Transition metal compound doped thermal activation delayed fluorescence film, electroluminescent device and preparation thereof
By doping chlorine (1,5-cyclooctadiene) copper (I) dimer into thermally activated delayed fluorescent materials, the problem of absorption loss caused by the accumulation of triplet excitons under electrical injection is solved, and the laser performance and The electroluminescence intensity realizes the reduction of optical loss of organic electrical pump laser.
Patent Information
- Application Number
- CN202310426423.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-22
AI Technical Summary
In existing organic electrical pump laser devices, the absorption loss and singlet exciton annihilation efficiency caused by the accumulation of triplet excitons under electrical injection are low, resulting in limited laser performance.
Doping the transition metal compound chlorine (1,5-cyclooctadiene) copper (I) dimer into the thermally activated delayed fluorescent material can reduce non-radiative transition dissipation, overcome the spin prohibition limit, and increase the triplet exciton utilization rate.
By doping transition metal compounds, the utilization rate of charge transfer state excitons is improved, the optical loss of organic electrical pump lasers is reduced, the luminescence performance is improved, and the electroluminescence intensity is increased by 68% at the same current density.
Smart Images

Figure CN118813239A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of organic light-emitting and laser material devices, and specifically relates to an organic thermally activated delayed fluorescent film doped with a transition metal compound, an electroluminescent device thereof and a preparation method thereof. Background Art
[0002] As a miniaturized coherent light source, organic electrically pumped lasers have the characteristics of solution processability, flexibility, and tunability over a wide wavelength range, which helps promote the effective integration and interconnection of photonic devices and other optoelectronic circuits, and thus show great application prospects in the fields of spectral imaging, display, remote communication, medical diagnosis, etc.
[0003] As the key to the practical application of organic solid-state lasers, electrically driven organic micro-nano lasers have attracted widespread attention, but have not yet been realized. One of the key bottlenecks is the absorption loss caused by the accumulation of triplet excitons under electrical injection and the annihilation of singlet excitons. Thermally activated delayed fluorescent materials have a small energy range between the triplet and singlet states, and can promote the reverse intersystem crossing process through external thermal excitation, so that triplet excitons are converted into singlet excitons for luminescence, which has attracted widespread attention. However, the rate of reverse intersystem crossing is not only affected by the energy range difference between the triplet and singlet states, but also by the law of conservation of spin angular momentum. It is a spin-forbidden process. Therefore, even if the energy range difference between the two is very small, reverse intersystem crossing is still an inefficient process, and the rate constant is often less than 10 6 s -1 , the accumulation of triplet excitons cannot be avoided. Summary of the invention
[0004] In order to solve the shortcomings of the prior art, the present invention provides a method for improving the utilization rate of charge transfer state excitons and reducing the optical loss of organic electrically pumped lasers by doping transition metal compounds in thermally activated delayed fluorescent molecules; the transition metal compound is chloro(1,5-cyclooctadiene)copper(I) dimer, which reduces the dissipation of non-radiative transitions in the system, overcomes the limitations of spin prohibition in the intersystem crossing process, and turns triplet excitons into treasure for the particle number inversion process, thereby improving the utilization rate of charge transfer state excitons, and can be used to prepare laser display panels and other products.
[0005] One of the purposes of the present invention is to provide a transition metal compound doped thermally activated delayed fluorescence film, comprising a fluorescence donor molecule, a fluorescence acceptor molecule and a transition metal compound, wherein the fluorescence donor molecule is a triphenylamine compound, the fluorescence acceptor molecule is an organic borane compound, and the transition metal compound is chloro(1,5-cyclooctadiene)copper(I) dimer.
[0006] According to an embodiment of the present invention, the fluorescent donor molecule is 4,4',4"-tri(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), and the fluorescent acceptor molecule is tri[2,4,6-trimethyl-3-(3-pyridyl)phenyl]borane (3TPYMB), wherein the structure of the m-MTDATA is shown in Formula 1, the structure of the 3TPYMB is shown in Formula 2, and the structure of the chloro(1,5-cyclooctadiene)copper(I) dimer is shown in Formula 3.
