Preparation method of hydrotalcite-coated MOF (Metal Organic Framework)-based PVC (Polyvinyl Chloride) heat stabilizer
By self-assembly on the hydrotalcite surface to form a MOF with zinc ions and 2-methylimidazole as the coordination framework, the problem of dispersion of MOF and hydrotalcite components in the PVC thermal stabilizer is solved, significantly improving the thermal stability and performance of PVC. Initial coloring performance, full utilization of raw materials and zero discharge of waste water.
Patent Information
- Application Number
- CN202411236099.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-10-22
AI Technical Summary
In the existing technology, components such as MOF and hydrotalcite in PVC thermal stabilizers are highly dispersed and have poor surface contact effects, which affects its thermal stability.
Using zinc oxide and 2-methylimidazole as raw materials, they self-assemble on the surface of hydrotalcite through the action of carbon dioxide to form a MOF with zinc ions and 2-methylimidazole as the coordination skeleton to prepare hydrotalcite@MOF composite materials to achieve high dispersion and synergy.
Significantly improving the thermal stability and initial coloring performance of PVC, the hydrotalcite@MOF material can stably absorb hydrogen chloride from thermal degradation of PVC, achieve good long-term thermal stability, and achieve full utilization of raw materials and zero discharge of waste water through the dehydration process.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of plastic additives, and in particular to a method for preparing a hydrotalcite@MOF-based PVC heat stabilizer. Background Art
[0002] Heat stabilizer is a kind of additive that must be added during the processing of PVC products. It can effectively inhibit the thermal degradation of PVC. Among environmentally friendly PVC heat stabilizers, hydrotalcite is a widely used long-acting PVC heat stabilizer component. Hydrotalcite can absorb the hydrogen chloride released by the thermal degradation of PVC through interlayer anion substitution and interlayer cation reaction, inhibiting the autocatalytic degradation of PVC, thereby showing good thermal stability for PVC. However, hydrotalcite has weak performance in inhibiting the initial coloring of PVC. Therefore, hydrotalcite is often used in combination with primary heat stabilizers to improve the overall performance of the base.
[0003] MOF is the abbreviation of metal organic framework material. It has a regular skeleton and pores and has been widely used in adsorption, catalysis, separation, biomedicine and polymer material additives. In recent years, researchers have tried to apply MOF to the field of PVC heat stabilizers. For example, Zhou Xi and others found that MOF-5 and other MOF materials can be combined with calcium stearate, hydrotalcite, β -Diketone compound use has good thermal stability for PVC (CN104387702A). Kodahao et al. reported that MOF as an auxiliary stabilizer can effectively improve the thermal stability of the main stabilizers calcium stearate and zinc stearate for PVC (CN116178792A).
[0004] Based on the regular pores and high specific surface area of MOF, achieving high dispersion and surface contact between MOF and components such as hydrotalcite to better exert their synergistic effect and further improve their performance as PVC composite thermal stabilizers is still one of the key technical problems that technicians in this field need to solve. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a hydrotalcite@MOF-based PVC heat stabilizer. The method uses zinc oxide and 2-methylimidazole as raw materials, and through the action of carbon dioxide, self-assembles on the surface of hydrotalcite to form a MOF with zinc ions and 2-methylimidazole as a coordination skeleton. The prepared hydrotalcite@MOF composite material has very excellent performance as a PVC heat stabilizer.
[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is a method for preparing a hydrotalcite@MOF-based PVC heat stabilizer, characterized in that it comprises the following steps: (1) Dispersing hydrotalcite in water, and then adding zinc oxide and 2-methylimidazole; (2) Add carbon dioxide and stir the reaction for 0.2 to 2 hours; (3) Stop introducing carbon dioxide, raise the temperature to 60-100° C., and continue the reaction for 0.5-3 hours. Dehydrate and dry the solid obtained by the reaction to obtain a hydrotalcite@MOF-based PVC thermal stabilizer.
[0007] The chemical formula of the hydrotalcite is [M 2+ 1-x M 3+ x (OH) 2 ] x+ (CO 3 ) 2- x / 2 , where M 2+ Mg 2+ 、Zn 2+ and Ca 2+ One or more of M 3+ For Al 3+ , 0.25 ≤ x ≤ 0.35.
[0008] The mass ratio of the hydrotalcite to water is 1:10-100.
[0009] The mass ratio of the hydrotalcite to zinc oxide is 1:0.3-2.
[0010] The molar ratio of zinc oxide to 2-methylimidazole is 1:3-8.
[0011] The pressure of carbon dioxide in step (2) is 0.1-0.5 MPa.
