Film-coated thermal insulation bag and manufacturing method thereof

Through improved printing and coating processes and modified PBAT materials, the problem of insolid bonding of aluminum-plated materials in fast-moving consumer goods insulation bags is solved, achieving higher insulation effect and environmental protection, avoiding health and environmental risks.

CN118812953BActive Publication Date: 2024-11-22SICHUAN KAIPU ECO-FRIENDLY PACKING PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411295884.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-22
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

In the existing fast-moving consumer goods insulation bags, the aluminum-plated material and non-woven fabric are not firmly combined, resulting in layering and bubbles, insufficient adhesion of the aluminum-plated layer, potential health and environmental risks, and the aluminum film material recycling and processing is complicated. .

Method used

Using improved printing and coating processes, the printing layer, non-woven fabric and insulation layer are combined through laminate positioning, and modified PBAT materials are used to enhance the adhesion of the coating, improve insulation effect and durability, and reduce recycling and processing costs.

Benefits of technology

Achieve stronger coating adhesion, avoid bubbles and layering, improve product durability and reliability, and provide environmentally friendly and economical insulation solutions, reducing the potential of aluminum layer to the human body and the environment. harm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812953B_ABST
    Figure CN118812953B_ABST
Patent Text Reader

Abstract

The present invention discloses a film-coated insulation bag and a method for making the same, which belongs to the technical field of layered materials and aims to solve the problems of delamination, blistering, aluminum layer shedding and environmental pollution encountered in the production and use of existing fast-moving consumer goods insulation bags. The present invention adopts printing and laminating technology to replace the traditional aluminum-plated film structure with a film-coated film, which not only achieves the insulation effect, but also forms an environmentally friendly material that is easy to recycle and reuse. In the production process, by optimizing the ink formula and the combination of laminating materials, especially the ratio of polypropylene and masterbatch, the production process is simplified, the adhesion of the film is enhanced, and blistering and delamination phenomena are effectively prevented, while the waterproof, moisture-proof, wear-resistant and chemical corrosion-resistant properties of the product are improved. Compared with the prior art, the film-coated insulation bag of the present invention has superior performance in chemical corrosion resistance and wear resistance, meeting the market demand for environmentally friendly, high-performance insulation bags.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of layered materials, and in particular to a film-coated thermal insulation bag and a manufacturing method thereof. Background Art

[0002] With the acceleration of the pace of modern life, the demand for thermal insulation packaging of fast-moving consumer goods is growing. At present, the thermal insulation bags of fast-moving consumer goods widely used in the market mostly use aluminum-plated materials to achieve the thermal insulation effect. This material is coated with a layer of aluminum film on non-woven fabrics or other substrates, and uses the reflective properties of aluminum to reduce heat loss and achieve the purpose of thermal insulation. Although it has certain advantages in thermal insulation performance, aluminum-plated materials have many limitations in actual production and use. The main problems include: insufficient bonding firmness. The bonding between the aluminum layer and the non-woven fabric is often not strong enough, and it is easy to delaminate and blister, which not only affects the appearance of the product, but also reduces the durability of the thermal insulation effect. Adhesion problem. The adhesion of the aluminum layer after corona treatment is insufficient, which may cause the aluminum layer powder to fall off during use, affecting the overall performance and service life of the product. Potential health risks. The aluminum layer as a metal may cause potential harm to human health, especially when packaging food. The safety of the aluminum layer needs to be strictly considered. Environmental impact. The recycling and processing of aluminum film materials is relatively complicated and not easy to degrade, which burdens the environment and increases the cost of waste disposal.

[0003] In the prior art, China's invention patent CN107139555B discloses a layered material for food insulation bags and its application. The layered material includes: an ultra-thin aluminum foil layer, a longitudinal film layer, a polyurethane foam layer and a water-blocking film layer in sequence. The longitudinal bubbles are evenly distributed in the longitudinal film layer, and the proportion of through bubbles in the bubbles is less than 3%. The polyurethane foam layer is prepared by ultra-soft polyurethane foaming. The specifically selected composition group obtains a layered material for food insulation bags with excellent insulation effect, durable material, and reusable. Although the invention provides excellent insulation effect and durability, the aluminum foil layer may fall off under certain conditions, which may pose a potential risk to food safety.

[0004] China's invention patent CN111234396B discloses a functional insulation bag and a preparation method thereof, wherein the insulation bag comprises a sandwich bag body and a filler filled in the sandwich of the sandwich bag body, wherein the sandwich bag body comprises the following raw materials in parts by weight: butyl rubber, polyisobutylene, nano calcium carbonate powder, phenolic resin, ultrafine aluminum hydroxide, silicon carbide whisker, plasticizer and antioxidant; the filler comprises the following raw materials in parts by weight: polyurethane resin, chitosan, sodium bisulfite, far infrared nano powder, nano silver powder, calcium powder, porous carbon microspheres. The functional insulation bag of the invention selects the appropriate ratio by selecting the raw material composition and optimizing the content of each raw material, which not only gives full play to the advantages of each raw material, but also complements and promotes each other. The obtained functional insulation bag has excellent toughness and high temperature resistance, and has excellent insulation performance. Although it has excellent insulation and high temperature resistance, the material cost is high, and the complex raw material composition may increase the difficulty and complexity of the manufacturing process. Summary of the invention