[0007]
[0008]
[0009] The present invention discloses a method for reducing the optical loss of an organic electrically pumped laser by doping a transition metal compound in a thermally activated delayed fluorescent molecule to improve the utilization rate of charge transfer state excitons. The organic thermally activated delayed fluorescent device comprises a donor molecule that provides electrons, an acceptor molecule that accepts electrons, and a transition metal compound as an additive, and the device structure is constructed by spin coating and evaporation. The organic thermally activated delayed fluorescent donor molecule and the acceptor molecule can form a uniform amorphous film, and the doped transition metal compound has almost no effect on the luminescence peak position and peak broadening of the film. The doped transition metal compound can overcome the limitation of reverse intersystem crossing spin prohibition, promote the capture of triplet excitons, improve the utilization rate of triplet excitons under electrical injection, and make them participate in the stimulated radiation process.
[0010] According to an embodiment of the present invention, the transition metal compound doped film can be used as a light-emitting layer and is compatible with an electroluminescent device. The light-emitting layer is formed by dissolving a mixed solution containing thermally activated delayed fluorescence donor and acceptor molecules and chloro(1,5-cyclooctadiene)copper(I) dimer under spin coating conditions.
[0011] According to a preferred embodiment of the present invention, the thickness of the transition metal compound doped thermally activated delayed fluorescent film is 30 to 150 nm, preferably 60 to 90 nm.
[0012] The second object of the present invention is to provide a method for preparing the above-mentioned thermally activated delayed fluorescent film, comprising: mixing a fluorescent material solution containing the fluorescent donor molecules and the fluorescent acceptor molecules and a transition metal compound solution, coating the mixture on a template, and annealing to obtain the fluorescent film.
[0013] According to an embodiment of the present invention, in the method for preparing the thermally activated delayed fluorescent film:
[0014] The solvent in the fluorescent material solution is selected from at least one of chlorobenzene and tetrahydrofuran;
[0015] The solvent in the transition metal compound solution is selected from at least one of acetonitrile and tetrahydrofuran;
[0016] The mass ratio of the fluorescent donor molecule to the fluorescent acceptor molecule is 1:(1-10), preferably 1:(1-3);
[0017] The mass ratio of the transition metal compound to the total mass of the fluorescent donor molecule and the fluorescent acceptor molecule is (0.5-10):100, preferably (1-5):100, more preferably (1.25-3):1, and most preferably (1.25-2.5):1;
[0018] In the fluorescent material solution, the total concentration of the fluorescent donor molecules and the fluorescent acceptor molecules is 5 to 80 mg / mL, preferably 12 to 32 mg / mL;
[0019] The concentration of the transition metal compound solution is 1 to 10 mg / mL, preferably 1 to 8 mg / mL.
[0020] According to an embodiment of the present invention, in the method for preparing the thermally activated delayed fluorescent film:
[0021] The annealing temperature is 60-150°C, and the annealing time is 1-15 minutes; preferably, the annealing temperature is 90-110°C, and the annealing time is 5-10 minutes;
[0022] The preparation process is completed under a nitrogen atmosphere.
[0023] A third object of the present invention is to provide an electroluminescent device comprising the thermally activated delayed fluorescent film, or comprising the thermally activated delayed fluorescent film obtained by the above preparation method.
[0024] According to an embodiment of the present invention, the electroluminescent device comprises: a cathode substrate, a hole transport layer, a light-emitting layer containing the thermally activated delayed fluorescent film, an electron transport layer, a hole blocking layer, and a metal anode material. The device is a stacked structure, and the anode material, the hole transport layer, the light-emitting layer, the electron transport layer, the hole blocking layer, and the cathode material are evenly distributed in the corresponding layers.
[0025] Specifically, the cathode substrate is ITO;
[0026] The hole transport layer is PEDOT:PSS;
[0027] The thickness of the hole transport layer is 10 to 60 nm, preferably 20 to 30 nm;
[0028] The electron transport layer is 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene;
[0029] The thickness of the electron transport layer is 10 to 30 nm, preferably 15 to 20 nm;
[0030] The hole blocking layer is lithium fluoride;
[0031] The thickness of the hole blocking layer is 0.5 to 2 nm, preferably 0.5 to 1 nm;
[0032] The metal anode is aluminum.
