PP corrugated pipe and preparation method thereof
By using copolymers of hydrophilic-modified and lipophilic-modified capsaicin and PP resin in polypropylene corrugated pipes, combined with anti-rodent coatings, the problem of poor anti-rodent effect of polypropylene corrugated pipes in automobile wiring harnesses has been solved and achieved Better dispersion and rodent resistance.
Patent Information
- Application Number
- CN202410922440.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-22
AI Technical Summary
Existing polypropylene corrugated pipes are prone to rat bites in automobile wiring harnesses, and capsaicin has poor dispersion in PP materials, resulting in poor anti-rat effects.
A copolymer of hydrophilic modified capsaicin and lipophilic modified capsaicin and PP resin is used to improve the dispersion of capsaicin through a modification reaction, and the anti-rodent coating is cured on the surface of the corrugated pipe to enhance the anti-rodent effect.
Significantly improves the dispersion of capsaicin in PP materials, improves the anti-rat gnawing performance of the corrugated pipe, makes its surface smooth and the anti-rat effect is stable and long-lasting.
Smart Images

Figure BDA0004937104550000051 
Figure BDA0004937104550000061 
Figure BDA0004937104550000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a PP corrugated pipe and a preparation method thereof. Background Art
[0002] In recent years, the automobile industry has developed greatly, and China's automobile wiring harness has also developed greatly. Polypropylene corrugated tubes are widely used in automobile wiring harnesses, mainly used for automobile wiring harnesses, providing wear resistance, damage prevention, heat insulation and other properties. However, the current corrugated protective sleeves do not have the function of anti-rodent damage. The wiring harnesses in the engine room and the body are often bitten off by rats, causing great safety hazards. Therefore, the development of polypropylene corrugated tubes with aging resistance and anti-rat bite functions for automobile wiring harnesses has a positive significance for improving the active safety performance of automobiles. The anti-rat effect of capsaicin is very obvious. Capsaicin is safe and non-toxic, but it is obviously irritating. After contact with the target rodents, it will form physical stimulation to it, resulting in strong skin irritation. Secondly, capsaicin will also hinder the synaptic nerve conduction, causing the mouse's sense of smell and taste to react, resulting in a highly nervous sense of fear, causing the mouse to flee in a hurry. However, when capsaicin is directly added to the PP material, the powder will easily agglomerate. The direct impact of poor dispersibility is that the surface of the corrugated tube is not smooth and has defects, and the anti-rat bite function is not obvious and not lasting. Studies have shown that after chemical modification of the capsaicin molecule, the loss of hydroxyl groups will cause the overall irritation of capsaicin to decrease, thereby reducing its effectiveness in preventing rat bites. Summary of the invention
[0003] The purpose of the present invention is to solve the problem that capsaicin is easy to agglomerate in PP material and has poor anti-rat bite performance, and to provide a PP corrugated pipe and a preparation method thereof.
[0004] In the first aspect, a PP corrugated pipe adopts the following technical solution:
[0005] A PP corrugated pipe, wherein the raw materials of the PP corrugated pipe include 76-97 parts of PP resin and 3-7 parts of hydrophilic modified capsaicin PP masterbatch in parts by weight;
[0006] The hydrophilic modified capsaicin PP masterbatch raw material includes, by weight, 0.1 to 2 parts of capsaicin, 0.5 to 5 parts of hydrophilic modified capsaicin, 89 to 99 parts of PP resin and 0.3 to 3 parts of dispersant;
[0007] The hydrophilic modified capsaicin comprises a copolymer of modified capsaicin and a hydrophilic monomer;
[0008] The modified capsaicin molecule contains a carbon-carbon double bond.
[0009] Furthermore, the PP corrugated pipe also includes a rodent-proof coating cured on the surface, and the raw materials of the rodent-proof coating include, by weight, 3 to 15 parts of peppermint oil, 3 to 15 parts of limonene, 25 to 35 parts of emulsifier, 5 to 10 parts of polyethylene glycol ester, 5 to 10 parts of polyoxyethylene ether and 15-59 parts of deionized water.
[0010] Furthermore, the PP corrugated pipe raw material further comprises 2 to 5 parts by weight of lipophilic modified capsaicin PP masterbatch;
[0011] The lipophilic modified capsaicin PP masterbatch raw material comprises, by weight, 0.5 to 5 parts of lipophilic modified capsaicin, 92 to 99 parts of PP resin and 0.3 to 3 parts of dispersant;
[0012] The lipophilic modified capsaicin comprises a copolymer of the modified capsaicin and a lipophilic monomer.
[0013] Furthermore, the PP corrugated pipe raw material further comprises 1 to 7 parts by weight of compound antioxidant PP masterbatch;
[0014] The compound antioxidant PP masterbatch raw material comprises, by weight, 1 to 3 parts of antioxidant 1010, 3 to 5 parts of antioxidant 168 and 92 to 96 parts of PP resin.