[0005] Aiming at the deficiencies of the existing technology, the invention aims to solve a series of problems encountered in the production of existing fast-moving consumer goods insulation bags, including delamination and blistering caused by the weak bonding between the aluminum-plated material and the non-woven fabric, the shedding caused by insufficient adhesion of the aluminum-plated layer, the potential harm of aluminum layer powder to human health and the environment, and the complexity of the recycling and processing of aluminum film materials. By improving the printing and laminating process, the invention not only improves the insulation effect and durability of the product, but also realizes the singleness of environmentally friendly materials, reduces the cost of product recycling and processing, improves production efficiency, and effectively prevents blistering and delamination during the use of the product by enhancing the adhesion of the film, providing the market with a solution for insulation bags that is both economical and practical and environmentally sustainable.

[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0007] A method for making a film-coated thermal insulation bag is as follows:

[0008] Material stacking and positioning: First, the printing layer, non-woven fabric and insulation layer are stacked from top to bottom to form the basic structure of the insulation bag through the laminating process;

[0009] The method for making the printed layer is as follows:

[0010] Step 1, ink formulation: In the preparation stage, pearlescent ink, color ink and connector are mixed, and through color display and measurement, they are continuously adjusted to obtain the ideal visual effect, and then adjusted to large-scale printing ink according to the sample formula;

[0011] Step 2: Equipment pre-inspection: Before starting the machine, conduct a comprehensive inspection of the pressurization, transmission, cooling, exhaust and ink absorption systems to ensure that they function normally;

[0012] Step 3: Plate assembly and fine-tuning: According to the design drawing, proofread and assemble the printing plate, and adjust the gap and angle between the doctor blade and the plate roller;

[0013] Step 4: Ink preparation: Pour the prepared ink into the ink tray and adjust its viscosity;

[0014] Step 5: Color calibration and test printing: After performing longitudinal and transverse color calibration, start test printing;

[0015] Step 6, quality inspection: Conduct detailed quality inspection on the printed product, including dot integrity, overprint accuracy and pattern clarity. Also check whether there are any cuts or dirty spots on the layout, and inspect the color. If necessary, make fine adjustments.

[0016] Step 7: Batch printing: After confirming that the quality meets the standards, start batch printing.

[0017] In the step 1, the mass ratio of pearlescent ink, color ink and connector is 0.5-2:0.5-2:15-19; the connector in the step 1 is composed of butyl acetate, ethyl acetate and n-propyl acetate in a mass ratio of 1-3:3-5:2-4.

[0018] In step 3, the distance between the scraper and the plate roller is 30-50 μm, and the angle is 40-50°.

[0019] In step 4, the ink viscosity is adjusted to 15-25 seconds (measured using a No. 4 Zahn cup).

[0020] The coating process is as follows:

[0021] S1. Material mixing: put polypropylene, masterbatch and polyethylene into a stirring device, wherein the mass ratio of polypropylene, masterbatch and polyethylene is 40-60:20-40:0.5-2; set the stirring speed, temperature and time to ensure uniform mixing;

[0022] S2. Material heating and melting: Pour the mixed material into the funnel of the laminating equipment, and heat and melt it through the temperature control of the screw, cylinder and film head;

[0023] S3, Uniform connection of cast layer: After the film mouth is extruded, the cast layer is evenly connected between the non-woven fabric and the printing layer, and between the non-woven fabric and the insulation layer by roller pressing, and the flow rate is controlled to meet the product process requirements;

[0024] S4. Product cooling: The product is quickly cooled and solidified through a circulating water cooling system.

[0025] Preferably, the coating process is as follows:

[0026] S1. Material mixing: put polypropylene, masterbatch, polyethylene and modified PBAT material into a stirring device, wherein the mass ratio of polypropylene, masterbatch, polyethylene and modified PBAT material is 40-60:20-40:0.5-2:1-3; set the stirring speed, temperature and time to ensure uniform mixing;

[0027] S2. Material heating and melting: Pour the mixed material into the funnel of the laminating equipment, and heat and melt it through the temperature control of the screw, cylinder and film head;

[0028] S3, Uniform connection of cast layer: After the film mouth is extruded, the cast layer is evenly connected between the non-woven fabric and the printing layer, and between the non-woven fabric and the insulation layer by roller pressing, and the flow rate is controlled to meet the product process requirements;

[0029] S4. Product cooling: The product is quickly cooled and solidified through a circulating water cooling system.

[0030] In the step S1, the stirring speed is set to 100-300 rpm, the temperature is set to 110-130° C., and the time is set to 10-30 minutes.

[0031] In step S2, the temperatures of the screw are 210-230°C, 230-250°C, and 250-270°C, respectively; the temperatures of the simplified body are 190-210°C, 240-260°C, and 260-280°C, respectively; and the temperature of the membrane head is 270-290°C;

[0032] In step S3, the membrane mouth extrusion pressure is 10-20 MPa.