[0033] The fourth object of the present invention is to provide a method for preparing the above-mentioned electroluminescent device, comprising: cleaning the surface of the cathode substrate, spin coating the hole transport layer, preparing a light-emitting layer containing the thermally activated delayed fluorescent film, and sequentially evaporating an electron transport layer, a hole blocking layer and a metal anode material; preferably, the preparation method specifically comprises the following steps:
[0034] (1) Cleaning the cathode substrate and performing surface treatment;
[0035] (2) spin coating the PEDOT:PSS aqueous solution on the pretreated ITO substrate and annealing to obtain a hole transport layer;
[0036] (3) mixing a fluorescent material solution containing fluorescent donor molecules and fluorescent acceptor molecules and a transition metal compound solution;
[0037] (4) spin coating the mixed solution obtained in step (3) on the hole transport layer obtained in step (2), and annealing;
[0038] (5) Sequentially evaporate the electron transport layer, hole blocking layer and metal anode.
[0039] According to an embodiment of the present invention, in the method for preparing the electroluminescent device:
[0040] The solvent in the fluorescent material solution is selected from at least one of chlorobenzene and tetrahydrofuran;
[0041] The solvent in the transition metal compound solution is selected from at least one of acetonitrile and tetrahydrofuran;
[0042] The mass ratio of the fluorescent donor molecule to the fluorescent acceptor molecule is 1:(1-10), preferably 1:(1-3);
[0043] The mass ratio of the transition metal compound to the total mass of the fluorescent donor molecule and the fluorescent acceptor molecule is (0.5-10):100, preferably (1-5):100;
[0044] In the fluorescent material solution, the total concentration of the fluorescent donor molecules and the fluorescent acceptor molecules is 5 to 80 mg / mL, preferably 12 to 32 mg / mL;
[0045] The concentration of the transition metal compound solution is 1 to 10 mg / mL, preferably 1 to 8 mg / mL;
[0046] The surface treatment in step (1) is to treat the cleaned ITO glass substrate with ultraviolet (UV)-ozone plasma (100W) for 8 minutes;
[0047] The concentration of the PEDOT:PSS aqueous solution in step (2) is 0.2-0.4 wt%, preferably 0.25-0.3 wt%;
[0048] The annealing temperature in step (2) is 100-150° C., preferably 140-150° C.;
[0049] The step (3) is carried out in a nitrogen atmosphere;
[0050] The spin coating step of step (4) is to first spin coat the mixed solution of the transition metal compound and the thermally activated delayed fluorescent molecule at 500 to 1000 rpm for 3 to 5 seconds and then at 3000 to 4000 rpm for 30 to 60 seconds;
[0051] The annealing temperature in step (4) is 60 to 150° C., preferably 90 to 110° C.;
[0052] The evaporation conditions in step (5) are as follows: the pressure in the evaporation chamber is maintained at 1×10 -5 Pa below / s rate.
[0053] Beneficial effects of the present invention:
[0054] The present invention provides a method for improving the utilization rate of triplet excitons and reducing the optical loss of organic electric pumping lasers by doping transition metal compounds in thermally activated delayed fluorescent molecules; the electric drive device having organic thermally activated delayed fluorescent materials doped with transition metal compounds has the following advantages:
[0055] 1. In the present invention, a chloro(1,5-cyclooctadiene)copper(I) dimer having a thermally excited triplet state at room temperature is introduced as a transition metal compound into a thermally activated delayed fluorescent material, so that the two participate in the spin flip process as a whole. The chloro(1,5-cyclooctadiene)copper(I) dimer changes from the ground state to the triplet state and the excited base complex crosses from the triplet state to the singlet state under thermal excitation, so that the spin angular momentum in the system is conserved before and after the reverse intersystem crossing. The limitation of spin prohibition in the system is overcome, and the conversion efficiency of the triplet state to the singlet state is improved, so that a large number of triplet excitons under electrical injection can be flipped to the corresponding luminescent singlet state through the introduced spin mixing channel, thereby realizing the use of triplet excitons in the radiative luminescence process, which provides a new idea for reducing the optical loss of organic electrically pumped lasers.
[0056] 2. The mixed solution of organic thermally activated delayed fluorescent molecules and transition metal compounds provided by the present invention has excellent solution processability, and can realize large-area preparation of thin films by spin coating; patterned construction can be achieved by screen printing; and large-area microcrystal arrays can be obtained by template confined growth method, and each microcrystal unit can be used as a high-quality optical resonant cavity to provide optical feedback and mode amplification for material particle number inversion.