[0015] Furthermore, the hydrophilic monomer includes one or more of hydroxyethyl methacrylate, 4-hydroxybutyl acrylate, and 2,3-dihydroxypropyl acrylate.
[0016] Furthermore, the lipophilic monomer includes one or more of lauryl methacrylate and hexadecyl methacrylate.
[0017] Furthermore, the dispersant includes one or more of polypropylene wax and ethylene bisstearamide.
[0018] In the second aspect, a method for preparing a PP corrugated pipe adopts the following technical solution:
[0019] A method for preparing a PP corrugated pipe comprises the following steps:
[0020] Step 1, capsaicin is reacted with an acyl chloride reagent containing a carbon-carbon double bond to obtain the modified capsaicin;
[0021] Step 2, the modified capsaicin and the hydrophilic monomer undergo polymerization reaction under the action of an initiator and ultraviolet radiation to obtain the hydrophilic modified capsaicin;
[0022] Step 3, uniformly mixing the hydrophilic modified capsaicin, PP resin, capsaicin and dispersant, and melt granulating to obtain the hydrophilic modified capsaicin PP masterbatch;
[0023] Step 4, uniformly mixing the hydrophilic modified capsaicin PP masterbatch and PP resin, and melt-extruded to obtain the PP corrugated pipe.
[0024] Furthermore, the raw materials in step 4 also include lipophilic modified capsaicin PP masterbatch; the preparation method of the lipophilic modified capsaicin PP masterbatch comprises the following steps:
[0025] The modified capsaicin and the lipophilic monomer undergo a polymerization reaction under the action of an initiator and ultraviolet radiation to obtain the lipophilic modified capsaicin;
[0026] The lipophilic modified capsaicin, PP resin and dispersant are uniformly mixed, melt-granulated, and the lipophilic modified capsaicin PP masterbatch is obtained.
[0027] Furthermore, the raw materials in step 4 also include compound antioxidant PP masterbatch; the preparation method of the compound antioxidant PP masterbatch includes the following steps:
[0028] The antioxidant 1010, the antioxidant 168 and the PP resin are uniformly mixed, melt-granulated, and the compound antioxidant PP masterbatch is obtained.
[0029] Furthermore, the method further comprises step 5, wherein the PP corrugated pipe obtained in step 4 is impregnated with a rodent-proof coating, and then dried and cured.
[0030] Beneficial effects of the present invention:
[0031] The present invention provides a PP corrugated pipe, wherein the modified capsaicin molecule contains a carbon-carbon double bond and can undergo a polymerization reaction with a hydrophilic monomer to obtain a hydrophilic modified capsaicin, wherein the hydrophilic end of the hydrophilic modified capsaicin, such as a hydroxyl group, is bonded to the hydroxyl group of the capsaicin through a hydrogen bond, and the oily chain segment of the hydrophilic modified capsaicin infiltrates the PP resin, thereby improving the dispersibility of the capsaicin in the PP system. The addition of the hydrophilic modified capsaicin significantly improves the phenomenon that capsaicin is prone to agglomeration in the PP material, the dispersibility of the entire system is good, and the surface of the PP corrugated pipe is smooth and free of pitting. The hydrophilic modified capsaicin PP masterbatch is compounded with the PP resin, and since the hydrophilic modified capsaicin PP masterbatch contains capsaicin, it has a strong spicy irritation and has the effect of repelling and avoiding rodents, and the obtained PP corrugated pipe has the effect of preventing rodents from biting.
[0032] The present invention provides a PP corrugated pipe, wherein the rat-proof coating cured on the surface of the PP corrugated pipe has a pungent and cool smell, has strong penetration, and has a stimulating and repelling effect on rodents, causing the rodents to avoid or escape. The rat-proof coating and the capsaicin uniformly dispersed in the PP corrugated pipe synergistically prevent rodents from biting. The PP corrugated pipe is further used in protecting automobile wiring harnesses, and has stability and durability.
[0033] The present invention provides a PP corrugated pipe, wherein the lipophilic modified capsaicin PP masterbatch is prepared by free radical polymerization of modified capsaicin and a paraffin-based lipophilic monomer, thereby helping to enhance the overall dispersibility between capsaicin molecules and the dispersibility between capsaicin molecules and a matrix material.