[0033] The preparation method of the modified PBAT material is as follows, in parts by weight:

[0034] Z1. First, 0.5-2 parts of diatomaceous earth and 0.2-0.4 parts of sodium octadecyl sulfate are added to 18-22 parts of 60-75 wt % ethanol aqueous solution, and stirred for 20-40 minutes, and then dried at a temperature of 100-120° C. for 5-10 hours to obtain a pretreated product;

[0035] Z2, adding 0.4-0.6 parts of gallic acid, 0.8-1.2 parts of polyglycerol and 1.3-1.8 parts of castor oil to 18-22 parts of 70-80wt% ethanol aqueous solution to form an active liquid; spraying the solution evenly on the pre-treated material prepared in step Z1 under the condition of 50-70°C while heating and stirring, and continuing to stir for 1-3 hours after spraying to obtain a post-treated material;

[0036] Z3. Mix 1 to 3 parts of polydopamine and 28 to 32 parts of PBAT material and add them to 180 to 220 parts of dimethylformamide, heat to 40 to 50°C and stir until completely dissolved. Add 1 to 3 parts of ethanol to the solution, mix with the post-treated product prepared in step Z2, and remove the solvent by heating and evaporation. Finally, prepare the mixture into a molten state in a twin-screw extruder, extrude, cool and cut by conventional processes to form a modified PBAT material.

[0037] In the method for making the film-coated thermal insulation bag of the present invention, each substance has the following functions:

[0038] Pearlescent inks, colored inks, these pigments and special effect additives are used to formulate inks to provide specific color effects and gloss to the printed film and enhance visual appeal.

[0039] Connectors (butyl acetate, ethyl acetate, n-propyl acetate) These solvents are used to adjust the viscosity and drying speed of the ink, ensuring that the ink can be evenly applied and dried as required during the printing process. They are mixed in a specific mass ratio to achieve the best printing effect.

[0040] Polyethylene and polypropylene are the main materials for the lamination process. They provide the basic physical properties of the film material, such as strength, temperature resistance and chemical resistance.

[0041] Masterbatches are used to adjust the color of polyethylene and polypropylene materials to ensure the desired color consistency after the materials are mixed.

[0042] In the method for preparing the modified PBAT material, the functions of each substance are as follows:

[0043] As a filler, diatomaceous earth can increase the strength and stability of PBAT materials, while its porous structure helps to improve the thermal insulation performance of the material.

[0044] As a surfactant, sodium octadecyl sulfate helps to improve the compatibility between diatomaceous earth and polymer substrates, improve dispersibility and prevent agglomeration.

[0045] The ethanol aqueous solution is used as a solvent, and 70 wt % of the ethanol aqueous solution is used to pretreat the diatomite, which is helpful for the uniform dispersion and subsequent treatment of the diatomite.

[0046] As an organic acid, gallic acid may act as a cross-linking agent in the active liquid, which helps to enhance the bonding between the filler and the PBAT substrate.

[0047] Polyglycerol Polyglycerol with multiple hydroxyl groups can be used as a dispersant and plasticizer, which helps to improve the processing properties and flexibility of PBAT materials.

[0048] As a natural vegetable oil, castor oil increases lubricity in active liquids and helps improve the processing properties of materials.

[0049] As an excellent solvent, dimethylformamide is used to dissolve PBAT and polydopamine to ensure uniform mixing and facilitate subsequent extrusion processing.

[0050] As a modifier, polydopamine has adhesion and antioxidant properties, and can enhance the chemical corrosion resistance and wear resistance of PBAT materials.

[0051] During the preparation of modified PBAT, the addition of ethanol helps to adjust the viscosity and volatility of the solution, promote the evaporation of the solvent, and reduce residue.

[0052] Through the synergistic effect of these substances, the preparation method of modified PBAT materials aims to improve the comprehensive performance of the materials, including processing performance, physical properties and chemical stability, while maintaining or enhancing their biodegradability and environmental friendliness.

[0053] Compared with the prior art, it has the following beneficial effects:

[0054] 1) The present invention adopts improved printing and laminating technology to replace traditional aluminum-plated coating materials, and realizes the single material of non-woven fabric products through process improvement, which is more environmentally friendly and easier to recycle. It also solves the adhesion problem of aluminum-plated layer corona and the problem of aluminum layer shedding and discoloration during the production process, effectively avoiding the possible harm of the aluminum layer to the human body.

[0055] 2) The film-coated thermal insulation bag of the present invention is waterproof, moisture-proof, wear-resistant and chemically resistant, and at the same time enhances the adhesion of the film, effectively prevents blistering and delamination, and improves the durability and reliability of the product. In addition, by adjusting the ink and coating formula, the color vividness and pattern clarity of the printed matter are improved.

[0056] 3) The present invention uses modified PBAT materials to obtain a coated insulation bag that exhibits better chemical corrosion resistance and wear resistance, which enables the product to maintain its structural integrity and functionality under various conditions of use. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 It is a process flow chart of the film-coated thermal insulation bag of the present invention.