[0057] 3. The monovalent transition metal copper of the transition metal compound of the present invention and the electron-rich nitrogen on the acceptor molecule have an overlap in wave function, so there is a spin-spin coupling between the chloro(1,5-cyclooctadiene)copper(I) dimer and the thermally activated delayed fluorescent material. The copper dimer has the property of room temperature activated spin energy level, which can be introduced into the reverse intersystem crossing process of the thermally activated delayed fluorescent material to achieve efficient utilization of charge transfer state excitons.
[0058] 4. After the light-emitting layer film of the present invention is doped with a transition metal compound, the activation energy of the reverse intersystem crossing of the thermally activated delayed fluorescent material is reduced, indicating that the participation of chloro(1,5-cyclooctadiene)copper(I) dimer can effectively promote the reverse intersystem crossing process by introducing the spin energy level activated at room temperature. At the same time, the thermal activation performance of the thermally activated delayed fluorescent material still exists. During the experiment, the reverse intersystem crossing process in the material can be affected by changing the temperature, thereby regulating the proportion of triplet excitons returning to the singlet state, and finally achieving the regulation of its laser performance.
[0059] 5. In the present invention, an external magnetic field can be used as a non-contact, non-destructive means to achieve the regulation of the reverse intersystem crossing process, thereby regulating the proportion of triplet excitons returning to the singlet state, and ultimately achieving the purpose of regulating laser performance.
[0060] 6. In the present invention, by introducing appropriate proportions of transition metal compounds, the luminescence performance of the electrically driven device can be improved by 68% compared with pure phase thermally activated delayed fluorescent materials at the same current density, demonstrating the great potential of transition metal compounds in overcoming optical losses in electrically pumped lasers. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 This is a diagram of the luminescence mechanism of the organic thermally activated delayed fluorescence doped with the transition metal compound of the present invention.
[0062] Figure 2 The UV-visible absorption graphs of the transition metal compound-doped thermally activated delayed fluorescent films prepared in Comparative Example 1 and Examples 1 to 3 are as follows: Figure 2 In the figure, the undoped curve is Comparative Example 1, the 1.25 wt% doped curve is Example 2, the 2.5 wt% doped curve is Example 1, and the 5 wt% doped curve is Example 3.
[0063] Figure 3 This is a scanning electron microscope test image of the transition metal compound-doped thermally activated delayed fluorescence film prepared in Example 1.
[0064] Figure 4 The photoluminescence spectra of the transition metal compound-doped thermally activated delayed fluorescent films prepared in Comparative Example 1 (undoped) and Example 1 (doped 2.5 wt %) are shown.
[0065] Figure 5 The magneto-photoluminescence curves of the transition metal compound-doped thermally activated delayed fluorescent films prepared in Comparative Example 1 (undoped) and Example 1 (doped 2.5 wt %) are shown.
[0066] Figure 6 The magneto-electroluminescence curves of the transition metal compound-doped electroluminescent devices prepared in Comparative Example 2 and Examples 4 to 6 are as follows: Figure 6 In the figure, the undoped curve is Comparative Example 2, the 1.25 wt% doped curve is Example 5, the 2.5 wt% doped curve is Example 4, and the 5 wt% doped curve is Example 6.
[0067] Figure 7 is a curve diagram showing the change of electroluminescence intensity and current density of the transition metal compound-doped electroluminescent devices prepared in Comparative Example 2 and Examples 4 to 6, Figure 7 In the figure, the undoped curve is Comparative Example 2, the 1.25 wt% doped curve is Example 5, the 2.5 wt% doped curve is Example 4, and the 5 wt% doped curve is Example 6.