[0034] The present invention provides a method for preparing a PP corrugated pipe, wherein the modified capsaicin is hydrophilic and lipophilic and is mixed with the capsaicin and PP resin for granulation, so that the dispersibility of the capsaicin in the PP material system is further improved, the surface of the prepared PP corrugated pipe is smooth, and the uniform dispersion of the capsaicin further prevents and controls rodents from gnawing. DETAILED DESCRIPTION
[0035] The following is a further detailed description of a PP corrugated pipe and a preparation method thereof described in the present invention in conjunction with an embodiment. For the sake of simplicity of description, this document cannot list all the alternative technical features and implementation schemes included in the present invention. Therefore, those skilled in the art should be aware that any technical features and implementation schemes in this embodiment do not limit the scope of protection of the present invention, which includes any alternative technical features and implementation schemes adopted by all those skilled in the art without creative labor. Specifically, the implementation schemes obtained by replacing any technical feature in the present invention or combining any two or more technical features provided by the present invention should be within the scope of protection of the present invention.
[0036] If no specific techniques and conditions are specified in the examples, the procedures are carried out according to the techniques and conditions described in the literature in the art or according to the product instructions. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0037] The modified capsaicin used in the following examples is capsaicin acrylate, which is prepared by the following steps:
[0038] This embodiment provides a method for preparing capsaicin acrylate, comprising the following steps:
[0039] Place a three-necked flask in an ice-water bath, maintain the temperature at 1°C-4°C, add capsaicin, catalyst and solvent to the flask in turn, place it in an ice-water bath, stir, stir at a speed of 150rpm-430rpm, pH of 8.0-10.0, and when the temperature is maintained in the temperature range of 1-4°C, dissolve acryloyl chloride in a certain amount of solvent and add it dropwise to the three-necked flask. After the addition is completed, heat to room temperature and keep stirring for 3h-6h before stopping the reaction, and the solvent is re-evaporated to remove water. The three-necked flask is equipped with a drying tube. After filtering the reaction mixture, use a saturated NaHCO3 solution to wash and remove hydrochloric acid, and rinse repeatedly with deionized water, place it in a 103°C oven and dry it for 5h-8h, then purify it through a column, and remove the solvent by rotary evaporation for 12h-24h to obtain capsaicin acrylate.
[0040] In some embodiments, the catalyst includes one or more of 4-dimethylaminopyridine (DMAP), pyridine, triethylamine (TEA), N-hydroxysuccinimide (NHS), tributylamine, N,N-diisopropylethylamine (DIPPA); the solvent includes one or more of dichloromethane, chloroform, toluene, THF.
[0041] Example
[0042] Example 1
[0043] Example 1 provides a PP corrugated pipe, wherein the raw material of the PP corrugated pipe includes 76g of PP resin and 3g of hydrophilic modified capsaicin PP masterbatch;
[0044] The raw materials of hydrophilic modified capsaicin PP masterbatch include 0.1g capsaicin, 0.5g hydrophilic modified capsaicin, 89g PP resin and 0.3g ethylene bis stearic acid amide;
[0045] The hydrophilic modified capsaicin is a copolymer of modified capsaicin and hydroxyethyl methacrylate.
[0046] Example 1 provides a method for preparing modified capsaicin, and the chemical reaction formula is as follows:
[0047]
[0048] The specific steps include:
[0049] The solvent was redissolved to remove water, and a three-necked flask was installed with a drying tube and placed in an ice-water bath. 60 g of capsaicin, 50 mL of TEA and 150 mL of dichloromethane were added to the flask in sequence and stirred for 0.5 h at a rotation speed of 250 rpm and a pH of 8.2. When the temperature was maintained at 1°C, 25 mL of acryloyl chloride was dissolved in 50 mL of the solvent and added dropwise to the three-necked flask. After the addition was completed, the temperature was raised to room temperature and stirred for 3 h before stopping the reaction. The reaction mixture was filtered, washed with a saturated NaHCO3 solution to remove hydrochloric acid and rinsed repeatedly with deionized water for 0.5 h. After drying in an oven at 103°C for 8 h, it was purified by column and the solvent was removed by rotary evaporation for 18 h to obtain capsaicin acrylate.
[0050] Example 1 provides a method for preparing hydrophilic modified capsaicin, and the chemical reaction formula is as follows:
[0051]
[0052] The following steps are involved:
[0053] 25 g of the prepared modified capsaicin (capsaicin acrylate) and 32 mL of hydroxyethyl methacrylate were dissolved in 130 mL of TFEA, respectively. After magnetic stirring for 30 min, they were transferred into a three-necked flask and stirred at a speed of 200 rpm. A condenser was installed in the three-necked flask, and a UV LED lamp (wavelength of 320 nm) was fixed at the bottom of the three-necked flask. The irradiation distance of the light source from the bottom of the flask was 2 cm. 2 mL of 2,2-diethoxyacetophenone initiator was dissolved in 4 mL of TFEA solution and added dropwise to the three-necked flask with the help of a peristaltic pump. The addition speed was 200 μL / min. After the dripping was completed, the ultraviolet lamp was irradiated for 1 h. After adding 100 μL of photoinitiator, the ultraviolet light was continued for 0.5 h and then the irradiation was stopped. The reaction was terminated and filtered and dried to obtain hydrophilic modified capsaicin.