[0058] Figure 2 It is a process flow chart of the printing layer of the present invention. DETAILED DESCRIPTION

[0059] Main sources of substances:

[0060] Pearlescent ink: Guangdong Hongchang Chemical Co., Ltd., model: HC18084PT.

[0061] Color ink: Sichuan Tuozhan New Materials Co., Ltd., item number: TCP-6 series.

[0062] Polyethylene: Yanshan Petrochemical, brand: 1C7A.

[0063] Polypropylene: Ningmei, brand: 1100N.

[0064] Masterbatch, Taizhou Tiansheng, color: white masterbatch, model: 8005.

[0065] Non-woven fabric: Sichuan Kaipu Environmental Protection Packaging Products Co., Ltd., main component: PP, weight: 80g / m 2 .

[0066] Diatomaceous earth, mesh size is 300~400 mesh.

[0067] The polyglycerol was polyglycerol-10 purchased from Shanghai Zhaoheng Industrial Co., Ltd.

[0068] Polydopamine, product number: 5651, Xi'an Qiyue Biotechnology Co., Ltd.

[0069] Kaolin was calcined kaolin purchased from Shanghai Xinguiyuan Chemical Co., Ltd.

[0070] Shell powder comes from the crushed pearl shells of triangular clams, with an average particle size of <1μm.

[0071] PBAT material was purchased from Suzhou Lvbo Degradable Materials Co., Ltd. with brand number 1908.

[0072] Commercially available adhesive: Dongguan Songke New Material Technology Co., Ltd., product number: N / A.

[0073] Membrane: Jintian (Chongqing), material: OPP, thickness: 15um.

[0074] The design idea of ​​the present invention is to develop a film-coated insulation bag with optimized structure and improved performance, and to achieve high visual effects and excellent insulation performance of the product through carefully designed printing layer and laminating process. In the production of the printing layer, a specific proportion of pearlescent ink, color ink and connector are mixed to ensure that the ink color is bright and stable, and the printing quality is ensured through meticulous equipment pre-inspection, layout assembly and fine-tuning, ink mixing, color correction, quality inspection, and final batch printing. In the laminating process, the basic structure of the insulation bag is formed by accurately controlling the material mixing, heating and melting, uniform connection of the cast layer and product cooling steps, wherein the modified PBAT material is further introduced, and the chemical corrosion resistance and wear resistance of the material are enhanced through specific pretreatment, active liquid spraying, mixed dissolution of polydopamine and PBAT, and preparation by a twin-screw extruder, thereby improving the performance of the overall product. The entire design concept runs through strict control of materials, processes and quality control to achieve a film-coated insulation bag that is both beautiful and practical.

[0075] Embodiment 1:

[0076] A method for making a film-coated thermal insulation bag is as follows:

[0077] Material stacking and positioning: First, the printing layer, non-woven fabric and insulation layer are stacked in order from top to bottom, and the basic structure of the insulation bag is formed through the laminating process. The process flow of the laminating insulation bag is as follows: Figure 1 shown.

[0078] The method for making the printed layer is as follows:

[0079] Step 1, ink formula: In the preparation stage, pearlescent ink, color ink and connector are mixed in a mass ratio of 1:1:18, where the connector is a mixture of butyl acetate, ethyl acetate and n-propyl acetate in a mass ratio of 2:4:3. Through color display and measurement, continuous adjustments are made to obtain the ideal visual effect, and then the sample formula is adjusted to large-scale printing ink;

[0080] Step 2: Equipment pre-inspection: Before starting the machine, conduct a comprehensive inspection of the pressurization, transmission, cooling, exhaust and ink absorption systems to ensure that they function normally;

[0081] Step 3: Plate assembly and fine-tuning: According to the design drawing, proofread and assemble the printing plate, and adjust the gap between the doctor blade and the plate roller to 40 microns and the angle to 45 degrees;

[0082] Step 4: Ink preparation: Pour the prepared ink into the ink tray and adjust its viscosity to 20 seconds (measured using a No. 4 Zahn cup);

[0083] Step 5: Color calibration and test printing: After performing longitudinal and transverse color calibration, start test printing;

[0084] Step 6, quality inspection: Conduct detailed quality inspection on the printed product, including dot integrity, overprint accuracy and pattern clarity. Also check whether there are any cuts or dirty spots on the layout, and inspect the color. If necessary, make fine adjustments.

[0085] Step 7, batch printing: After confirming that the quality meets the standards, start batch printing. The process flow of the printing layer is as follows: Figure 2 shown.

[0086] The coating process is as follows:

[0087] S1. Material mixing: put polypropylene, masterbatch and polyethylene into a stirring device at a mass ratio of 50:30:1, set the stirring speed to 200 rpm, the temperature to 120°C and the stirring time to 20 minutes to ensure uniform mixing;

[0088] S2. Material heating and melting: Pour the mixed material into the funnel of the laminating equipment, and heat and melt it through the temperature control of the screw, cylinder and film head. The temperature of the screw is 220℃, 240℃, 260℃, the temperature of the cylinder is 200℃, 250℃, 265℃, and the temperature of the film head is 280℃.