[0012] The technical solution provided by the present invention uses zinc oxide and 2-methylimidazole as raw materials, and through the action of carbon dioxide, self-assembles on the surface of hydrotalcite to form a MOF shell with zinc ions and 2-methylimidazole as the coordination skeleton to prepare a hydrotalcite @ MOF-based PVC thermal stabilizer. In the hydrotalcite @ MOF composite material, a high dispersion of hydrotalcite in MOF is achieved. The MOF framework contains Zn 2+ The structural units of hydrotalcite and 2-methylimidazole can not only replace the unstable allyl chloride on the PVC chain, but also react quickly with hydrogen chloride, and have excellent performance in inhibiting the initial coloring of PVC. Hydrotalcite can stably absorb the hydrogen chloride released by the thermal degradation of PVC, and has good long-term thermal stability for PVC. Highly dispersed hydrotalcite has good synergistic effect with MOF and shows very excellent thermal stability for PVC. In addition, the filtrate obtained from the dehydration process in the preparation process can be recycled, thereby achieving full utilization of raw materials and zero discharge of wastewater. DETAILED DESCRIPTION
[0013] The specific embodiments of the present invention are further described in detail below. For those skilled in the art, the above and other objects, features and advantages of the present invention will be apparent from the detailed description of the present invention. Example 1
[0014] 10 g of the chemical formula [Mg 2+ 0.7 Al 3+ 0.3 (OH) 2 ] 0.3+ (CO 3 ) 2- 0.3 / 2 The hydrotalcite was dispersed in 300 ml of water, and then 6 g of zinc oxide and 25 g of 2-methylimidazole were added. Carbon dioxide was introduced, and the carbon dioxide pressure was maintained at 0.1 MPa. The reaction was stirred for 0.5 hours. The introduction of carbon dioxide was stopped, the temperature was raised to 80°C, and the reaction was continued for 1 hour. The precipitate obtained by the reaction was dehydrated and dried to obtain about 25 g of hydrotalcite@MOF-based PVC thermal stabilizer. Example 2
[0015] 10 g of the chemical formula [Ca 2+ 0.7 Al 3+ 0.3 (OH) 2 ] 0.3+ (CO 3 ) 2- 0.3 / 2 The hydrotalcite was dispersed in 200 ml of water, and then 12 g of zinc oxide and 60 g of 2-methylimidazole were added. Carbon dioxide was introduced, and the carbon dioxide pressure was maintained at 0.1 MPa. The reaction was stirred for 1 hour. The introduction of carbon dioxide was stopped, the temperature was raised to 90°C, and the reaction was continued for 2 hours. The precipitate obtained by the reaction was dehydrated and dried to obtain about 36 g of hydrotalcite@MOF-based PVC thermal stabilizer. Example 3
[0016] 10 g of the chemical formula [Zn 2+ 0.67 Al 3+ 0.33 (OH) 2 ] 0.33+ (CO 3 ) 2- 0.33 / 2The hydrotalcite was dispersed in 500 ml of water, and then 4 g of zinc oxide and 24 g of 2-methylimidazole were added. Carbon dioxide was introduced, and the carbon dioxide pressure was maintained at 0.3 MPa. The reaction was stirred for 1.5 hours. The introduction of carbon dioxide was stopped, the temperature was raised to 80°C, and the reaction was continued for 3 hours. The precipitate obtained by the reaction was dehydrated and dried to obtain about 19 g of hydrotalcite@MOF-based PVC thermal stabilizer. Example 4
[0017] The filtrate obtained in the dehydration step during the preparation process of Example 1 was recovered, and fresh water was added to 300 ml; except that the amount of 2-methylimidazole added was replaced with 12 g, the rest of the preparation process was the same as Example 1, and about 25 g of hydrotalcite@MOF-based PVC thermal stabilizer was obtained. Comparative Example 1
[0018] Except that hydrotalcite was not added, the rest of the preparation process was the same as Example 1 to obtain a MOF-based PVC heat stabilizer. Comparative Example 2
[0019] 10 g of the hydrotalcite used in Example 1 was physically mixed with the MOF prepared in Comparative Example 1 to obtain a hydrotalcite and MOF mixed PVC heat stabilizer. Performance test experiment:
[0020] The hydrotalcite@MOF-based PVC heat stabilizer is uniformly mixed with other additives to prepare a PVC additive, and its specific composition is (mass fraction): 80% of the hydrotalcite@MOF-based PVC heat stabilizer, 7% of calcium stearate, 5% of 1,3-dimethyl-6-aminouracil, 1% of antioxidant 1010, and 7% of PE wax.