[0054] Example 1 provides a method for preparing a hydrophilic modified capsaicin PP masterbatch, comprising the following steps:
[0055] Capsaicin, hydrophilic modified capsaicin and PP resin are mixed, ethylene bis stearamide is added and mixed evenly at high speed, melt extrusion granulation is performed by a twin-screw extruder, and drying is performed to obtain hydrophilic modified capsaicin PP masterbatch.
[0056] Embodiment 1 provides a method for preparing a PP corrugated pipe, comprising the following steps:
[0057] The PP resin and hydrophilic modified capsaicin PP masterbatch were evenly mixed and put into the single-screw corrugated pipe forming unit. The temperatures of the eight zones of the screw extruder were set to 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C, and 195°C, the main engine speed was 330rpm, the feeding speed was 25-35rpm, and extrusion and cooling were performed to obtain a PP corrugated pipe.
[0058] Example 2
[0059] Embodiment 2 provides a PP corrugated pipe, wherein the raw material of the PP corrugated pipe includes 97g PP resin and 7g hydrophilic modified capsaicin PP masterbatch;
[0060] The raw materials of hydrophilic modified capsaicin PP masterbatch include 2g capsaicin, 5g hydrophilic modified capsaicin, 99g PP resin and 3g ethylene bis stearic acid amide;
[0061] The hydrophilic modified capsaicin is a copolymer of modified capsaicin and hydroxyethyl methacrylate.
[0062] The preparation method of modified capsaicin, the preparation method of hydrophilic modified capsaicin, the preparation method of hydrophilic modified capsaicin PP masterbatch, and the preparation method of PP corrugated pipe provided in Example 2 are the same as those in Example 1.
[0063] Example 3
[0064] Example 3 provides a PP corrugated pipe, wherein the raw material of the PP corrugated pipe includes 86g of PP resin and 5g of hydrophilic modified capsaicin PP masterbatch;
[0065] The raw materials of hydrophilic modified capsaicin PP masterbatch include 1g capsaicin, 2.5g hydrophilic modified capsaicin, 95g PP resin and 1.5g ethylene bis stearic acid amide;
[0066] The hydrophilic modified capsaicin is a copolymer of modified capsaicin and hydroxyethyl methacrylate.
[0067] The preparation method of modified capsaicin, the preparation method of hydrophilic modified capsaicin, the preparation method of hydrophilic modified capsaicin PP masterbatch, and the preparation method of PP corrugated pipe provided in Example 3 are the same as those in Example 1.
[0068] Example 4
[0069] Embodiment 4 provides a PP corrugated tube, which is different from Embodiment 3 in that the raw material of the PP corrugated tube further includes 2g of lipophilic modified capsaicin PP masterbatch;
[0070] The raw materials of lipophilic modified capsaicin PP masterbatch include 0.5g lipophilic modified capsaicin, 92g PP resin and 0.3g ethylene bis stearic acid amide;
[0071] The lipophilic modified capsaicin includes a copolymer of modified capsaicin and lauryl methacrylate.
[0072] Example 4 provides a method for preparing lipophilic modified capsaicin, and the chemical reaction formula is as follows:
[0073]
[0074] The following steps are involved:
[0075] 20 g of modified capsaicin (capsaicin acrylate) and 53 mL of lauryl methacrylate were dissolved in 160 mL of TFEA respectively, and after magnetic stirring for 30 min, they were transferred into a three-necked flask for stirring at a speed of 200 rpm. A condenser was installed in the three-necked flask, and a UV LED lamp (wavelength of 320 nm) was fixed at the bottom of the three-necked flask. The irradiation distance from the light source to the bottom of the flask was 2 cm. 2 mL of 2,2-diethoxyacetophenone initiator was dissolved in 4 mL of TFEA solution and added dropwise to the three-necked flask with the help of a peristaltic pump at a dropping speed of 200 μL / min. After the dropwise addition, the solution was irradiated with a UV lamp for 1 h. After adding 100 μL of photoinitiator, the solution was irradiated with UV light for 0.5 h and then stopped. The reaction was terminated, filtered and dried to obtain lipophilic modified capsaicin.
[0076] Example 4 provides a method for preparing a lipophilic modified capsaicin PP masterbatch, comprising the following steps:
[0077] The lipophilic modified capsaicin is mixed with PP resin, ethylene bisstearamide is added and mixed at high speed, melt-extruded and granulated by a twin-screw extruder, and dried to obtain the lipophilic modified capsaicin PP masterbatch.