[0089] S3, uniform connection of cast layer: after the film mouth is squeezed by 15MPa pressure, rollers are used to press the cast layer evenly between the non-woven fabric and the printing layer, and between the non-woven fabric and the insulation layer. The insulation layer is a film (purchased from Jintian (Chongqing), material: OPP, thickness: 15um), and the flow rate is controlled to meet the product process requirements;

[0090] S4. Product cooling: The product is quickly cooled and solidified through a circulating water cooling system.

[0091] Embodiment 2:

[0092] The method for making a film-coated thermal insulation bag is basically the same as that in Example 1, the only difference being that the film coating process is different.

[0093] The coating process is as follows:

[0094] S1. Material mixing: put polypropylene, masterbatch, polyethylene and modified PBAT materials into a stirring device at a mass ratio of 50:30:1:2, set the stirring speed to 200 rpm, the temperature to 120°C and the stirring time to 20 minutes to ensure uniform mixing;

[0095] S2. Material heating and melting: Pour the mixed material into the funnel of the laminating equipment, and heat and melt it through the temperature control of the screw, cylinder and film head. The temperature of the screw is 220℃, 240℃, 260℃, the temperature of the cylinder is 200℃, 250℃, 265℃, and the temperature of the film head is 280℃.

[0096] S3, uniform connection of cast layer: after the film mouth is squeezed by 15MPa pressure, rollers are used to press the cast layer evenly between the non-woven fabric and the printing layer, and between the non-woven fabric and the insulation layer. The insulation film is a film (purchased from Jintian (Chongqing), material: OPP, thickness: 15um), and the flow rate is controlled to meet the product process requirements;

[0097] S4. Product cooling: The product is quickly cooled and solidified through a circulating water cooling system.

[0098] The preparation method of the modified PBAT material is as follows:

[0099] Z1. First, 1 kg of diatomaceous earth and 0.3 kg of sodium octadecyl sulfate were added to 20 kg of 70 wt% ethanol aqueous solution, and stirred for 30 minutes, and then dried at 110° C. for 8 hours to obtain a pretreated product;

[0100] Z2, 0.5 kg of gallic acid, 1 kg of polyglycerol and 1.5 kg of castor oil were mixed and added into 20 kg of 75 wt% ethanol aqueous solution to form an active liquid; under the condition of 60° C., the solution was evenly sprayed on the pre-treated material prepared in step Z1 while heating and stirring, and the stirring was continued for 2 hours after the spraying was completed to obtain a post-treated material;

[0101] Z3. Mix 2 kg of polydopamine and 30 kg of PBAT material and add them to 200 kg of dimethylformamide, heat to 45 ° C and stir until completely dissolved, add 2 kg of ethanol to this solution, mix it with the post-treated product prepared in step Z2, and remove the solvent by heating and evaporation. Finally, prepare the mixture into a molten state in a twin-screw extruder, extrude, cool and cut it through conventional processes to form a modified PBAT material.

[0102] Embodiment 3:

[0103] The method for making a film-coated insulation bag is basically the same as that in Example 2, the only difference being the method for making the modified PBAT material.

[0104] The preparation method of the modified PBAT material is as follows:

[0105] Z1. First, 1 kg of kaolin and 0.3 kg of sodium octadecyl sulfate were added to 20 kg of 70 wt% ethanol aqueous solution, and stirred for 30 minutes, and then dried at 110° C. for 8 hours to obtain a pretreated product;

[0106] Z2, 0.5 kg of gallic acid, 1 kg of polyglycerol and 1.5 kg of castor oil were mixed and added into 20 kg of 75 wt% ethanol aqueous solution to form an active liquid; under the condition of 60° C., the solution was evenly sprayed on the pre-treated material prepared in step Z1 while heating and stirring, and the stirring was continued for 2 hours after the spraying was completed to obtain a post-treated material;

[0107] Z3. Mix 2 kg of polydopamine and 30 kg of PBAT material and add them to 200 kg of dimethylformamide, heat to 45 ° C and stir until completely dissolved, add 2 kg of ethanol to this solution, mix it with the post-treated product prepared in step Z2, and remove the solvent by heating and evaporation. Finally, prepare the mixture into a molten state in a twin-screw extruder, extrude, cool and cut it through conventional processes to form a modified PBAT material.

[0108] Embodiment 4:

[0109] The method for making a film-coated insulation bag is basically the same as that in Example 2, the only difference being the method for making the modified PBAT material.