[0068] Figure 8is a curve diagram showing the variation of the electroluminescent intensity and doping concentration of the transition metal compound-doped electroluminescent devices prepared in Comparative Example 2 and Examples 4 to 7, Figure 6 In the figure, the undoped curve is Comparative Example 2, the 1.25 wt% doped curve is Example 5, the 2.5 wt% doped curve is Example 4, the 3.75 wt% doped curve is Example 7, and the 5 wt% doped curve is Example 6. DETAILED DESCRIPTION
[0069] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0070] The raw materials used in the examples and comparative examples can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0071] Example 1 Preparation of transition metal compound doped thermally activated delayed fluorescence film
[0072] 8 mg of donor molecule 4,4',4"-tri(N-3-methylphenyl-N-phenylamino)triphenylamine and 24 mg of acceptor molecule tri[2,4,6-trimethyl-3-(3-pyridyl)phenyl]borane were dissolved in 2 ml of chlorobenzene solvent to obtain a thermally activated delayed fluorescent molecular solution with a donor-acceptor ratio of 1:3. Then 4 mg of chloro(1,5-cyclooctadiene)copper(I) dimer was added to 1 ml of acetonitrile solution and ultrasonicated for one hour to obtain a 4 mg / ml transition metal compound solution. The fluorescent molecular solution was mixed with the transition metal compound The solutions were mixed in a volume ratio of 9:1 to obtain a transition metal-catalyzed thermally activated delayed fluorescence stock solution. 58 μl of the obtained stock solution was dripped onto the substrate, and then the mixed solution containing 2.5% of chloro(1,5-cyclooctadiene)copper(I) dimer-doped thermally activated delayed fluorescence molecules was evenly spin-coated onto the substrate at a speed of 800 rpm for 3 seconds and then 4000 rpm. The entire coating process lasted for 30 seconds. Annealing was performed at 100 degrees Celsius for 10 minutes to improve the uniformity of the film, and the obtained film thickness was 30 nm.
[0073] Example 2 Preparation of transition metal compound doped thermally activated delayed fluorescence film
[0074] The preparation process of Example 1 was followed, except that 2 mg of chloro(1,5-cyclooctadiene)copper(I) dimer was added to 1 ml of acetonitrile solution, and the obtained film thickness was 30 nm.
[0075] Example 3 Preparation of transition metal compound doped thermally activated delayed fluorescence film
[0076] The preparation process of Example 1 was followed, except that 8 mg of chloro(1,5-cyclooctadiene)copper(I) dimer was added to 1 ml of acetonitrile solution, and the obtained film thickness was 30 nm.
[0077] Comparative Example 1 Preparation of Thermally Activated Delayed Fluorescence Film
[0078] 8 mg of donor molecules and 24 mg of acceptor molecules were dissolved in 2 ml of chlorobenzene solvent to obtain a thermally activated delayed fluorescent molecule solution with a donor-acceptor ratio of 1:3. 58 microliters of the obtained solution was dropped on the substrate, and then the thermally activated delayed fluorescent molecule solution was evenly spin-coated on the substrate at a speed of 800 rpm for 3 seconds and then 4000 rpm. The entire coating process lasted for 30 seconds. Annealing was performed at 100 degrees Celsius for 10 minutes to improve the uniformity of the film.
[0079] Example 4 Preparation of electroluminescent device based on transition metal compound doping
[0080] 1) Pre-coat a 180nm thick layer of indium tin oxide (ITO) on a clean glass substrate;
[0081] 2) ultrasonically cleaning the substrate with toluene, acetone, and isopropanol for 20 minutes in sequence, and then drying the substrate with nitrogen and subjecting the substrate to surface plasma treatment for 8 minutes;
[0082] 3) on the substrate obtained in step 2), the PEDOT:PSS solution was spin-coated onto the ITO at a speed of 3000 rpm for 30 seconds, and then annealed at 140 degrees Celsius in air for 20 minutes to obtain a hole transport layer with a thickness of 30 nm;
[0083] 4) then transferring the substrate into a glove box, and spin coating a mixed solution containing 2.5% by mass of chloro(1,5-cyclooctadiene)copper(I) dimer-doped thermally activated delayed fluorescent molecules (same as in Example 1) on the substrate obtained in step 3) at a speed of 800 rpm for 3 seconds and then 4000 rpm for 30 seconds, and annealing at 100 degrees Celsius for 10 minutes to improve the uniformity of the film;
[0084] 5) Transfer the substrate obtained in step 4) to a high vacuum thermal evaporator (less than 10 -7 Torr), evaporate 20nm thick TPBI as an electron transport layer at a rate of 1 angstrom per second, evaporate 1 nanometer lithium fluoride at a rate of 0.1 angstrom per second, and evaporate 100 nanometers of aluminum at a rate of 0.8 angstroms per second to complete the preparation of an electrically driven electroluminescent device doped with transition metal compounds.
[0085] Example 5 Preparation of electroluminescent devices based on transition metal compound doping
[0086] The preparation method of Example 4 is adopted, except that in step 4), a mixed solution containing 1.25% by mass of chloro(1,5-cyclooctadiene)copper(I) dimer-doped thermally activated delayed fluorescent molecules (same as Example 2) is spin-coated on the substrate obtained in step 3).