[0078] The preparation method of modified capsaicin, the preparation method of hydrophilic modified capsaicin, and the preparation method of hydrophilic modified capsaicin PP masterbatch provided in Example 4 are the same as those in Example 3.
[0079] Embodiment 4 provides a method for preparing a PP corrugated pipe, comprising the following steps:
[0080] The PP resin, hydrophilic modified capsaicin PP masterbatch and lipophilic modified capsaicin PP masterbatch are evenly mixed and put into the single-screw corrugated pipe forming unit. The temperatures of the eight zones of the screw extruder are set to 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C and 195°C, the main engine speed is 330rpm, the feeding speed is 25-35rpm, extrusion and cooling are performed to obtain a PP corrugated pipe.
[0081] Example 5
[0082] Example 5 provides a PP corrugated tube which is different from Example 4 in that the raw material of the PP corrugated tube includes 5g of lipophilic modified capsaicin PP masterbatch;
[0083] The raw materials of lipophilic modified capsaicin PP masterbatch include 5g lipophilic modified capsaicin, 99g PP resin and 3g ethylene bisstearic acid amide.
[0084] The preparation method of lipophilic modified capsaicin, the preparation method of lipophilic modified capsaicin PP masterbatch, the preparation method of modified capsaicin, the preparation method of hydrophilic modified capsaicin, the preparation method of hydrophilic modified capsaicin PP masterbatch, and the preparation method of PP corrugated pipe provided in Example 5 are the same as those in Example 4.
[0085] Example 6
[0086] Example 6 provides a PP corrugated tube which is different from Example 4 in that the raw material of the PP corrugated tube includes 3g of lipophilic modified capsaicin PP masterbatch;
[0087] The raw materials of lipophilic modified capsaicin PP masterbatch include 2.5g lipophilic modified capsaicin, 95g PP resin and 1.5g ethylene bisstearic acid amide.
[0088] The preparation method of lipophilic modified capsaicin, the preparation method of lipophilic modified capsaicin PP masterbatch, the preparation method of modified capsaicin, the preparation method of hydrophilic modified capsaicin, the preparation method of hydrophilic modified capsaicin PP masterbatch, and the preparation method of PP corrugated pipe provided in Example 6 are the same as those in Example 4.
[0089] Example 7
[0090] Embodiment 7 provides a PP corrugated pipe which is different from Embodiment 6 in that the raw material of the PP corrugated pipe further includes 1g of compound antioxidant PP masterbatch;
[0091] The raw materials of compound antioxidant PP masterbatch include 1g antioxidant 1010, 3g antioxidant 168 and 92g PP resin.
[0092] Embodiment 7 provides a method for preparing a composite antioxidant PP masterbatch, comprising the following steps:
[0093] The antioxidant 1010, antioxidant 168 and PP resin are mixed evenly, melt-extruded and granulated by a twin-screw extruder, and dried to obtain a compound antioxidant PP masterbatch.
[0094] Example 7 provides a method for preparing lipophilic modified capsaicin, a method for preparing lipophilic modified capsaicin PP masterbatch, a method for preparing modified capsaicin, a method for preparing hydrophilic modified capsaicin, and a method for preparing hydrophilic modified capsaicin PP masterbatch, which are the same as Example 6.
[0095] Embodiment 7 provides a method for preparing a PP corrugated pipe, comprising the following steps:
[0096] The PP resin, hydrophilic modified capsaicin PP masterbatch, lipophilic modified capsaicin PP masterbatch and compound antioxidant PP masterbatch are mixed evenly and put into the single-screw corrugated pipe forming unit. The temperatures of the eight zones of the screw extruder are set to 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C and 195°C, the main engine speed is 330rpm, the feeding speed is 25-35rpm, extrusion and cooling are performed to obtain a PP corrugated pipe.
[0097] Example 8
[0098] Embodiment 8 provides a PP corrugated pipe which is different from Embodiment 7 in that the raw material of the PP corrugated pipe further includes 7g of compound antioxidant PP masterbatch;
[0099] The raw materials of the compound antioxidant PP masterbatch include 3g antioxidant 1010, 5g antioxidant 168 and 96g PP resin.
[0100] The preparation method of the compound antioxidant PP masterbatch, the preparation method of the lipophilic modified capsaicin, the preparation method of the lipophilic modified capsaicin PP masterbatch, the preparation method of the modified capsaicin, the preparation method of the hydrophilic modified capsaicin, the preparation method of the hydrophilic modified capsaicin PP masterbatch, and the preparation method of the PP corrugated pipe provided in Example 8 are the same as those in Example 7.
[0101] Example 9
[0102] Embodiment 9 provides a PP corrugated pipe which is different from Embodiment 7 in that the raw material of the PP corrugated pipe further includes 4g of compound antioxidant PP masterbatch;
[0103] The raw materials of the compound antioxidant PP masterbatch include 2g antioxidant 1010, 4g antioxidant 168 and 94g PP resin.