[0021] The performance of the PVC additive prepared with hydrotalcite@MOF-based PVC heat stabilizer as the main component was tested using a Harp RM-200A torque rheometer under the following test conditions: material temperature 190°C, test load 5 kg, and rotation speed 35 rpm. The test sample composition: 55 parts PVC (SG-3 type) resin, 1.6 parts composite heat stabilizer, 12 parts CaCO 3 , 5 parts CPE, 1.8 parts titanium dioxide, 0.2 parts PE wax, 1 part ACR. Test method: After mixing in the torque rheometer for 10 minutes, take out the sample, use a colorimeter to test the initial whiteness, and take another sample to test the dynamic thermal stability time. The test results are shown in Table 1.
[0022] Table 1:
[0023] From the performance test results of Examples 1-3 in Table 1, it can be seen that the prepared hydrotalcite @ MOF can not only effectively inhibit the initial coloring of PVC, but also has excellent long-term thermal stability, and exhibits very excellent performance as a PVC thermal stabilizer. From the performance test results of Example 4, it can be seen that the hydrotalcite @ MOF prepared using the recovered filtrate also has excellent thermal stability for PVC, and is comparable to the performance of the product prepared using fresh raw materials in Example 1. From the performance test results of Example 1 and Comparative Examples 1 and 2, it can be seen that the performance of the hydrotalcite @ MOF-based PVC thermal stabilizer is significantly better than that of a single MOF and a hydrotalcite and MOF mixed PVC thermal stabilizer obtained by physical mixing. This shows that the hydrotalcite and MOF components in the hydrotalcite @ MOF material are highly dispersed and interact with each other, thereby exhibiting good synergistic effects.
[0024] The technical solution provided by the present invention is to use zinc oxide and 2-methylimidazole as raw materials, and through the action of carbon dioxide, self-assemble on the surface of hydrotalcite to form a MOF shell with zinc ions and 2-methylimidazole as the coordination skeleton. In the hydrotalcite@MOF composite material, the high dispersion of hydrotalcite in MOF is achieved. The framework of MOF contains Zn 2+ The structural units of hydrotalcite and 2-methylimidazole can replace the unstable allyl chloride on the PVC chain and react quickly with hydrogen chloride, which has excellent performance in inhibiting the initial coloring of PVC. Hydrotalcite can stably absorb the hydrogen chloride released by the thermal degradation of PVC and has good long-term thermal stability for PVC. Highly dispersed hydrotalcite has good synergistic effect with MOF and shows very excellent thermal stability for PVC. In addition, the filtrate obtained from the dehydration process in the preparation process can be recycled, thereby achieving full utilization of raw materials and zero discharge of wastewater.
[0025] It should be understood that although the present invention has been clearly illustrated by the above embodiments, without departing from the spirit and essence of the present invention, technicians in the relevant technical field can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a hydrotalcite@MOF-based PVC heat stabilizer, characterized in that: The following steps are involved: (1) Dispersing hydrotalcite in water, and then adding zinc oxide and 2-methylimidazole; (2) Add carbon dioxide and stir the reaction for 0.2 to 2 hours; (3) Stop introducing carbon dioxide, raise the temperature to 60-100° C., and continue the reaction for 0.5-3 hours. Dehydrate and dry the solid obtained by the reaction to obtain a hydrotalcite@MOF-based PVC thermal stabilizer.
2. The method for preparing a hydrotalcite@MOF-based PVC heat stabilizer according to claim 1, characterized in that: The chemical formula of the hydrotalcite is [M 2+ 1-x M 3+ x (OH)2] x+ (CO3) 2- x / 2 , where M 2+ Mg 2+ 、Zn 2+ and Ca 2+ One or more of M 3 + For Al 3+ , 0.25 ≤ x ≤ 0.
35.
3. The method for preparing the hydrotalcite@MOF-based PVC heat stabilizer according to claim 1, characterized in that: The mass ratio of the hydrotalcite to water is 1:10-100.
4. The method for preparing the hydrotalcite@MOF-based PVC heat stabilizer according to claim 1, characterized in that: The mass ratio of the hydrotalcite to zinc oxide is 1:0.3-2.
5. The method for preparing the hydrotalcite@MOF-based PVC heat stabilizer according to claim 1, characterized in that: The molar ratio of zinc oxide to 2-methylimidazole is 1:3-8.
6. The method for preparing the hydrotalcite@MOF-based PVC heat stabilizer according to claim 1, characterized in that: The pressure of carbon dioxide in step (2) is 0.1-0.5 MPa.
Citation Information
Cited By
AIL-MIL-96-based magnesium-aluminum hydrotalcite as well as preparation method and application thereof
CN121271027A