[0087] Example 6 Preparation of electroluminescent devices based on transition metal compound doping
[0088] The preparation method of Example 4 is adopted, except that in step 4), a mixed solution containing 5% by mass of chloro(1,5-cyclooctadiene)copper(I) dimer-doped thermally activated delayed fluorescent molecules (same as Example 3) is spin-coated on the substrate obtained in step 3).
[0089] Example 7 Preparation of electroluminescent device based on transition metal compound doping
[0090] The preparation method of Example 4 is adopted, except that in step 4), a mixed solution containing 3.75% by mass of chloro(1,5-cyclooctadiene)copper(I) dimer-doped thermally activated delayed fluorescent molecules is spin-coated on the substrate obtained in step 3).
[0091] Comparative Example 2 Preparation of electroluminescent device
[0092] 1) Pre-coat a 180nm thick layer of indium tin oxide (ITO) on a clean glass substrate;
[0093] 2) ultrasonically cleaning the substrate with toluene, acetone, and isopropanol for 20 minutes, and then drying the substrate with nitrogen and subjecting the substrate to surface plasma treatment for 8 minutes;
[0094] 3) on the substrate obtained in step 2), the PEDOT:PSS solution was spin-coated onto the ITO at a speed of 3000 rpm for 30 seconds, and then annealed at 140 degrees Celsius in air for 20 minutes to obtain a hole transport layer with a thickness of 30 nm;
[0095] 4) the substrate was then transferred to a glove box, and a solution of thermally activated delayed fluorescent molecules (Comparative Example 1) was spin-coated on the substrate obtained in step 3) at a speed of 800 rpm for 3 seconds and then 4000 rpm for 30 seconds, and annealed at 100 degrees Celsius for 10 minutes to improve the uniformity of the film;
[0096] 5) Transfer the substrate obtained in step 4) to a high vacuum thermal evaporator (less than 10 -7Torr), evaporate 20nm thick TPBI as an electron transport layer at a rate of 1 angstrom per second, evaporate 1 nanometer lithium fluoride at a rate of 0.1 angstrom per second, and evaporate 100 nanometers of aluminum at a rate of 0.8 angstrom per second to complete the manufacture of an electrically driven transition metal compound-doped thermally activated delayed fluorescent display panel.
[0097] Example 8 Structural Characterization of Transition Metal Compound Doped Thermally Activated Delayed Fluorescence Thin Films Obtained from Examples 1 to 3 and Comparative Example 1
[0098] The optical properties of the light-emitting layer film prepared in Example 1 were characterized using an ultraviolet spectrophotometer UH4150. Figure 2 It can be seen that compared with the thermally activated delayed fluorescence film, the absorption peak of the film absorption spectrum after doping with chloro(1,5-cyclooctadiene)copper(I) dimer at around 220 nanometers is significantly increased, and the peak position is blue-shifted by 12 nanometers. In contrast, the absorption peak position at 336 nanometers did not move significantly, and the absorption peak position at 213 nanometers after doping was different from that of the pure phase thermally activated delayed fluorescence material and the pure phase chloro(1,5-cyclooctadiene)copper(I) dimer, indicating that the change is not caused by the simple superposition of absorption spectra, and there is an interaction between the transition metal compound and the thermally activated delayed fluorescence molecules. In order to rule out the possibility that doping will change the film morphology and structure and thus affect the luminescence performance of the device, a scanning electron microscope test was carried out after gold was sprayed on the film surface. Figure 3 The left and right sides are pure phase film and doped film respectively. The results show that the surface of the film is very flat regardless of whether it is doped or not, and the introduction of dopants does not have a significant effect on the morphological structure of the film.
[0099] Example 9 Characterization of the Photoluminescence Performance of the Transition Metal Compound Doped Thermally Activated Delayed Fluorescence Films Obtained from Examples 1 to 3 and Comparative Example 1
[0100] The optical properties of the light-emitting layer film prepared in Example 1 were characterized using a fluorescence spectrometer, Spectrascan PR650. Figure 4 It can be seen that the introduction of chloro(1,5-cyclooctadiene)copper(I) dimer has no effect on the luminescence peak position of the film, and chloro(1,5-cyclooctadiene)copper(I) dimer does not participate in the luminescence process as an emitter. When the energy injection method is light injection, all the excitations are singlet excitons. The presence of transition metal compounds allows spin-permitting, so that a large number of photogenerated singlet excitons can be converted into lower energy triplets through intersystem crossing, making the density of singlet and triplet states approach the same. Therefore, as more photogenerated singlet excitons are converted into triplet states that do not participate in luminescence and dissipate, the luminescence intensity of the film gradually decreases with doping. Magnetophotoluminescence (MPL) ( Figure 5) proves that transition metal compounds promote reverse intersystem crossing. When the energy injection method is light injection, all the excitations are singlet excitons. The presence of transition metal compounds allows spin-permitting, so that a large number of photogenerated singlet excitons can be converted into lower energy triplet states through intersystem crossing. The triplet density in the system regulated by the external magnetic field increases, so the MPL gradually increases with the introduction of transition metal compounds.