[0104] The preparation method of the compound antioxidant PP masterbatch, the preparation method of the lipophilic modified capsaicin, the preparation method of the lipophilic modified capsaicin PP masterbatch, the preparation method of the modified capsaicin, the preparation method of the hydrophilic modified capsaicin, the preparation method of the hydrophilic modified capsaicin PP masterbatch, and the preparation method of the PP corrugated pipe provided in Example 9 are the same as those in Example 7.
[0105] Example 10
[0106] Embodiment 10 provides a PP corrugated pipe which is different from Embodiment 9 in that the PP corrugated pipe further includes a rodent-proof coating cured on the surface;
[0107] The raw materials of the rodent-proof paint include 10g of peppermint oil, 10g of limonene, 30g of an emulsifier, preferably fatty acid polyester, 10g of polyethylene glycol ester, 10g of polyoxyethylene ether and 30g of deionized water.
[0108] The preparation method of the compound antioxidant PP masterbatch, the preparation method of the lipophilic modified capsaicin, the preparation method of the lipophilic modified capsaicin PP masterbatch, the preparation method of the modified capsaicin, the preparation method of the hydrophilic modified capsaicin, and the preparation method of the hydrophilic modified capsaicin PP masterbatch provided in Example 10 are the same as those in Example 9.
[0109] Embodiment 10 provides a method for preparing a PP corrugated pipe, comprising the following steps:
[0110] PP resin, hydrophilic modified capsaicin PP masterbatch, lipophilic modified capsaicin PP masterbatch and compound antioxidant PP masterbatch are mixed evenly and put into a single screw corrugated pipe forming unit, and the temperatures of the eight zones of the screw extruder are set to 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C and 195°C, the main engine speed is 330rpm, the feeding speed is 25-35rpm, extrusion is performed, cooling is performed, and a PP corrugated pipe is obtained;
[0111] The PP corrugated pipe is passed through a rodent-proof coating tank and a circulating bellows in sequence, the temperature of the circulating bellows is 75° C., and dried and solidified to obtain the product.
[0112] Comparative Example
[0113] Comparative Example 1
[0114] Comparative Example 1 provides a PP corrugated tube, which is different from Example 10 in that the lipophilic modified capsaicin PP masterbatch is replaced by an equal amount of hydrophilic modified capsaicin PP masterbatch, that is, the amount of hydrophilic modified capsaicin PP masterbatch is 8 g.
[0115] The preparation method of the compound antioxidant PP masterbatch, the preparation method of modified capsaicin, the preparation method of hydrophilic modified capsaicin, and the preparation method of hydrophilic modified capsaicin PP masterbatch provided in Comparative Example 1 are all the same as those in Example 10.
[0116] Comparative Example 1 provides a method for preparing a PP corrugated pipe, comprising the following steps:
[0117] PP resin, hydrophilic modified capsaicin PP masterbatch and compound antioxidant PP masterbatch are mixed evenly and put into a single screw corrugated pipe forming unit, and the temperatures of the eight zones of the screw extruder are set to 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C and 195°C, the main engine speed is 330rpm, the feeding speed is 25-35rpm, extrusion is performed, and cooling is performed to obtain a PP corrugated pipe;
[0118] The PP corrugated pipe is passed through a rodent-proof coating tank and a circulating bellows in sequence, the temperature of the circulating bellows is 75° C., and dried and solidified to obtain the product.
[0119] Comparative Example 2
[0120] Comparative Example 2 provides a PP corrugated tube, which is different from Example 10 in that the hydrophilic modified capsaicin PP masterbatch is replaced by an equal amount of lipophilic modified capsaicin PP masterbatch, that is, the amount of lipophilic modified capsaicin PP masterbatch is 8 g.
[0121] The preparation method of the compound antioxidant PP masterbatch, the preparation method of the lipophilic modified capsaicin, and the preparation method of the modified capsaicin provided in Comparative Example 2 are the same as those in Example 10.
[0122] Comparative Example 2 provides a method for preparing a PP corrugated pipe, comprising the following steps:
[0123] PP resin, lipophilic modified capsaicin PP masterbatch and compound antioxidant PP masterbatch are mixed evenly and put into a single screw corrugated pipe forming unit, and the temperatures of the eight zones of the screw extruder are set to 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C and 195°C, the main engine speed is 330rpm, the feeding speed is 25-35rpm, extrusion is performed, and cooling is performed to obtain a PP corrugated pipe;
[0124] The PP corrugated pipe is passed through a rodent-proof coating tank and a circulating bellows in sequence, the temperature of the circulating bellows is 75° C., and dried and solidified to obtain the product.
