grinding temperature not higher than 50℃, and grind to D99<1μ m. Take 300g, add 1.5g of polyvinyl pyrrolidone K15 and stir evenly, and obtain a nano zinc oxide dispersion for polyamide.

[0077] The final particle size data of the nano zinc oxide dispersion using this method is shown in Table 1.

[0078] Example 6 Take 50g of zinc oxide powder with a particle size of about 50nm, put it in a container, add 430g of deionized water, disperse at high speed for 30 minutes, and the particle size test shows that D50=1.68μm. Add ammonia water to adjust the pH value to about 8. Slowly add 50g of 10% isopropoxy tris(ethylenediamine-N-ethoxy) titanate aqueous solution hydrolyzed to a conductivity of about 400μs / cm, and add it dropwise within 10 minutes. Heat to 75℃, stir and react for 12 hours, filter with a ceramic membrane until the conductivity of the dispersion containing the zinc oxide part is less than 100μs / cm, and remove small molecules that have not reacted with zinc oxide. Grind the zinc oxide dispersion with 0.3mm grinding beads, keep the grinding temperature not higher than 50℃, and grind until D99<1μm. Because it cannot be completely discharged from the grinding machine cavity, take 300g of the ground dispersion, add 2g of hydroxypropyl methylcellulose and stir evenly to obtain a nano zinc oxide dispersion for polyamide.

[0079] The final particle size data of the nano zinc oxide dispersion using this method is shown in Table 1.

[0080] Performance Testing (I) Particle size test: The particle size was determined using a Malvern 3000 laser particle size analyzer.

[0081] Table 1 (1) The difference between Control Example 1 and Example 1 is whether or not the surface of the zinc oxide is modified by a modifier. From the data in Table 1, it can be seen that the surface modification step of zinc oxide is essential. The particle size of the zinc oxide dispersion cannot be reduced by simply adding several stabilizers selected by the present invention after grinding; The difference between Control Example 2 and Example 1 is that the particle size of the pre-dispersion liquid is different. From the above data, it can be seen that the dispersion effect of the pre-dispersion liquid has a great influence on the dispersion of zinc oxide in the later stage. It is necessary to fully pre-disperse to fully wet the zinc oxide and improve the reaction activity during the modification of the later modifier; The difference between Control Examples 3 and 4 and Example 1 is that the degree of pre-hydrolysis (conductivity) of the modifier is too low and too high, and its degree has a certain influence on the modification of zinc oxide. If the degree of hydrolysis is too low, the modifier tends to self-polymerize after being added to the pre-dispersion liquid, and cannot fully modify the surface of zinc oxide; when it is too high, due to the long hydrolysis time, the modifier will undergo a certain degree of self-polymerization during the pre-hydrolysis, resulting in a decrease in the effective modified component. Therefore, too high or too low a concentration cannot effectively modify the surface of zinc oxide, resulting in certain changes in the degree of dispersion and stability.

[0082] (2) The difference between Control Example 5 and Example 2 is whether or not ultrafiltration treatment is performed. Control Example 5 does not remove small molecules, and finally obtains a nano zinc oxide dispersion with a qualified particle size and good dispersion. However, due to the bridging effect of the residual small molecules, the long-term storage stability of the dispersion is poor, and stratification occurs after 15 days of storage.

[0083] (3) The difference between Example 3-6 and Example 1 is that other types of modifiers are replaced. The results show that under the modification of the modifiers selected in Examples 3-6, the zinc oxide particle size is all less than 1 μm, and the effect of polyethylene glycol trimethoxysilyl propyl ether is better and the particle size is smaller.

[0084] Figure 1 The dispersion of zinc oxide in the zinc oxide antibacterial polyamide 6 prepared by in-situ hydrolysis ring-opening polymerization in the dispersion of Example 1. The zinc oxide has a small particle size and is evenly distributed in the nylon 6 matrix, and fewer particles can be seen under an optical microscope.

[0085] (II) Application of zinc oxide antibacterial dispersion The above-mentioned embodiment and control example were subjected to in-situ antibacterial polyamide 6 polymerization, and the preparation method thereof was as follows: caprolactam, zinc oxide antibacterial dispersion, deionized water (including water in the dispersion) and boric acid in a mass ratio of 100:1:5:0.1 were added to the reactor, heated until the caprolactam melted, slurried, nitrogen was introduced to remove the air in the device, the internal temperature was raised to 230°C, and the pressure was 1.0 MPa. After reacting for 2 hours, the pressure was slowly released to discharge water; after the pressure was released to 0, the temperature was raised to 250°C, and vacuumed to -0.05 MPa, reacted for 3 hours, pelletized, and dried to obtain in-situ polymerized polyamide 6 slices. The slices were observed for agglomerated particles, and the test results are shown in Table 2.