[0110] The preparation method of the modified PBAT material is as follows:

[0111] Z1. First, 1 kg of shell powder and 0.3 kg of sodium octadecyl sulfate were added to 20 kg of 70 wt% ethanol aqueous solution, and stirred for 30 minutes, and then dried at 110° C. for 8 hours to obtain a pretreated product;

[0112] Z2, 0.5 kg of gallic acid, 1 kg of polyglycerol and 1.5 kg of castor oil were mixed and added into 20 kg of 75 wt% ethanol aqueous solution to form an active liquid; under the condition of 60° C., the solution was evenly sprayed on the pre-treated material prepared in step Z1 while heating and stirring, and the stirring was continued for 2 hours after the spraying was completed to obtain a post-treated material;

[0113] Z3. Mix 2 kg of polydopamine and 30 kg of PBAT material and add them to 200 kg of dimethylformamide, heat to 45 ° C and stir until completely dissolved, add 2 kg of ethanol to this solution, mix it with the post-treated product prepared in step Z2, and remove the solvent by heating and evaporation. Finally, prepare the mixture into a molten state in a twin-screw extruder, extrude, cool and cut it through conventional processes to form a modified PBAT material.

[0114] Embodiment 5:

[0115] The method for making a film-coated insulation bag is basically the same as that in Example 2, the only difference being the method for making the modified PBAT material.

[0116] The preparation method of the modified PBAT material is as follows:

[0117] Z1. First, 1 kg of diatomaceous earth and 0.3 kg of sodium octadecyl sulfate were added to 20 kg of 70 wt% ethanol aqueous solution, and stirred for 30 minutes, and then dried at 110° C. for 8 hours to obtain a pretreated product;

[0118] Z2, 0.5 kg of gallic acid, 1 kg of polyglycerol and 1.5 kg of castor oil were mixed and added into 20 kg of 75 wt% ethanol aqueous solution to form an active liquid; under the condition of 60° C., the solution was evenly sprayed on the pre-treated material prepared in step Z1 while heating and stirring, and the stirring was continued for 2 hours after the spraying was completed to obtain a post-treated material;

[0119] Z3. Mix 2 kg of methyl-β-cyclodextrin and 30 kg of PBAT material and add them to 200 kg of dimethylformamide, heat to 45 ° C and stir until completely dissolved, add 2 kg of ethanol to this solution, mix it with the post-treated product prepared in step Z2, and remove the solvent by heating and evaporation. Finally, prepare the mixture into a molten state in a twin-screw extruder, extrude, cool and cut it through conventional processes to form a modified PBAT material.

[0120] Embodiment 6:

[0121] The method for making a film-coated insulation bag is basically the same as that in Example 2, the only difference being the method for making the modified PBAT material.

[0122] The preparation method of the modified PBAT material is as follows:

[0123] Z1. First, 1 kg of diatomaceous earth and 0.3 kg of sodium octadecyl sulfate were added to 20 kg of 70 wt% ethanol aqueous solution, and stirred for 30 minutes, and then dried at 110° C. for 8 hours to obtain a pretreated product;

[0124] Z2, 0.5 kg of gallic acid, 1 kg of polyglycerol and 1.5 kg of castor oil were mixed and added into 20 kg of 75 wt% ethanol aqueous solution to form an active liquid; under the condition of 60° C., the solution was evenly sprayed on the pre-treated material prepared in step Z1 while heating and stirring, and the stirring was continued for 2 hours after the spraying was completed to obtain a post-treated material;

[0125] Z3. Mix 2kg of γ-cyclodextrin and 30kg of PBAT material and add them to 200kg of dimethylformamide, heat to 45°C and stir until completely dissolved. Add 2kg of ethanol to the solution, mix it with the post-treated product prepared in step Z2, and remove the solvent by heating and evaporation. Finally, prepare the mixture into a molten state in a twin-screw extruder, extrude, cool and cut it by conventional processes to form a modified PBAT material.

[0126] Embodiment 7:

[0127] The method for making a film-coated insulation bag is basically the same as that in Example 2, the only difference being the method for making the modified PBAT material.

[0128] The preparation method of the modified PBAT material is as follows:

[0129] Z1. First, 1 kg of diatomaceous earth and 0.3 kg of sodium octadecyl sulfate were added to 20 kg of 70 wt% ethanol aqueous solution, and stirred for 30 minutes, and then dried at 110° C. for 8 hours to obtain a pretreated product;

[0130] Z2, 0.5 kg of gallic acid, 1 kg of polyglycerol and 1.5 kg of castor oil were mixed and added into 20 kg of 75 wt% ethanol aqueous solution to form an active liquid; under the condition of 60° C., the solution was evenly sprayed on the pre-treated material prepared in step Z1 while heating and stirring, and the stirring was continued for 2 hours after the spraying was completed to obtain a post-treated material;

[0131] Z3. Mix 2kg of β-cyclodextrin and 30kg of PBAT material and add them to 200kg of dimethylformamide, heat to 45°C and stir until completely dissolved. Add 2kg of ethanol to the solution, mix it with the post-treated product prepared in step Z2, and remove the solvent by heating and evaporation. Finally, prepare the mixture into a molten state in a twin-screw extruder, extrude, cool and cut it by conventional processes to form a modified PBAT material.

[0132] Comparative Example 1:

[0133] The method for making a film-coated thermal insulation bag is basically the same as that in Example 1, the only difference being that the film coating process is different.