[0101] Example 10 Performance Characterization of the Transition Metal Compound-Doped Electroluminescent Devices Obtained in Examples 4 to 7 and Comparative Example 2
[0102] The device was placed between the two poles of an electromagnet controlled by a computer, and a constant voltage or current was applied using Keithley 2450; then a photomultiplier (Thorlab PDA 200C) was used to convert the light signal emitted by the device into an electrical signal, which was then collected using Keithley 2400. Thus, the performance of the electroluminescent device prepared in Example 2 was characterized. Figure 6 As shown, when the energy injection method is electrical injection, the ratio of singlet to triplet states is 1:3 due to the constraints of the statistical rules of spin quantum numbers. The presence of transition metal compounds suppresses the forbidden effect of the intersystem crossing process. The presence of transition metal compounds is closer to opening a bidirectional channel for spin flipping. Due to the generation of high-cardinality triplet states under electrical injection, more triplet excitons are converted into singlet states that can be stimulated to emit light through reverse intersystem crossing. The presence of transition metal compounds makes the density of singlet and triplet states approach the same. Therefore, as more triplet excitons are converted into singlet states participating in luminescence, the triplet density regulated by the external magnetic field decreases, and magneto-electroluminescence (MEL) shows a decreasing trend with increasing doping concentration. At the same time, from Figure 7 It can be clearly seen that the doped device has a higher electroluminescence intensity at the same current density. The comparison with the magnetophotoluminescence data confirms that the introduction of chloro(1,5-cyclooctadiene)copper(I) dimer increases the concentration of the components occupied by the luminescent excited state in the system under the same current density injection. Figure 8 The curve of electroluminescence intensity changing with doping concentration shows that the electroluminescence performance reaches the best when the doping concentration is 2.5% by mass, and the electroluminescence performance of the organic thermally activated delayed fluorescence film is improved by 68% under the same current density injection. However, when the transition metal compound is introduced in excess, as more triplet singlet states reverse back and forth, the transition metal compound component becomes a new exciton relaxation dissipation mode, resulting in a decrease in the electroluminescence performance of the film when the doping concentration is 5wt%.
Claims
1. A transition metal compound doped thermally activated delayed fluorescent film, comprising a fluorescent donor molecule, a fluorescent acceptor molecule and a transition metal compound, wherein: The fluorescent donor molecule is a triphenylamine compound, the fluorescent acceptor molecule is an organic borane compound, and the transition metal compound is chloro(1,5-cyclooctadiene)copper(I) dimer.
2. The fluorescent film according to claim 1, characterized in that: The thickness of the film is 30 to 150 nm, preferably 60 to 90 nm; and / or, The fluorescent donor molecule is 4,4',4"-tri(N-3-methylphenyl-N-phenylamino)triphenylamine; and / or, The fluorescent acceptor molecule is tris[2,4,6-trimethyl-3-(3-pyridyl)phenyl]borane.
3. A method for preparing the thermally activated delayed fluorescent film according to claim 1 or 2, comprising: The fluorescent material solution containing the fluorescent donor molecule and the fluorescent acceptor molecule and the transition metal compound solution are mixed, coated on the template, and annealed to obtain the fluorescent film.
4. The preparation method according to claim 3, characterized in that: The solvent in the fluorescent material solution is selected from at least one of chlorobenzene and tetrahydrofuran; and / or, The solvent in the transition metal compound solution is selected from at least one of acetonitrile and tetrahydrofuran; and / or, The mass ratio of the fluorescent donor molecule to the fluorescent acceptor molecule is 1:(1-10), preferably 1:(1-3); and / or, The mass ratio of the transition metal compound to the total mass of the fluorescent donor molecule and the fluorescent acceptor molecule is (0.5-10):100, preferably (1-5):100; and / or, In the fluorescent material solution, the total concentration of the fluorescent donor molecules and the fluorescent acceptor molecules is 5 to 80 mg / mL, preferably 12 to 32 mg / mL; and / or, The concentration of the transition metal compound solution is 1 to 10 mg / mL, preferably 1 to 8 mg / mL.