[0125] Comparative Example 3
[0126] Comparative Example 3 provides a PP corrugated pipe which is different from Example 10 in that the raw materials of the PP corrugated pipe are different, as follows:
[0127] The raw materials of PP corrugated pipe include 4g compound antioxidant PP masterbatch, 86g PP resin, and 8g capsaicin PP masterbatch;
[0128] The raw materials of capsaicin PP masterbatch include 1g capsaicin, 95g PP resin and 1.5g ethylene bisstearamide.
[0129] Comparative Example 3 provides a method for preparing capsaicin PP masterbatch, comprising the following steps:
[0130] The capsaicin, ethylene bisstearic acid amide and PP resin are uniformly mixed, melt-extruded and granulated by a twin-screw extruder, and dried to obtain the capsaicin PP masterbatch.
[0131] Comparative Example 3 provides a method for preparing a PP corrugated pipe, comprising the following steps:
[0132] PP resin, capsaicin PP masterbatch and compound antioxidant PP masterbatch are mixed evenly and put into the single screw corrugated pipe forming unit, and the temperatures of the eight zones of the screw extruder are set to 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C and 195°C, the main engine speed is 330rpm, the feeding speed is 25-35rpm, extrusion is performed, and cooling is performed to obtain a PP corrugated pipe;
[0133] The PP corrugated pipe is passed through a rodent-proof coating tank and a circulating bellows in sequence, the temperature of the circulating bellows is 75° C., and dried and solidified to obtain the product.
[0134] Comparative Example 4
[0135] Comparative Example 4 provides a PP corrugated pipe which is different from Example 10 in that the raw materials of the PP corrugated pipe are different, as follows:
[0136] The raw materials of PP corrugated pipe include 4g compound antioxidant PP masterbatch, 94g PP resin and 3g ethylene bisstearamide.
[0137] Comparative Example 4 provides a method for preparing a PP corrugated pipe, comprising the following steps:
[0138] PP resin, ethylene bis stearamide and compound antioxidant PP masterbatch are mixed evenly and put into a single screw corrugated pipe forming unit, and the temperatures of the eight zones of the screw extruder are set to 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C, and 195°C, the main engine speed is 330rpm, the feeding speed is 25-35rpm, extrusion is performed, and cooling is performed to obtain a PP corrugated pipe;
[0139] The PP corrugated pipe is passed through a rodent-proof coating tank and a circulating bellows in sequence, the temperature of the circulating bellows is 75° C., and dried and solidified to obtain the product.
[0140] Performance Testing
[0141] The PP corrugated pipes provided in Examples 1-10 and Comparative Examples 1-4 were subjected to a tensile property test in accordance with GB / T 1040.2-2006. The surface appearance of the PP corrugated pipes provided in each Example and Comparative Example was observed to determine whether they were smooth, whether there were obvious pits, and the number of pits per unit length. The test results are shown in Table 1.
[0142] Table 1 Appearance and performance test results of PP corrugated pipes provided by Examples 1-10 and Comparative Examples 1-4
[0143]
[0144] As shown in Table 1, the tensile properties of each test case are not much different, but the appearance of the corrugated tube is obviously different. Compared with the system with only capsaicin, the addition of hydrophilic modified capsaicin PP masterbatch and lipophilic modified capsaicin PP masterbatch can significantly improve the dispersibility of the corrugated protective tube, and the surface of the obtained corrugated protective tube is smooth without obvious pitting.
[0145] The PP corrugated pipes prepared in Examples 1-10 and Comparative Examples 1-4 were subjected to a rat-proof test, and the experimental results were compared. The test was based on GB / T 34016-2017 "General Rules for Rat-proof and Ant-proof Wires and Cables" and JB / T 10696.10-2011 "Test Methods for Mechanical and Physical and Chemical Properties of Wires and Cables Part 10: Rat Bite Test". Two PP corrugated protective sleeves were taken from each of the above cases, and placed in an open box space with mice for 14 days. The surface of the corrugated protective sleeves was observed, and the rat bite conditions were recorded. The details are shown in Table 2.
[0146] Table 2 Rat-proof performance of PP corrugated pipes provided in Examples 1-10 and Comparative Examples 1-4
[0147]
[0148] As shown in Table 2, the smell of rat-proof coating is pungent and cool, with strong penetration, which has a stimulating and repelling effect on rodents. On the basis of adding capsaicin modified masterbatch, the rat-proof coating has less rat bite marks on the surface of the corrugated pipe compared with the corrugated pipe without rat-proof coating. This shows that the rat-proof coating has the effect of making rodents avoid or escape to a certain extent.