[0134] The coating process is as follows:

[0135] S1. Material mixing: put polypropylene, masterbatch, polyethylene and commercially available adhesive into a stirring device at a mass ratio of 50:30:1:2, set the stirring speed to 200 rpm, the temperature to 120°C and the stirring time to 20 minutes to ensure uniform mixing;

[0136] S2. Material heating and melting: Pour the mixed material into the funnel of the laminating equipment, and heat and melt it through the temperature control of the screw, cylinder and film head. The temperature of the screw is 220℃, 240℃, 260℃, the temperature of the cylinder is 200℃, 250℃, 265℃, and the temperature of the film head is 280℃.

[0137] S3, uniform connection of cast layer: after the film mouth is squeezed by 15MPa pressure, rollers are used to press the cast layer evenly between the non-woven fabric and the printing layer, and between the non-woven fabric and the insulation layer. The insulation film is a film (purchased from Jintian (Chongqing), material: OPP, thickness: 15um), and the flow rate is controlled to meet the product process requirements;

[0138] S4. Product cooling: The product is quickly cooled and solidified through a circulating water cooling system.

[0139] Test Example 1:

[0140] Chemical corrosion resistance test:

[0141] In order to evaluate the chemical corrosion resistance of the material, the following test process was used in this experiment:

[0142] By producing uniform test bags, the size is standardized to 600 mm long and 800 mm wide. Sulfuric acid and industrial pure water are mixed in a weight ratio of 7:3 to form a sulfuric acid solution for the experiment. The prepared sulfuric acid solution is quantitatively filled into the test bag until the volume is 3 liters, and then sealed to ensure no leakage. The sealed bag is placed in a room temperature environment, continuously observed, and the time when the test bag is damaged or leaked is recorded.

[0143] The test results are shown in Table 1.

[0144] Table 1:

[0145]

[0146] Test Example 2:

[0147] Wear resistance test:

[0148] Wear coefficient: The wear coefficient of live fish inflatable bags is tested according to GB / T 5478-2008 "Test method for rolling wear of plastics". The wear coefficient is mass wear.

[0149] The test results are shown in Table 2.

[0150] Table 2:

[0151]

[0152] It can be seen from test examples 1 and 2 that the film-coated insulation bag obtained in Example 2 of the present invention has the best chemical corrosion resistance and wear resistance.

[0153] The diatomite used in Example 2 exhibits excellent chemical corrosion resistance and wear resistance due to its unique porous structure and high content of silicon dioxide. This structure not only increases the contact area with the polymer substrate, thereby improving the interfacial bonding strength, but also the porous nature helps to disperse surface stress and reduce the penetration of chemical media. At the same time, the silicon dioxide component in diatomite provides a high degree of chemical stability, making it less likely to react in an acidic environment, maintaining the integrity of the material. In contrast, the layered structure of kaolin may peel off under the action of chemical media, and the calcium carbonate component in shell powder is easily dissolved under acidic conditions, resulting in reduced chemical corrosion resistance. Therefore, these molecular characteristics of diatomite provide better chemical corrosion resistance and wear resistance than kaolin and shell powder in the production of coated insulation bags.

[0154] The reason why the polydopamine selected in Example 2 performs better than the cyclodextrins in Examples 5, 6 and 7 in terms of chemical corrosion resistance and wear resistance is mainly due to the unique molecular structure of polydopamine. Polydopamine contains a large amount of phenolic hydroxyl groups, which can not only enhance the interaction with other molecules by forming covalent bonds or hydrogen bonds, but also in terms of chemical stability, the phenolic hydroxyl groups can resist the erosion of various chemical substances, thereby providing an additional protective layer. At the same time, the polymer network structure of polydopamine physically increases the toughness and durability of the material, helps to disperse and absorb externally applied stress, and reduces wear. In contrast, although cyclodextrin has inclusion capacity, its glycosyl structure is relatively fragile, susceptible to chemical environment, and does not have a cross-linked network like polydopamine to provide mechanical strength and chemical stability, so it is not as excellent as polydopamine in terms of chemical corrosion resistance and wear resistance.

[0155] The modified PBAT material in Example 2 has better chemical corrosion resistance and wear resistance. In the process of making the modified PBAT material, diatomaceous earth and sodium octadecyl sulfate are first treated in an ethanol aqueous solution to enhance the hydrophilicity and dispersibility of diatomaceous earth. The subsequent drying step ensures the dryness of the material, providing a basis for subsequent modification. Next, the active liquid formed by mixing gallic acid, polyglycerol and castor oil is sprayed on the pretreated material, which not only introduces active functional groups, but also increases the interfacial compatibility and adhesion of the material. Finally, the mixed dissolution of polydopamine and PBAT material in dimethylformamide and the post-treatment of adding ethanol promote the interaction between polydopamine and PBAT to form a uniform mixture. The melt mixing, cooling and cutting prepared by the twin-screw extruder form a modified PBAT material with improved performance. This process not only improves the chemical stability and thermal stability of the material, but also enhances the mechanical properties and durability of the material through the synergy of physical and chemical effects. In contrast, commercially available adhesives may lack this inherent chemical stability, and without the addition of modified PBAT materials, they lack this reinforced cross-linked network and therefore do not perform as well in terms of chemical corrosion resistance and wear resistance as with the addition of modified PBAT materials.