5. The preparation method according to claim 4, characterized in that: The annealing temperature is 60-150° C., and the annealing time is 1-15 min; preferably, the annealing temperature is 90-110° C., and the annealing time is 5-10 min; and / or, The preparation process was completed under a nitrogen atmosphere.
6. An electroluminescent device comprising the thermally activated delayed fluorescent film according to claim 1 or 2, or comprising the thermally activated delayed fluorescent film obtained by the preparation method according to any one of claims 3 to 5.
7. The electroluminescent device according to claim 6, characterized in that The electroluminescent device comprises: a cathode substrate, a hole transport layer, a light-emitting layer containing the thermally activated delayed fluorescent film, an electron transport layer, a hole blocking layer, and a metal anode material.
8. The electroluminescent device according to claim 7, characterized in that The cathode substrate is ITO; and / or, The hole transport layer is PEDOT:PSS; and / or, The thickness of the hole transport layer is 10 to 60 nm, preferably 20 to 30 nm; and / or, The electron transport layer is 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene; and / or, The thickness of the electron transport layer is 10 to 30 nm, preferably 15 to 20 nm; and / or, The hole blocking layer is lithium fluoride; and / or, The thickness of the hole blocking layer is 0.5 to 2 nm, preferably 0.5 to 1 nm; and / or, The metal anode material is aluminum.
9. A method for preparing the electroluminescent device according to any one of claims 6 to 8, comprising: The cathode substrate surface is cleaned, a hole transport layer is spin-coated, a light-emitting layer containing the thermally activated delayed fluorescent film is prepared, and an electron transport layer, a hole blocking layer and a metal anode material are sequentially evaporated.
10. The preparation method according to claim 9, characterized in that: The preparation method specifically comprises the following steps: (1) Cleaning the cathode substrate and performing surface treatment; (2) spin coating the PEDOT:PSS aqueous solution on the pretreated ITO substrate and annealing to obtain a hole transport layer; (3) mixing a fluorescent material solution containing fluorescent donor molecules and fluorescent acceptor molecules and a transition metal compound solution; (4) spin coating the mixed solution obtained in step (3) on the hole transport layer obtained in step (2), and annealing; (5) Sequentially evaporate the electron transport layer, hole blocking layer and metal anode material.
11. The preparation method according to claim 10, characterized in that: The solvent in the fluorescent material solution is selected from at least one of chlorobenzene and tetrahydrofuran; and / or, The solvent in the transition metal compound solution is selected from at least one of acetonitrile and tetrahydrofuran; and / or, The mass ratio of the fluorescent donor molecule to the fluorescent acceptor molecule is 1:(1-10), preferably 1:(1-3); and / or, The mass ratio of the transition metal compound to the total mass of the fluorescent donor molecule and the fluorescent acceptor molecule is (0.5-10):100, preferably (1-5):100; and / or, In the fluorescent material solution, the total concentration of the fluorescent donor molecules and the fluorescent acceptor molecules is 5 to 80 mg / mL, preferably 12 to 32 mg / mL; and / or, The concentration of the transition metal compound solution is 1 to 10 mg / mL, preferably 1 to 8 mg / mL; and / or, The surface treatment in step (1) is to treat the cleaned ITO glass substrate with ultraviolet-ozone plasma; and / or, The concentration of the PEDOT:PSS aqueous solution in step (2) is 0.2-0.4 wt%, preferably 0.25-0.3 wt%; and / or, The annealing temperature in step (2) is 100-150° C., preferably 140-150° C.; and / or, The step (3) is carried out in a nitrogen atmosphere; and / or, The spin coating step of step (4) is to first spin coat the mixed solution at 500-1000 rpm for 3-5 seconds and then at 3000-4000 rpm for 30-60 seconds; and / or, The annealing temperature in step (4) is 60 to 150° C., preferably 90 to 110° C.; and / or, The evaporation conditions in step (5) are as follows: the pressure in the evaporation chamber is maintained at 1×10 -5 Pa below rate.