[0149] The experiment shows that the overall performance of anti-rat bite performance is more positively correlated with the proportion of capsaicin active ingredients. However, the anti-rat bite effect of the corrugated pipe with only pure capsaicin is far inferior to that of the corrugated pipe with hydrophilic modified capsaicin PP masterbatch and lipophilic modified capsaicin PP masterbatch, which shows that the presence of hydrophilic modified capsaicin PP masterbatch and lipophilic modified capsaicin PP masterbatch can significantly improve the distribution of capsaicin in PP and the dispersion of capsaicin molecules. The improvement of the overall dispersion of the corrugated protective sleeve is conducive to the balance and durability of the anti-rat bite effect.
[0150] For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived from them are still within the scope of protection of the claims of the invention.
Claims
1. A PP corrugated pipe, characterized in that: The raw material of the PP corrugated pipe comprises, by weight, 76 to 97 parts of PP resin and 3 to 7 parts of hydrophilic modified capsaicin PP masterbatch; The hydrophilic modified capsaicin PP masterbatch raw material includes, by weight, 0.1 to 2 parts of capsaicin, 0.5 to 5 parts of hydrophilic modified capsaicin, 89 to 99 parts of PP resin and 0.3 to 3 parts of dispersant; The hydrophilic modified capsaicin comprises a copolymer of modified capsaicin and a hydrophilic monomer; The modified capsaicin molecule contains a carbon-carbon double bond.
2. A PP corrugated pipe according to claim 1, characterized in that: The PP corrugated pipe also includes a rodent-proof coating cured on the surface. The raw materials of the rodent-proof coating include, by weight, 3 to 15 parts of peppermint oil, 3 to 15 parts of limonene, 25 to 35 parts of emulsifier, 5 to 10 parts of polyethylene glycol ester, 5 to 10 parts of polyoxyethylene ether and 15-59 parts of deionized water.
3. A PP corrugated pipe according to claim 1, characterized in that: The PP corrugated pipe raw material also includes 2 to 5 parts of lipophilic modified capsaicin PP masterbatch in parts by weight; The lipophilic modified capsaicin PP masterbatch raw material comprises, by weight, 0.5 to 5 parts of lipophilic modified capsaicin, 92 to 99 parts of PP resin and 0.3 to 3 parts of dispersant; The lipophilic modified capsaicin comprises a copolymer of the modified capsaicin and a lipophilic monomer.
4. A PP corrugated pipe according to claim 1, characterized in that: The PP corrugated pipe raw material also includes 1 to 7 parts of compound antioxidant PP masterbatch in parts by weight; The compound antioxidant PP masterbatch raw material comprises, by weight, 1 to 3 parts of antioxidant 1010, 3 to 5 parts of antioxidant 168 and 92 to 96 parts of PP resin.
5. A PP corrugated pipe according to claim 1, characterized in that: The hydrophilic monomer includes one or more of hydroxyethyl methacrylate, 4-hydroxybutyl acrylate, and 2,3-dihydroxypropyl acrylate.
6. A PP corrugated pipe according to claim 3, characterized in that: The lipophilic monomer includes one or more of lauryl methacrylate and hexadecyl methacrylate.
7. A method for preparing a PP corrugated pipe according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1, capsaicin is reacted with an acyl chloride reagent containing a carbon-carbon double bond to obtain the modified capsaicin; Step 2, the modified capsaicin and the hydrophilic monomer undergo polymerization reaction under the action of an initiator and ultraviolet radiation to obtain the hydrophilic modified capsaicin; Step 3, uniformly mixing the hydrophilic modified capsaicin, PP resin, capsaicin and dispersant, and melt granulating to obtain the hydrophilic modified capsaicin PP masterbatch; Step 4, uniformly mixing the hydrophilic modified capsaicin PP masterbatch and PP resin, and melt-extruded to obtain the PP corrugated pipe.
8. The method for preparing a PP corrugated pipe according to claim 7, characterized in that: Step 4: The raw materials also include lipophilic modified capsaicin PP masterbatch; the preparation method of the lipophilic modified capsaicin PP masterbatch comprises the following steps: The modified capsaicin and the lipophilic monomer undergo a polymerization reaction under the action of an initiator and ultraviolet radiation to obtain the lipophilic modified capsaicin; The lipophilic modified capsaicin, PP resin and dispersant are uniformly mixed, melt-granulated, and the lipophilic modified capsaicin PP masterbatch is obtained.
9. The method for preparing a PP corrugated pipe according to claim 8, characterized in that: Step 4: The raw materials also include compound antioxidant PP masterbatch; the preparation method of the compound antioxidant PP masterbatch includes the following steps: The antioxidant 1010, the antioxidant 168 and the PP resin are uniformly mixed, melt-granulated, and the compound antioxidant PP masterbatch is obtained.
10. The method for preparing a PP corrugated pipe according to claim 9, characterized in that: The method further comprises step 5, wherein the PP corrugated pipe obtained in step 4 is impregnated with a rodent-proof coating, and then dried and cured.