Claims

1. A method for making a film-coated thermal insulation bag, characterized in that: Here’s how: Material stacking and positioning: First, the printing layer, non-woven fabric and insulation layer are stacked from top to bottom to form the basic structure of the insulation bag through the laminating process; The method for making the printed layer is as follows: Step 1, ink formulation: In the preparation stage, pearlescent ink, color ink and connector are mixed, and through color display and measurement, they are continuously adjusted to obtain the ideal visual effect, and then adjusted to large-scale printing ink according to the sample formula; Step 2: Equipment pre-inspection: Before starting the machine, conduct a comprehensive inspection of the pressurization, transmission, cooling, exhaust and ink absorption systems to ensure that they function normally; Step 3: Plate assembly and fine-tuning: According to the design drawing, proofread and assemble the printing plate, and adjust the gap and angle between the doctor blade and the plate roller; Step 4: Ink preparation: Pour the prepared ink into the ink tray and adjust its viscosity; Step 5: Color calibration and test printing: After performing longitudinal and transverse color calibration, start test printing; Step 6, quality inspection: Conduct quality inspection on printed products, including dot integrity, overprint accuracy and pattern clarity. Also check whether there are any cuts or dirty spots on the layout, and inspect the color. If necessary, make fine adjustments. Step 7, batch printing: After confirming that the quality meets the standards, start batch printing; The coating process is as follows: S1. Material mixing: put polypropylene, masterbatch, polyethylene and modified PBAT material into a stirring device, wherein the mass ratio of polypropylene, masterbatch, polyethylene and modified PBAT material is 40-60:20-40:0.5-2:1-3; set the stirring speed, temperature and time to ensure uniform mixing; S2. Material heating and melting: Pour the mixed material into the funnel of the laminating equipment, and heat and melt it through the temperature control of the screw, cylinder and film head; S3, Uniform connection of cast layer: After the film mouth is extruded, the cast layer is evenly connected between the non-woven fabric and the printing layer, and between the non-woven fabric and the insulation layer by roller pressing, and the flow rate is controlled to meet the product process requirements; S4. Product cooling: The product is quickly cooled and solidified through the circulating water cooling system; The preparation method of the modified PBAT material is as follows, in parts by weight: Z1. First, 0.5-2 parts of diatomaceous earth and 0.2-0.4 parts of sodium octadecyl sulfate are added to 18-22 parts of 60-75 wt % ethanol aqueous solution, and stirred for 20-40 minutes, and then dried at a temperature of 100-120° C. for 5-10 hours to obtain a pretreated product; Z2, adding 0.4-0.6 parts of gallic acid, 0.8-1.2 parts of polyglycerol and 1.3-1.8 parts of castor oil to 18-22 parts of 70-80wt% ethanol aqueous solution to form an active liquid; spraying the solution evenly on the pre-treated material prepared in step Z1 under the condition of 50-70°C while heating and stirring, and continuing to stir for 1-3 hours after spraying to obtain a post-treated material; Z3. Mix 1 to 3 parts of polydopamine and 28 to 32 parts of PBAT material and add them to 180 to 220 parts of dimethylformamide, heat to 40 to 50°C and stir until completely dissolved. Add 1 to 3 parts of ethanol to the solution, mix with the post-treated product prepared in step Z2, and remove the solvent by heating and evaporation. Finally, prepare the mixture into a molten state in a twin-screw extruder, extrude, cool and cut by conventional processes to form a modified PBAT material.

2. The method for making a film-coated thermal insulation bag according to claim 1, characterized in that: In the step 1, the mass ratio of pearlescent ink, color ink and connector is 0.5-2:0.5-2:15-19; the connector in the step 1 is composed of butyl acetate, ethyl acetate and n-propyl acetate in a mass ratio of 1-3:3-5:2-4.

3. The method for making a film-coated thermal insulation bag according to claim 1, characterized in that: In step 3, the distance between the scraper and the plate roller is 30-50 μm, and the angle is 40-50°.

4. The method for making a film-coated thermal insulation bag according to claim 1, characterized in that: In step 4, the ink viscosity is adjusted to 15-25 seconds and measured using a No. 4 Zahn cup.

5. The method for making a film-coated thermal insulation bag according to claim 1, characterized in that: In the step S1, the stirring speed is set to 100-300 rpm, the temperature is set to 110-130° C., and the time is set to 10-30 minutes.

6. The method for making a film-coated thermal insulation bag according to claim 1, characterized in that: In step S2, the temperatures of the screw are 210-230°C, 230-250°C, and 250-270°C, respectively; the temperatures of the simplified body are 190-210°C, 240-260°C, and 260-280°C, respectively; and the temperature of the membrane head is 270-290°C; In step S3, the membrane mouth extrusion pressure is 10-20 MPa.

7. A film-coated thermal insulation bag, characterized in that: The invention is produced by the production method according to any one of claims 1 to 6.