[0086] Table 2 Case Agglomerated particles (pieces / mg) Example 1 0.5 Comparative Example 1 Unable to count Comparative Example 2 Unable to count Comparative Example 3 12 Comparative Example 4 Unable to count Example 2 0.8 Comparative Example 5 2.3 Example 3 0.9 Example 4 0.2 Example 5 0.5 Example 6 0.6 The number of slice agglomerated particles obtained by polymerization of Examples 1-6 is less than 1 / mg. The control example 1 does not perform modifier modification, resulting in poor compatibility between zinc oxide and polyamide 6 during the polymerization process, and serious agglomeration during polymerization, resulting in too many agglomerated particles. The control example 2 has insufficient pre-dispersion effect, and the control examples 3 and 4 have poor degree of coupling agent modification on the surface of zinc oxide due to the degree of hydrolysis of the pre-hydrolyzed liquid. The zinc oxide particles agglomerate during polymerization, resulting in an increase in the number of agglomerated particles. The control example 5 does not perform ultrafiltration of small molecules. The residual small molecules during polymerization will cause a small increase in agglomerated particles, which does not affect the quality of the slices.

[0087] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0088] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a zinc oxide antibacterial dispersion for in-situ polymerized polyamide, Features The following steps are involved: 1) Preparing an acidic or alkaline zinc oxide pre-dispersion solution with a zinc oxide particle size D50 < 2 μm; 2) dissolving the modifier in water and stirring to hydrolyze to obtain a modifier hydrolyzate; the modifier is a silane containing a polyether segment and a terminal hydroxyl group, or one or more zirconate, titanate and silane compounds containing a hydrolyzable group and a terminal amino group or epoxy group or polyhydroxyl group; 3) adding the modifier hydrolyzate dropwise to the zinc oxide pre-dispersion solution, and heating the solution for reaction after the addition is complete; 4) Grinding until the particle size D99 of the modified nano zinc oxide in the obtained dispersion is less than 1 μm; 5) Adding a stabilizer to the dispersion obtained in step 4) and dispersing the dispersion evenly to obtain an antibacterial zinc oxide dispersion for in-situ polymerized polyamide.

2. The preparation method according to claim 1, Features: In step 1), the pH of the zinc oxide pre-dispersion liquid is 5-6 or 8-10.

3. The preparation method according to claim 1, Features: In step 2), the hydrolysis is performed to a conductivity of 400-500 μs / cm.

4. The preparation method according to claim 1 or 3, Features: In step 2), the silane containing a polyether segment and a terminal hydroxyl group is polyethylene glycol trimethoxysilyl propyl ether.

5. The preparation method according to claim 1 or 3, Features: In step 2), The zirconate compound is selected from one or more of tetrakis(triethanolamine)zirconium, neoalkoxytris(ethylenediamine N-ethoxy)zirconate, and bis-neoalkoxybis(4-aminobenzoyloxy)zirconate; The phthalate compound is isopropoxy tris(ethylenediamino-N-ethoxy) titanate; The silane compound is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-diethylenetriaminopropylmethyldimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.

6. The preparation method according to claim 1 or 3, Features: In step 2), the amount of the modifier used is 2-6 wt % of zinc oxide.

7. The preparation method according to claim 1, Features: In step 3), The modifier hydrolyzate was added dropwise within 20 minutes; The temperature of the temperature-raising reaction is 70-95° C. and the time is 2-12 hours.

8. The preparation method according to claim 1 or 7, Features: In step 3), After the temperature rise reaction, unreacted small molecules are removed by filtration; A ceramic filter membrane is used for filtration, and the pore size of the membrane is smaller than the primary particle size of the nano zinc oxide used; Stop filtering when the conductivity of the dispersion containing the zinc oxide portion is <100 μs / cm.

9. The preparation method according to claim 1, Features: In step 5), The stabilizer is selected from one or more of polyethylene glycol, polyvinyl pyrrolidone, hydroxypropyl methylcellulose, carboxymethyl cellulose and Span 80; The amount of the stabilizer used is 2-10wt% of zinc oxide.

10. The preparation method according to claim 1 or 9, Features: In step 5), the solid content of the zinc oxide antibacterial dispersion for in-situ polymerization of polyamide is 10-20wt%.

11. Use of the zinc oxide antibacterial dispersion for in-situ polymerization of polyamide obtained by the preparation method according to any one of claims 1 to 10 in in-situ polymerization of polyamide.

12. The use according to claim 11, Features: The preparation method of the in-situ polymerized polyamide comprises: mixing caprolactam, zinc oxide antibacterial dispersion for in-situ polymerized polyamide, water and a catalyst, heating until the caprolactam melts, beating, removing air, heating to react, pelletizing, extracting and drying to obtain in-situ polymerized polyamide slices.

Citation Information

Cited By

  • Method for preparing zinc oxide / nylon 6 slice through in-situ polymerization

    CN119931027A

  • A method for in-situ polymerization of zinc oxide / nylon 6 chips

    CN119931027B

  • Antibacterial nylon 6 elastomer and preparation method thereof

    CN120271813A